A cross-linked polyolefin material and its preparation method and application
By using PE resin, EVA resin and polyolefin resin thermoplastic elastomer in high-voltage wire conductor materials, combined with silane grafted polyolefin, silicone rubber and hydrogen-containing silicone oil, the problem of insufficient softness and wear resistance of the material is solved and high temperature is achieved and excellent performance under aging conditions.
Patent Information
- Application Number
- CN202311429525.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2043-10-31
AI Technical Summary
The softness of the existing high-voltage wire conductor materials is insufficient, and it is difficult to maintain wear resistance while improving the softness, especially under high temperature and aging conditions, the performance changes are large.
Using PE resin, EVA resin and polyolefin resin thermoplastic elastomer as the matrix, silane grafted polyolefin, silicone rubber and hydrogen-containing silicone oil are added to improve the compatibility and cross-linking of the material through a specific ratio combination, and improve the softness. and wear resistance.
It achieves excellent wear resistance and softness of the material, and shows a low elongation rate reduction in break under aging conditions, which is suitable for the preparation of high-voltage wire conductors.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a cross-linked polyolefin material and a preparation method and application thereof. Background Art
[0002] At present, countries around the world have launched plans to delist fuel vehicles, and the market share of new energy vehicles has increased rapidly. With the increase in driving range, battery capacity continues to increase, charging efficiency continues to improve, voltage continues to increase, and the cross-sectional area of high-voltage wire conductors in the car continues to increase. In order to facilitate the installation of wiring harnesses in the car, the requirements for material softness are getting higher and higher.
[0003] At present, the traditional low-smoke, halogen-free, cross-linked polyolefin materials used for high-voltage wires in vehicles are not flexible enough. The products on the market are uneven, and the hardness is generally concentrated around 85-90A, which cannot meet the increasingly stringent softness requirements. At the same time, due to the low softness of polyolefin materials, low-crystallinity resins are usually used, and the material has poor wear resistance.
[0004] CN101397380A discloses a high temperature resistant soft low smoke halogen free flame retardant polyolefin cable material. The present invention selects a soft ethylene-vinyl acetate copolymer with a vinyl acetate content greater than 30% as one of the resin base materials, which can increase the softness of the cable material on the one hand, and give the cable material a higher limiting oxygen index on the other hand. The softell series resin products of Basell Company have a melting point greater than 140°C and a Shore A hardness less than 90. After being evenly dispersed in the cable material of the present invention, the high temperature resistance of the material can be greatly improved, and the softness of the material will not be greatly reduced like adding high density polyethylene; however, its Shore A hardness is still relatively high, higher than 80A, and its mechanical properties are lower than 10Mpa. After hot air aging, the mechanical properties change greatly.
[0005] CN106867090A discloses a high temperature resistant soft thermoplastic low smoke halogen free flame retardant polyolefin cable, wherein the comonomer content of the selected ethylene-vinyl acetate and ethylene-acrylate copolymers is greater than 26%, and the selected polymer compatibilizers are maleic anhydride grafted ethylene copolymer and ethylene-acrylate-maleic anhydride terpolymer, both of which have a hardness higher than 80A, thereby ensuring both the flame retardant property and the softness of the material. Although it has good aging performance, its Shore A hardness is still relatively high, higher than 80A, sacrificing the wear resistance of the material.
[0006] Therefore, how to provide a polyolefin material with excellent wear resistance and softness has become a technical problem that needs to be solved urgently by those skilled in the art. Summary of the invention
[0007] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a cross-linked polyolefin material and a preparation method and application thereof. The cross-linked polyolefin material uses PE resin, EVA resin and polyolefin resin thermoplastic elastomer as base resins, and by adding silane grafted polyolefin, silicone rubber and hydrogen-containing silicone oil, a cross-linked polyolefin material with excellent wear resistance and softness is obtained.
[0008] To achieve the above object, the technical solution adopted by the present invention is:
[0009] A cross-linked polyolefin material comprises the following components in parts by weight: 5 to 10 parts of PE resin, 15 to 30 parts of EVA resin, 15 to 25 parts of polyolefin resin thermoplastic elastomer, 13 to 45 parts of silicone rubber, 5 to 10 parts of silane grafted polyolefin, 1 to 2 parts of a cross-linking aid, 0.5 to 2 parts of hydrogen-containing silicone oil, and 0.5 to 2 parts of a catalyst;
[0010] The vinyl content in the silicone rubber is 0.12% to 1.79%.
