A composite adhesive for lithium battery protective film and a method for manufacturing the same

By modifying petroleum resin and curing agent, the high temperature resistance and flame retardant properties of polyacrylate adhesive are improved, and the problems of reduced adhesion and insufficient flame retardant properties in high temperature environments are solved, ensuring the lithium battery protective film Stability and safety.

CN117343667BActive Publication Date: 2024-11-12JIANGXI XINMEI NEW MATERIAL TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202311505618.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-13
Publication Date
2024-11-12
Estimated Expiration
2043-11-13

AI Technical Summary

Technical Problem

Polyacrylate adhesives have reduced adhesion in high temperature environments, resulting in protective film shedding and battery damage, and their flame retardant performance is insufficient, increasing the risk of spontaneous combustion of new energy vehicles.

Method used

By modifying petroleum resin and curing agent and adding it to the polyacrylate adhesive, a composite adhesive is prepared, including petroleum resin-based flame retardant and modified curing agent, improving its high temperature resistance and flame retardant resistance performance.

Benefits of technology

It significantly improves the high temperature resistance and flame retardant properties of the adhesive, prevents the protective film from falling off and battery damage, and reduces the risk of spontaneous combustion of new energy vehicles.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117343667B_ABST
    Figure CN117343667B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, and discloses a composite adhesive for a lithium battery protective film and a manufacturing method thereof. The adhesive comprises a soft monomer, a hard monomer, a functional monomer, an emulsifier, a petroleum resin-based flame retardant, an initiator, a modified curing agent and a solvent, wherein the petroleum resin-based flame retardant is prepared by chemically modifying petroleum resin and then grafting a nitrogen-phosphorus flame retardant, and the modified curing agent is prepared by introducing a heteroazo silicon tricyclic ring into the structure of polyethylene imine, and then the modified curing agent and the petroleum resin-based flame retardant are added into the preparation process of a polyacrylate adhesive, so as to effectively improve the high temperature resistance and flame retardancy of the adhesive, and the adhesive can be widely used in the protective film of a lithium battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of adhesives, and in particular to a composite adhesive for a lithium battery protective film and a method for manufacturing the same. Background Art

[0002] With the rapid development of the market economy, energy shortage and environmental pollution problems have gradually aroused people's high vigilance. New energy vehicles, as an environmentally friendly means of transportation, have gradually appeared in people's vision. In the field of new energy vehicles, the most widely used is lithium batteries. There is a protective film on the surface of the lithium battery cell, which can insulate and protect the lithium battery. The protective film includes a substrate layer and an adhesive layer. For the adhesive layer, commonly used adhesives include epoxy resin adhesives, organic silicone adhesives and polyacrylate adhesives, among which polyacrylate adhesives have good resistance to It has the advantages of strong impact resistance, good weather resistance, good corrosion resistance and good adhesion, and is therefore widely used. The invention patent with application number CN201510248474.2 discloses a polyacrylate pressure-sensitive adhesive and a preparation method thereof. The polyacrylate pressure-sensitive adhesive is prepared through reasonable proportioning and simple process. The prepared glue has excellent electrolyte corrosion resistance and good initial adhesion. It is used in pressure-sensitive tapes for protection and assembly of power lithium batteries of new energy vehicles. It will not fall off, warp or the like, and has good use effect.

[0003] However, lithium batteries, which are key components of new energy vehicles, work in high-temperature environments for a long time, and the adhesive in the protective film on the battery surface will reduce its adhesion due to excessively high temperature, causing the protective film to fall off, resulting in the electrolyte flowing out of the battery, and causing the battery to be damaged and contaminated. In addition, spontaneous combustion incidents of new energy vehicles are common. During use, the car may have problems such as line short circuit, charger failure and motor overload, resulting in excessively high internal temperature, thereby causing the car to spontaneously combust, posing a threat to life and property. Based on this, the present invention provides a composite adhesive for lithium battery protective film and a method for manufacturing the same. By modifying the curing agent and petroleum resin and adding them to the preparation process of the polyacrylate adhesive, the composite adhesive has excellent high temperature resistance and flame retardant properties. Summary of the invention

[0004] The purpose of the present invention is to provide a composite adhesive for lithium battery protective film and a method for manufacturing the same, which solves the following technical problems:

[0005] (1) Solved the problem of poor high temperature resistance of polyacrylate adhesives;

[0006] (2) The problem of poor flame retardancy of polyacrylate adhesives has been solved.