[0011] The vinyl content in the silicone rubber is obtained by testing according to the standard of GB / T 36691-2018.
[0012] The present invention combines the above-mentioned various raw materials in a specific ratio to obtain a cross-linked polyolefin material with excellent wear resistance and softness. The cross-linked polyolefin material uses PE resin, EVA resin and polyolefin resin thermoplastic elastomer as matrix resins. The addition of silane-grafted polyolefin can improve the compatibility problem between silicone rubber and polyolefin resin, so that the polyolefin / silicone rubber composite material can exert the softness and wear resistance of silicone rubber, thereby achieving the advantages of improved softness and wear resistance.
[0013] Compared with directly adding silane, the silane grafted polyolefin has better compatibility with the polyolefin system of the present invention, and can further improve the softness and wear resistance of the present invention.
[0014] The silicone rubber molecules contain vinyl groups, and the double bonds are broken during the irradiation process, which can react with -Si-O-CH3 in the silane-grafted polyolefin molecular structure. During the reaction, small molecules are removed. The combination of the two improves the softness, wear resistance and aging resistance. Therefore, both are indispensable to the present invention.
[0015] The inventors have found that silicone rubber not only needs to contain vinyl, but also the vinyl content needs to be in the range of 0.19% to 1.79%. Within this range, the material has good softness and wear resistance. If the vinyl content is too low, the degree of cross-linking of the silicone rubber is insufficient and the wear resistance is poor. If the vinyl content is too high, the degree of cross-linking is too high, resulting in reduced flexibility of the molecular chain, insufficient softness, and a harder material.
[0016] The inventors further explored the influence of the amount of silane-grafted polyolefin added on the effect, and controlled the amount added within the scope of the present invention. If the amount added is too large, the molecular chains will be too tightly entangled, thereby causing the elongation of the material to decrease and the hardness to increase. If the amount added is too small, the compatibility of silicone rubber and polyolefin resin will be insufficient, and the performance and wear resistance of the material will be poor. Therefore, it is necessary to control the amount of silane-grafted polyolefin added.
[0017] The inventors further explored the influence of the amount of silicone rubber added on the effect, and controlled the amount of silicone rubber added within the scope of the present invention. If the amount of silicone rubber added is too large, the system will be too soft, which will lead to too low strength. If the amount of silicone rubber added is too small, the hardness of the material will be too high. Therefore, the amount of silicone rubber added needs to be controlled.
[0018] The polyolefin resin thermoplastic elastomer (POE) is a thermoplastic elastomer obtained by in-situ polymerization of ethylene and α-olefin using a metallocene catalyst, wherein the α-olefin includes at least one of α-olefins having 4 to 8 carbon atoms.
[0019] Preferably, the α-olefin includes at least one of 1-butene, 1-hexene and 1-octene.
[0020] Furthermore, the polyolefin elastomer is preferably a thermoplastic elastomer obtained by in-situ polymerization of ethylene and 1-octene using a metallocene catalyst.
[0021] Preferably, the PE resin is LLDPE.
[0022] Preferably, the amount of the silicone rubber is 15 to 30 parts.
[0023] Among them, the sum of the weight percentages of the PE resin, EVA resin and polyolefin resin thermoplastic elastomer accounts for more than 80% of the resin components in the cross-linked polyolefin material. Preferably, the sum of the weight percentages of the PE resin, EVA resin and polyolefin resin thermoplastic elastomer accounts for more than 85% of the resin components in the cross-linked polyolefin material.
[0024] Preferably, the silicone rubber includes at least one of methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, methyl β-cyano vinyl silicone rubber, and trifluoropropyl methyl vinyl silicone rubber.