[0007] The purpose of the present invention can be achieved through the following technical solutions:

[0008] A composite adhesive for a lithium battery protective film comprises the following raw materials in parts by weight: 60-70 parts of a soft monomer, 15-20 parts of a hard monomer, 6-8 parts of a functional monomer, 4-6 parts of an emulsifier, 10-20 parts of a petroleum resin-based flame retardant, 0.5-1 parts of an initiator, 1-2 parts of a modified curing agent, and 30-40 parts of a solvent.

[0009] Furthermore, the soft monomer is one or more of ethyl acrylate, butyl acrylate, n-octyl acrylate, and isooctyl acrylate; the hard monomer is one or more of methyl acrylate, methyl methacrylate, and ethyl methacrylate; the functional monomer is one or more of acrylic acid, methacrylic acid, and methacrylic acid; the emulsifier is any one of allyloxy nonylphenol ether, allyl alcohol polyoxyethylene ether, or sodium allyl alkyl ether sulfonate; the initiator is any one of ammonium persulfate, potassium persulfate, or sodium persulfate; and the solvent is any one of ethyl acetate, acetone, or toluene.

[0010] Furthermore, the method for producing the petroleum resin-based flame retardant comprises the following steps:

[0011] S1: Put petroleum resin and xylene in a reactor, heat to 80-90°C, add maleic anhydride, stir evenly, then add dicumyl peroxide, react for 1-2h, remove the solvent, and obtain modified petroleum resin;

[0012] S2: Mix the modified petroleum resin and toluene, raise the temperature to 40-50°C, add 4-aminobenzyl diethyl phosphate, stir evenly, and keep the temperature to react for 5-6 hours. After the reaction is completed, remove the solvent by vacuum distillation and dry to obtain a petroleum resin-based flame retardant.

[0013] Furthermore, in step S1, the petroleum resin is C5 petroleum resin, and the acid value is 0.5-0.8 mgKOH / g.

[0014] In the above technical scheme, petroleum resin is chemically modified by maleic anhydride through the action of an initiator, anhydride groups are introduced, and its polarity is increased to obtain a modified petroleum resin. The anhydride in its structure can react with the amino group in the structure of 4-aminobenzyl diethyl phosphate, and the flame retardant elements phosphorus and nitrogen are introduced into the structure of the petroleum resin to obtain a petroleum resin-based flame retardant. The flame retardant is added to the preparation process of the polyacrylate adhesive to effectively improve the flame retardant properties of the adhesive. The petroleum resin itself, as a tackifying resin, can enhance the adhesion of the polyacrylate adhesive. The grafted nitrogen-phosphorus flame retardant in its structure can decompose to produce organic acids and other substances during combustion, which promotes the dehydration and carbonization of the adhesive. The formed carbon layer is non-flammable and can isolate oxygen, making combustion impossible. At the same time, the nitrogen-phosphorus flame retardant can also decompose at high temperature to produce non-flammable gas to dilute the oxygen concentration, thereby achieving a flame retardant effect.

[0015] Furthermore, the manufacturing method of the modified curing agent is specifically as follows:

[0016] Mix polyethyleneimine and ethanol, add 1-vinyl silane, mix well, stir and react at 35-40° C. for 6-8 hours, remove the solvent after the reaction is completed, and vacuum dry to obtain a modified curing agent.

[0017] Furthermore, the average molecular weight of the polyethyleneimine is 1800.

[0018] Furthermore, the molar ratio of the polyethyleneimine to 1-vinyl silatriane is 1:2-3.

[0019] In the above technical scheme, the amino group in polyethyleneimine can undergo Michael addition reaction with the alkenyl group in 1-vinyl azasilatrioxane, thereby introducing azasilatricycle into the molecular chain of polyethyleneimine to obtain a modified curing agent. The SiO bond and rigid structure contained in the modified curing agent can effectively improve the high temperature resistance of the adhesive, prevent the adhesive from reducing the adhesion due to excessive temperature, thereby avoiding the shedding of the protective film, making the electrolyte less likely to leak, and protecting the battery from damage and pollution. On the other hand, the modified curing agent structure also contains nitrogen and silicon flame retardant elements, which can play a synergistic role with the petroleum resin-based flame retardant to further improve the flame retardant properties of the polyacrylate adhesive.

[0020] A method for manufacturing a composite adhesive for a lithium battery protective film comprises the following steps:

[0021] Step 1: Add soft monomer, hard monomer, functional monomer, emulsifier and solvent into the reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 60-70°C, add initiator, keep the temperature for reaction for 5-6h, discharge the material, and obtain polyacrylate emulsion;

[0022] Step 2: Add a petroleum resin-based flame retardant and a modified curing agent to the above polyacrylate emulsion, mix well, stir for 2-3 hours, and discharge to obtain a composite adhesive for a lithium battery protective film.

[0023] Furthermore, in step 2, the stirring rate is 800-1000 r / min, and the stirring temperature is 40-45°C.

[0024] Beneficial effects of the present invention:

[0025] The present invention provides a composite adhesive for a lithium battery protective film and a method for manufacturing the same. A modified curing agent and a petroleum resin-based flame retardant are prepared and then added into the preparation process of a polyacrylate adhesive, so that the adhesive has excellent high temperature resistance and flame retardant properties and can be widely used in protective films of lithium batteries.

[0026] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0028] Figure 1 This is the infrared spectrum of polyethyleneimine and modified curing agent. DETAILED DESCRIPTION

[0029] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0030] Example 1

[0031] 1. Preparation of petroleum resin-based flame retardant

[0032] S1: 10 g of C5 petroleum resin with an acid value of 0.6 mgKOH / g and 100 mL of xylene are placed in a reactor, heated to 90° C., 8.7 g of maleic anhydride are added, stirred evenly, and then 1.4 g of diisopropylbenzene peroxide is added. After reacting for 2 h, the solvent is removed to obtain a modified petroleum resin;

[0033] S2: Mix 4.5 g of modified petroleum resin and 60 mL of toluene, heat to 50°C, add 3.8 g of 4-aminobenzyl diethyl phosphate, stir evenly, and keep warm for 5 hours. After the reaction is completed, remove the solvent by vacuum distillation and dry to obtain a petroleum resin-based flame retardant.

[0034] 5 mg of petroleum resin-based flame retardant was weighed, and the carbon, hydrogen and nitrogen contents of the modified petroleum resin and the petroleum resin-based flame retardant were determined using a Var io ELⅢ element analyzer. The test showed that the carbon content of the modified petroleum resin was 74.5%, the hydrogen content was 9.7%, and it did not contain nitrogen. The carbon content of the petroleum resin-based flame retardant was 78.2%, the hydrogen content was 11.3%, and the nitrogen content was 1.08%. It is speculated that this is due to the reaction between the anhydride in the structure of the modified petroleum resin and the amino group in 4-aminobenzyl diethyl phosphate, resulting in the introduction of nitrogen.

[0035] 2. Preparation of modified curing agent

[0036] 5 g of polyethyleneimine with an average molecular weight of 1800 and 50 mL of ethanol were mixed, 1.7 g of 1-vinyl azasilane was added, and after mixing evenly, the mixture was stirred and reacted at 40° C. for 6 h. After the reaction was completed, the solvent was removed and vacuum dried to obtain a modified curing agent.

[0037] The infrared characterization of polyethyleneimine and modified curing agent showed that Figure 1 As shown, the modified curing agent is at 3426cm -1 and 3375cm -1 The absorption peaks of amino and imino groups appear at 2904 cm -1 The absorption peak of CH in the methylene group appears at 1051 cm -1 The absorption peak of CN appears at 1103 cm -1 The absorption peak of Si-OC appeared at the position, indicating that polyethyleneimine and 1-vinyl azasilane reacted and polyethyleneimine was successfully modified.