[0025] Preferably, the VA content of the EVA resin is 15% to 43%. By controlling the VA content of the EVA resin to be 15% to 43%, if the VA content is too low, the PE content in the EVA will be high, the hardness of the material will increase, the elongation will decrease, and the softness requirement cannot be met; if the VA content is too high, the wear resistance will deteriorate. Therefore, in the present invention, the VA content needs to be controlled between 15% and 43%.
[0026] Preferably, the VA content of the EVA resin is 18% to 40%.
[0027] Preferably, the VA content of the EVA resin is 26% to 40%.
[0028] Preferably, the vinyl content in the silicone rubber is 0.19% to 1.70%.
[0029] Preferably, the melt index of the EVA is 2 to 10 g / 10 min at 190° C. and 2.16 kg, and the melt index of the EVA is tested according to the ISO1133-2011 method.
[0030] Preferably, the polyolefin resin thermoplastic elastomer has a melt index of 1 to 10 g / 10 min at 190° C. and 2.16 kg.
[0031] Preferably, the melt index of the PE resin at 190° C. and 2.16 kg is 1 to 10 g / 10 min, and the melt index of the PE resin is tested according to ISO1133-2011 method.
[0032] Preferably, the melt index of the EVA is 3-7 g / 10 min at 190° C. and 2.16 kg, and the melt index of the EVA is tested according to the ISO1133-2011 method.
[0033] Preferably, the polyolefin resin thermoplastic elastomer has a melt index of 1 to 5 g / 10 min at 190° C. and 2.16 kg.
[0034] Preferably, the melt index of the PE resin at 190° C. and 2.16 kg is 1 to 5 g / 10 min, and the melt index of the PE resin is tested according to ISO1133-2011 method.
[0035] Preferably, the silane-grafted polyolefin includes at least one of silane-grafted PE, silane-grafted POE and silane-grafted EVA.
[0036] Preferably, the silane-grafted polyolefin includes silane-grafted PE and silane-grafted POE, and the weight ratio of the silane-grafted PE to the silane-grafted POE is 1:(1-4).
[0037] The inventors further discovered in their research that the silane-grafted polyolefin can better balance the softness and wear resistance when using silane-grafted PE and silane-grafted POE.
[0038] Preferably, the silane in the silane-grafted polyolefin includes at least one of vinyltrimethoxysilane, vinyltriethoxysilane, 3-methacryloxypropyltrimethoxysilane, vinyldimethylmethoxysilane, vinylmethyldibutoxysilane and γ-(meth)acryloxypropyltrimethoxysilane.
[0039] Preferably, the weight ratio of the silane-grafted PE to the silane-grafted POE is 1:2.
[0040] Preferably, the hydrogen-containing silicone oil includes at least one of terminal hydrogen-containing silicone oil (Si-H located at both ends of the molecular chain), side hydrogen-containing silicone oil (Si-H located at the side of the molecular chain), and terminal side hydrogen-containing silicone oil (Si-H located at both ends and the side of the molecular chain).
[0041] Preferably, the hydrogen content of the hydrogen-containing silicone oil is 0.5% to 2%, and the hydrogen content of the hydrogen-containing silicone oil is obtained by infrared spectroscopy. The addition of the hydrogen-containing silicone oil can be cross-linked under a catalyst to serve as a cross-linking point of silicone rubber, thereby further improving the aging resistance and wear resistance of silicone rubber, especially when the hydrogen content is 1.3% to 1.8%, the effect is better.
[0042] Preferably, the cross-linking auxiliary agent includes at least one of triallyl isocyanurate, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate.
[0043] Preferably, the catalyst comprises a Pt catalyst.
[0044] Preferably, the invention further comprises 50 to 100 parts of a flame retardant and 1 to 4 parts of an auxiliary agent, wherein the auxiliary agent comprises at least one of an anti-copper agent and an antioxidant.
[0045] Preferably, the copper inhibitor comprises a hydrazide metal passivator. Preferably, the antioxidant comprises at least one of a hindered phenol antioxidant, a hindered amine antioxidant, a phosphite antioxidant, and a thioester antioxidant.
[0046] Further preferably, the antioxidant includes at least one of antioxidant 1790, antioxidant 168, and antioxidant DLTDP.