[0038] 3. Preparation of composite adhesive for lithium battery protective film

[0039] Step 1: Add 60 parts of ethyl acrylate, 15 parts of ethyl methacrylate, 6 parts of methacrylic acid, 4 parts of allyloxy nonylphenol ether and 30 parts of ethyl acetate into a reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 60°C, add 0.5 parts of ammonium persulfate, keep the temperature for reaction for 5 hours, discharge the material, and obtain a polyacrylate emulsion;

[0040] Step 2: Add 10 parts of petroleum resin-based flame retardant and 1 part of modified curing agent to the above polyacrylate emulsion, mix well, stir for 2 hours at a speed of 800 r / min and a temperature of 40°C, and discharge to obtain a composite adhesive for lithium battery protective film.

[0041] The petroleum resin-based flame retardant and modified curing agent prepared in this example are used in the following examples and comparative examples.

[0042] Example 2

[0043] Preparation of composite adhesive for lithium battery protective film

[0044] Step 1: add 65 parts of ethyl acrylate, 18 parts of ethyl methacrylate, 7 parts of methacrylic acid, 5 parts of allyloxy nonylphenol ether and 35 parts of ethyl acetate into a reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 65°C, add 0.8 parts of ammonium persulfate, keep the temperature for reaction for 5.5 hours, discharge the material, and obtain a polyacrylate emulsion;

[0045] Step 2: Add 15 parts of petroleum resin-based flame retardant and 1.5 parts of modified curing agent to the above polyacrylate emulsion, mix well, stir for 2.5 hours at a speed of 900 r / min and a temperature of 40°C, and discharge to obtain a composite adhesive for lithium battery protective film.

[0046] Example 3

[0047] Preparation of composite adhesive for lithium battery protective film

[0048] Step 1: add 70 parts of ethyl acrylate, 20 parts of ethyl methacrylate, 8 parts of methacrylic acid, 6 parts of allyloxy nonylphenol ether and 40 parts of ethyl acetate into a reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 70°C, add 1 part of ammonium persulfate, keep the temperature for reaction for 6 hours, discharge the material, and obtain a polyacrylate emulsion;

[0049] Step 2: Add 20 parts of petroleum resin-based flame retardant and 2 parts of modified curing agent to the above polyacrylate emulsion, mix well, stir for 3 hours at a speed of 1000r / min and a temperature of 45°C, and discharge to obtain a composite adhesive for lithium battery protective film.

[0050] Comparative Example 1

[0051] Preparation of composite adhesive for lithium battery protective film

[0052] Step 1: add 70 parts of ethyl acrylate, 20 parts of ethyl methacrylate, 8 parts of methacrylic acid, 6 parts of allyloxy nonylphenol ether and 40 parts of ethyl acetate into a reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 70°C, add 1 part of ammonium persulfate, keep the temperature for reaction for 6 hours, discharge the material, and obtain a polyacrylate emulsion;

[0053] Step 2: Add 2 parts of modified curing agent to the above polyacrylate emulsion, mix well, stir for 3 hours at a speed of 1000 r / min and a temperature of 45° C., and discharge to obtain a composite adhesive for a lithium battery protective film.

[0054] Comparative Example 2

[0055] Preparation of composite adhesive for lithium battery protective film

[0056] Step 1: add 70 parts of ethyl acrylate, 20 parts of ethyl methacrylate, 8 parts of methacrylic acid, 6 parts of allyloxy nonylphenol ether and 40 parts of ethyl acetate into a reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 70°C, add 1 part of ammonium persulfate, keep the temperature for reaction for 6 hours, discharge the material, and obtain a polyacrylate emulsion;

[0057] Step 2: Add 20 parts of petroleum resin-based flame retardant and 2 parts of polyethyleneimine to the above polyacrylate emulsion, mix well, stir for 3 hours at a speed of 1000 r / min and a temperature of 45°C, and discharge to obtain a composite adhesive for lithium battery protective film.