[0047] Preferably, the flame retardant includes at least one of aluminum hydroxide, magnesium hydroxide, and aluminum hypophosphite. Further preferably, the cross-linked polyolefin material further includes the following components in parts by weight: 1-2 parts of an anti-copper agent, 1-2 parts of an antioxidant, and 50-100 parts of a flame retardant.
[0048] The present invention also provides a method for preparing the cross-linked polyolefin material, comprising the following steps:
[0049] Add silicone rubber, catalyst and hydrogen-containing silicone oil into a banbury mixer and knead them. After kneading, they enter a single screw and are extruded and granulated at 100-140°C to obtain a mixed material.
[0050] The mixed material and the remaining materials in the formula are added to the internal mixer again, and after being internally kneaded to 140-160° C., they are transferred to a twin-screw extruder at an extrusion temperature of 120-140° C.; finally, they are extruded and granulated by a single-screw extruder at 140-160° C. to finally obtain a cross-linked polyolefin material.
[0051] The present invention also provides a use of the soft cross-linked polyolefin material described above in the preparation of cable materials and / or wire and cable materials.
[0052] The beneficial effects of the present invention are as follows: (1) The cross-linked polyolefin material of the present invention uses PE resin, EVA resin and polyolefin resin thermoplastic elastomer as matrix resin, and by adding silane grafted polyolefin, silicone rubber and hydrogen-containing silicone oil, under the joint action of each component, a cross-linked polyolefin material with excellent wear resistance and softness is obtained, and the cross-linked polyolefin material has excellent aging resistance; (2) The Shore hardness of the cross-linked polyolefin material of the present invention is lower than 79A, and the number of wear resistance is greater than 3000 times, which shows that the cross-linked polyolefin of the present invention has excellent wear resistance and softness, and can be widely used in the preparation of cable materials and / or cable materials; after aging at 175°C×240h, the elongation at break decreases by less than 38.7%, and the cross-linked polyolefin material has excellent aging resistance. DETAILED DESCRIPTION
[0053] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present invention in detail, rather than to limit the present invention. All other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0054] The raw materials used in the embodiments and comparative examples are described as follows:
[0055] PE resin: The melt flow rate at 190°C and 2.16 kg is 3.8 g / 10 min, Exxon
[0056] LLDPE 3812PA.
[0057] Polyolefin resin thermoplastic elastomer (hereinafter referred to as POE resin): according to ISO1133-2011 method, the melt flow rate at 190°C and 2.16kg is 0.5g / 10min, Dow Chemical POE 58750.
[0058] EVA-1: The melt flow rate at 190°C and 2.16kg is 7g / 10min, the VA content is 26%, EVA 7470M from Taiwan Plastics Industry Co., Ltd.
[0059] EVA-2: The melt flow rate at 190°C and 2.16kg is 3g / 10min, the VA content is 18%, EVA 7350M from Taiwan Plastics Industry Co., Ltd.
[0060] EVA-3: The melt flow rate at 190°C and 2.16kg is 3g / 10min, the VA content is 40%, DuPont ELVAX 40L-03.
[0061] EVA-4: The melt flow rate at 190°C and 2.16kg is 2g / 10min, the VA content is 14%, Beijing Organic, EVA 14-2.
[0062] EVA-5: VA content is 50%, ARLANXEO High Performance Elastomer Co., Ltd. LEVAPREN 500.
[0063] Silicone rubber-1: Methyl vinyl silicone rubber, vinyl content: 0.19-0.24%, Dongjue Silicone (Nanjing) Co., Ltd., 110-3.
[0064] Silicone rubber-2: methyl vinyl silicone rubber, vinyl content: 0.25-0.49%, Dongjue Silicone (Nanjing) Co., Ltd., 110-4.
[0065] Silicone rubber-3: Methyl vinyl silicone rubber, vinyl content: 1.0-1.70%, Dongjue Silicone (Nanjing) Co., Ltd., 110-6.
[0066] Silicone rubber-4: methyl vinyl silicone rubber, vinyl content: 0.13-0.18%, Dongjue Silicone (Nanjing) Co., Ltd., 110-2.
[0067] Silicone rubber-5: methyl vinyl silicone rubber, vinyl content: 3.0-5.0%, Dongjue Silicone (Nanjing) Co., Ltd., 110-7.