[0058] Comparative Example 3

[0059] Preparation of composite adhesive for lithium battery protective film

[0060] Step 1: add 70 parts of ethyl acrylate, 20 parts of ethyl methacrylate, 8 parts of methacrylic acid, 6 parts of allyloxy nonylphenol ether and 40 parts of ethyl acetate into a reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 70°C, add 1 part of ammonium persulfate, keep the temperature for reaction for 6 hours, discharge the material, and obtain a polyacrylate emulsion;

[0061] Step 2: Add 20 parts of petroleum resin and 2 parts of modified curing agent to the above polyacrylate emulsion, mix well, stir for 3 hours at a speed of 1000 r / min and a temperature of 45° C., and discharge to obtain a composite adhesive for a lithium battery protective film.

[0062] Comparative Example 4

[0063] Preparation of composite adhesive for lithium battery protective film

[0064] Step 1: add 70 parts of ethyl acrylate, 20 parts of ethyl methacrylate, 8 parts of methacrylic acid, 6 parts of allyloxy nonylphenol ether and 40 parts of ethyl acetate into a reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 70°C, add 1 part of ammonium persulfate, keep the temperature for reaction for 6 hours, discharge the material, and obtain a polyacrylate emulsion;

[0065] Step 2: Add 2 parts of polyethyleneimine to the above polyacrylate emulsion, mix well, stir for 3 hours at a speed of 1000 r / min and a temperature of 45° C., and discharge to obtain a composite adhesive for a lithium battery protective film.

[0066] Performance Testing

[0067] ①. High temperature resistance test

[0068] The adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were coated on transparent PET films, respectively, and dried to form adhesive layers with a thickness of 25 μm to prepare test tapes. The 180° peel strength test was performed according to the national standard GB / T 2792-2014, and the test result was recorded as R1 (N / m). The prepared tapes were placed in a constant temperature oven and heat treated at 150°C for 8 hours. The 180° peel strength was tested again, and the test result was recorded as R2 (N / m). The peel strength retention rate was calculated using the formula:

[0069]

[0070] The higher the peel strength retention rate, the better the high temperature resistance of the adhesive. The test results are shown in the following table:

[0071] <![CDATA[R1(N / m)]]> <![CDATA[R2(N / m)]]> X(%) Example 1 410 387 94.4 Example 2 416 394 94.7 Example 3 409 385 94.1 Comparative Example 1 327 279 85.3 Comparative Example 2 391 286 73.1 Comparative Example 3 384 352 91.7 Comparative Example 4 315 223 70.8

[0072] As can be seen from the above table, the peel strength of the adhesives prepared by Examples 1 to 3 of the present invention and Comparative Examples 2 to 3 before heat treatment is higher. Since petroleum resin capable of enhancing the adhesion of the adhesive is added during the preparation process, the peel strength before heat treatment is higher than that of Comparative Examples 1 and 4 without adding petroleum resin. The peel strength retention rate of the adhesives prepared by Examples 1 to 3 is also higher, so they have excellent high temperature resistance. The adhesives prepared by Comparative Examples 1 and 3 have good high temperature resistance because a modified curing agent containing aza-silatricycle is added, while the adhesives prepared by Comparative Examples 2 and 4 do not have a modified curing agent added, so the high temperature resistance is poor.

[0073] ② Flame retardant performance test

[0074] The adhesives prepared in Examples 1 to 3 and Comparative Examples 1 to 4 were dried and prepared into samples meeting the specifications. The oxygen index was measured according to the national standard GB / T 2406.2-2009. The test results are shown in the following table:

[0075] Oxygen index (%) Example 1 31.5 Example 2 32.4 Example 3 31.7 Comparative Example 1 28.1 Comparative Example 2 30.9 Comparative Example 3 28.3 Comparative Example 4 23.6

[0076] As can be seen from the above table, the oxygen index of the adhesives prepared in Examples 1 to 3 of the present invention is relatively high, indicating excellent flame retardant properties. The oxygen index of the adhesive prepared in Comparative Example 2 is also relatively high, and the flame retardant effect is also good due to the addition of a petroleum resin-based flame retardant. The adhesives prepared in Comparative Examples 1 and 3 also have a certain flame retardant effect, because a modified curing agent containing flame retardant elements nitrogen and silicon is added in the structure when preparing the adhesive, while the oxygen index of the adhesive prepared in Comparative Example 4 is only 23.6%, and neither a petroleum resin-based flame retardant nor a modified curing agent containing nitrogen and silicon flame retardant elements is added, so there is no flame retardant effect.

[0077] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0078] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the concept of the invention or exceed the scope defined by the claims, they should all fall within the protection scope of the present invention.

Claims

1. A composite adhesive for lithium battery protective film, It is characterized in that The invention comprises the following raw materials in parts by weight: 60-70 parts of soft monomer, 15-20 parts of hard monomer, 6-8 parts of functional monomer, 4-6 parts of emulsifier, 10-20 parts of petroleum resin-based flame retardant, 0.5-1 parts of initiator, 1-2 parts of modified curing agent, and 30-40 parts of solvent; The method for producing the petroleum resin-based flame retardant comprises the following steps: S1: Put petroleum resin and xylene in a reactor, heat to 80-90°C, add maleic anhydride, stir evenly, then add dicumyl peroxide, react for 1-2h, remove the solvent, and obtain a modified petroleum resin; the petroleum resin is C 5 Petroleum resin, acid value is 0.5-0.8mgKOH / g; S2: Mix the modified petroleum resin and toluene, raise the temperature to 40-50° C., add 4-aminobenzyl diethyl phosphate, stir evenly, and keep the temperature to react for 5-6 hours. After the reaction is completed, remove the solvent by vacuum distillation, and dry to obtain a petroleum resin-based flame retardant; The manufacturing method of the modified curing agent is specifically as follows: Mix polyethyleneimine and ethanol, add 1-vinyl silatriane, mix well, stir and react at 35-40° C. for 6-8 hours, remove the solvent after the reaction is completed, and vacuum dry to obtain a modified curing agent; The average molecular weight of the polyethyleneimine is 1800; The molar ratio of polyethyleneimine to 1-vinyl silatriane is 1:2-3; The soft monomer is one or more of ethyl acrylate, butyl acrylate, n-octyl acrylate, and isooctyl acrylate; the hard monomer is one or more of methyl acrylate, methyl methacrylate, and ethyl methacrylate; the functional monomer is one or more of acrylic acid, methacrylic acid, and methacrylic acid; the emulsifier is any one of allyloxy nonylphenol ether, allyl alcohol polyoxyethylene ether, or sodium allyl alkyl ether sulfonate; the initiator is any one of ammonium persulfate, potassium persulfate, or sodium persulfate; and the solvent is any one of ethyl acetate, acetone, or toluene.

2. A method for producing the composite adhesive for lithium battery protective film according to claim 1, It is characterized in that The following steps are involved: Step 1: Add soft monomer, hard monomer, functional monomer, emulsifier and solvent into the reactor and mix them evenly, introduce nitrogen protection, raise the temperature to 60-70°C, add initiator, keep the temperature for reaction for 5-6h, discharge the material, and obtain polyacrylate emulsion; Step 2: Add a petroleum resin-based flame retardant and a modified curing agent to the above polyacrylate emulsion, mix well, stir for 2-3 hours, and discharge to obtain a composite adhesive for a lithium battery protective film.

3. A method for producing a composite adhesive for a lithium battery protective film according to claim 2, It is characterized in that In step 2, the stirring rate is 800-1000 r / min, and the stirring temperature is 40-45°C.

Citation Information

Patent Citations

  • Polyacrylate pressure-sensitive glue and preparation method therefor

    CN104910746A

  • High temperature-resistant polyacrylate pressure-sensitive adhesive emulsion and preparation method and application thereof

    CN101974299A

  • Polyacrylate emulsion pressure-sensitive adhesive for electronic protective films, preparation method and application thereof

    CN107602760A

  • High-viscosity flame-retardant environmentally-friendly pressure-sensitive adhesive and preparation method thereof, and pressure-sensitive adhesive film preparation method

    CN110684491A

  • Waterproof roll hot-melt pressure-sensitive adhesive and preparation method thereof

    CN111320955A