[0068] Silicone rubber-6: Methyl silicone rubber, Dongjue Silicone (Nanjing) Co., Ltd., 101.
[0069] Silane grafted PE: DFDA 5451NT, Dow Chemical.
[0070] Silane grafted POE: R1020, Coase Chemical Co., Ltd.
[0071] Silane grafted EVA: PK 500N, Mitsubishi Chemical.
[0072] Hydrogen-containing silicone oil: hydrogen content is 1.6%, KF-99, Shin-Etsu Chemical Co., Ltd.
[0073] Crosslinker: triallyl isocyanurate.
[0074] Anti-copper agent: MD-1024 anti-copper agent, BASF.
[0075] Antioxidants: antioxidant 1790, antioxidant 168 and antioxidant DLTDP, mass ratio 3:1:2.
[0076] Catalyst: Pt catalyst, Shenzhen Ousibang New Materials Co., Ltd.
[0077] Unless otherwise specified, the components and raw materials used in the embodiments and comparative examples of the present invention are all commercially available raw materials, and the components and raw materials used in each parallel experiment are all of the same kind.
[0078] Performance Test:
[0079] The cross-linked polyolefin materials of the embodiments and comparative examples were subjected to performance tests, and the specific test methods are as follows:
[0080] Sample preparation: The cross-linked polyolefin materials of the embodiment and the comparative example were pressed on a flat vulcanizer at 180°C*15min to obtain 1mm and 3mm samples at a pressure of 15MPa. After successful sample preparation, they were irradiated and cross-linked for 16h and tested.
[0081] Testing: The special materials of the embodiments and comparative examples were tested according to the following method (see Table 1). The test results are shown in Table 4 below.
[0082] Table 1 Performance test methods
[0083]
[0084] Embodiment and comparative example:
[0085] The components and weight parts of the cross-linked polyolefin materials of the embodiments and comparative examples are shown in Table 2 and Table 3 (all parts are by weight in the tables).
[0086] The preparation methods of the cross-linked polyolefin materials of the embodiment and the comparative example both include the following steps:
[0087] Firstly, silicone rubber, hydrogenated silicone oil, Pt catalyst and antioxidant are added to a banbury mixer for internal kneading. After the internal kneading, they are put into a single-screw extruder for granulation at a temperature of 100-140°C. Then, the prepared silicone rubber particles and the remaining materials in the formula are added into the banbury mixer again, kneaded to 140-160°C, and then transferred to a twin-screw extruder at an extrusion temperature of 120-140°C. Finally, a single-screw extruder is used for granulation at a temperature of 140-160°C to finally obtain a cross-linked polyolefin material.
[0088] Table 2
[0089]
[0090]
[0091] Table 3
[0092]
[0093]
[0094] Table 4
[0095]
[0096]
[0097] It can be seen from Table 4 that the cross-linked polyolefin material of the present invention has excellent wear resistance and softness, and the cross-linked polyolefin material also has excellent aging resistance.
[0098] Among them, the Shore hardness of the cross-linked polyolefin material described in the present invention is lower than 79A, and the wear resistance number is greater than 3000 times, which shows that the cross-linked polyolefin of the present invention has excellent wear resistance and softness, and can be widely used in the preparation of cable materials and / or cable materials; after aging at 175°C × 240h, the elongation at break decreases by less than 38.7%, and it also has excellent aging resistance.
[0099] By comparing Example 2 with Examples 8 to 10, it can be seen that in the present invention, the combination of silane-grafted PE and silane-grafted POE has a more excellent effect and further improves the performance.
[0100] By comparing Example 2 with Comparative Examples 1 to 2, it can be seen that the use of the EVA resin of the present invention having a VA content of 18% to 40% can further improve the performance. If the VA content is lower than 18%, the PE content in the EVA will be high, the material hardness will increase, the elongation will decrease, and the softness requirement cannot be met. If the EVA content is too high, the wear resistance will deteriorate. Therefore, in the present invention, the VA content needs to be controlled between 18% and 40%.
[0101] By comparing Example 2 with Comparative Example 3, it can be seen that silicone rubber is an indispensable raw material in the present invention. Without silicone rubber, the performance will be significantly reduced and the requirements will not be met.
[0102] By comparing Example 2 with Comparative Examples 5 to 6, it can be seen that the silicone rubber not only needs to contain vinyl, but also the vinyl content needs to be in the range of 0.12% to 1.79%. Within this range, the material has good softness and wear resistance. If the vinyl content is too low, the silicone rubber has insufficient crosslinking and poor wear resistance. If the vinyl content is too high, the crosslinking degree is too high, resulting in reduced flexibility of the molecular chain, insufficient softness, and a harder material.
[0103] By comparing Example 2 with Comparative Example 7, it can be seen that if a rubber not containing vinyl groups is used, the performance will be reduced. This is because it does not contain vinyl groups and its compatibility in the system is very poor, which leads to negative effects.
[0104] By comparing Example 2 with Comparative Examples 8 to 9, it can be seen that if the amount of silane grafted material added is too large, the molecular chains will be too tightly entangled, thereby causing the elongation of the material to decrease and the hardness to increase. If the amount added is too small, the compatibility of silicone rubber and polyolefin resin will be insufficient, and the performance and wear resistance of the material will be poor. Therefore, it is necessary to control the amount of silane grafted polyolefin added.
[0105] By comparing Example 2 with Comparative Example 10, it can be seen that the present invention further improves the aging resistance and wear resistance of silicone rubber by adding hydrogen-containing silicone oil.
[0106] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A cross-linked polyolefin material, characterized in that: The invention comprises the following components in parts by weight: 5 to 10 parts of PE resin, 15 to 30 parts of EVA resin, 15 to 25 parts of polyolefin resin thermoplastic elastomer, 13 to 45 parts of silicone rubber, 5 to 10 parts of silane grafted polyolefin, 1 to 2 parts of crosslinking aid, 0.5 to 2 parts of hydrogen-containing silicone oil, and 0.5 to 2 parts of catalyst; The vinyl content of the silicone rubber is 0.12% to 1.79%; The VA content of the EVA resin is 15% to 43%; The silane-grafted polyolefin includes at least one of silane-grafted PE, silane-grafted POE, and silane-grafted EVA; Hydrogen-containing silicone oil can be cross-linked under the catalyst and exist as the cross-linking point of silicone rubber; The cross-linking auxiliary agent includes at least one of triallyl isocyanurate, trimethylolpropane triacrylate and trimethylolpropane trimethacrylate.
2. The cross-linked polyolefin material according to claim 1, characterized in that: The silicone rubber includes at least one of methyl vinyl silicone rubber, methyl phenyl vinyl silicone rubber, methyl β-cyano vinyl silicone rubber, and trifluoropropyl methyl vinyl silicone rubber.
3. The cross-linked polyolefin material according to claim 1, characterized in that: The vinyl content in the silicone rubber is 0.19% to 1.70%.
4. The cross-linked polyolefin material according to claim 1, characterized in that: The silane-grafted polyolefin includes silane-grafted PE and silane-grafted POE, and the weight ratio of the silane-grafted PE to the silane-grafted POE is 1:(1-4).
5. The cross-linked polyolefin material according to claim 1, characterized in that: The hydrogen content of the hydrogen-containing silicone oil is 0.5% to 2%.
6. The cross-linked polyolefin material according to claim 1, characterized in that: The invention also comprises 50 to 100 parts of flame retardant and 1 to 4 parts of auxiliary agent, wherein the auxiliary agent comprises at least one of an anti-copper agent and an antioxidant.
7. The method for preparing the cross-linked polyolefin material according to claim 6, characterized in that: The following steps are involved: Add silicone rubber, catalyst and hydrogen-containing silicone oil into a banbury mixer and knead them. After kneading, they enter a single screw and are extruded and granulated at 100-140°C to obtain a mixed material. The mixed material and the remaining materials in the formula are added to the internal mixer again, and after being internally kneaded to 140-160° C., they are transferred to a twin-screw extruder at an extrusion temperature of 120-140° C.; finally, they are extruded and granulated by a single-screw extruder at 140-160° C. to finally obtain a cross-linked polyolefin material.