A PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber, preparation and application
Through the pipe rod fading technology combined with quartz glass cladding and PIN-PMN-PT microcrystalline glass fiber core, the problem of difficult to prepare homogeneous, highly transmissive large-scale ferroelectric microcrystalline glass fibers in the prior art is solved, and the problem of difficult to prepare homogeneous, highly transmissive large-scale ferroelectric microcrystalline glass fibers is realized. It efficiently prepares long and controllable optical fibers, has excellent light transmittance and nonlinear properties, and is suitable for nonlinear optical devices.
Patent Information
- Application Number
- CN202311401660.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-26
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-10-26
AI Technical Summary
The prior art is difficult to prepare homogeneous, highly transmissive, large-volume PIN-PMN-PT ferroelectric microcrystalline glass fibers, and it is difficult to regulate their size and performance.
Glass fiber drawing technology using tube rod method, combining quartz glass cladding and PIN-PMN-PT microcrystalline glass fiber core, microcrystalline glass thin rods are prepared by melting and heat treatment, and wire drawing in a graphite furnace to form continuous glass Cladding and microcrystalline fibers achieve efficient preparation.
A standard optical fiber with a diameter of about 125μm, a controllable core diameter, a light transmittance of up to 80-99%, and a hundred times that of quartz fiber. It is suitable for the transmission of all-fiber waveguides of nonlinear optical devices.
Smart Images

Figure CN117383817B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of novel functional optical fiber materials, and specifically relates to a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber, and its preparation and application. Background Art
[0002] Ferroelectric materials are materials with ferroelectric effect, which are widely used in the fields of electricity, optics, magnetism, etc. In the field of electricity, ferroelectric materials can be used to manufacture new storage devices, such as ferroelectric memory and random access memory, which have the advantages of fast speed, low power consumption, and high reliability; ferroelectric materials can also be used to manufacture ferroelectric sensors, ferroelectric controllers and other devices to achieve intelligent control. In the field of optics, ferroelectric materials can be used to manufacture ferroelectric liquid crystal displays, organic light-emitting diodes and other displays, which have the advantages of wide viewing angle, low power consumption, and bright colors; in addition, ferroelectric materials are also expected to be used to manufacture ferroelectric fiber-integrated modulators, lasers, sensors and other equipment to achieve high-precision, broadband, high-speed communication and measurement.
[0003] PIN-PMN-PT is a relaxor ferroelectric crystal material that has been widely used in piezoelectric materials and devices such as medical ultrasound probes and ocean sonar torpedoes. After AC polarization, PIN-PMN-PT single crystals have high transparency and high voltage electrical properties. At the same time, they have excellent electro-optic modulation performance and nonlinear optical properties, which put high-performance piezoelectric crystals in the ranks of optical devices and opened the door to the design of new acousto-optic-electric devices (Liu X, Tan P, Ma X, et al. Ferroelectric crystals with giant electro-optic property enabling ultracompact Q-switches [J]. Science, 2022, 376: 371-377). So far, there has been no report on optical fiber materials composited with PIN-PMN-PT related crystals and glass. In 2020, Yang Zhongmin and others invented ferroelectric glass-ceramics (Yang Zhongmin, Shi Zhenguo, Zhou Shifeng, A Bi2GeO5 ferroelectric glass-ceramics with continuous and tunable ferroelectric properties and its preparation method [P], Chinese Invention, 2020, CN111533457A), and prepared ferroelectric glass with Bi2GeO5 crystals using heat treatment crystallization technology; however, the ferroelectric glass-ceramics prepared by this heat treatment crystallization technology mainly precipitates on the surface, and its size is difficult to control, making it difficult to use to achieve homogeneous, highly transmittance, large-scale adjustable ferroelectric glass-ceramics and its optical fiber preparation. Summary of the invention
[0004] In order to overcome the shortcomings of the above-mentioned prior art, the purpose of the present invention is to provide a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber, preparation and application, which fully combines the performance advantages of high nonlinearity of ferroelectric ceramic crystals and high transmittance of glass cladding materials, and adopts the glass fiber drawing technology of the tube-rod method to prepare ferroelectric microcrystalline glass optical fiber, so as to achieve homogeneous, high transmittance, and large-scale preparation of ferroelectric microcrystalline glass optical fiber.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is:
[0006] A PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber, wherein the composite optical fiber cladding material is quartz glass and the core material is (0.2+x)Pb(In 1 / 2 Nb 1 / 2 )O3–(0.5-x)Pb(Mg 1 / 3 Nb 2 / 3 )O3–0.3PbTiO3(PIN-PMN-PT,0≤x≤0.1) glass-ceramics.
[0007] A method for preparing a PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber comprises the following steps:
[0008] 1) Fiber core glass melting and processing: PIN-PMN-PT ferroelectric ceramic powder and raw material SiO2 powder are mixed evenly according to (5-6):1, melted at 1300℃-1400℃, quenched, and heat-treated to obtain microcrystalline glass, which is then processed into a fiber core microcrystalline glass rod;
[0009] 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame or drawing tower to heat and draw a cone to seal one end of the center hole of the quartz glass tube, leaving a slender tail cone, and then fill the core microcrystalline glass thin rod into the center hole of the glass tube to form an optical fiber preform;
[0010] 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. During the heating process, argon gas is passed through the furnace for protection. The temperature is about 1900℃-1950℃ when the tail cone is drawn to obtain a continuous glass-clad microcrystalline glass optical fiber. The fiber diameter is adjusted by the glass tube feeding speed and the fiber traction wheel speed parameters.
[0011] The invention discloses an application of a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber, which is suitable for single-mode transmission of all-optical fiber waveguides in various nonlinear optical devices or preparation of optical fiber devices.
[0012] Compared with the prior art, the present invention has the following beneficial effects:
[0013] (1) The present invention combines the advantages of glass and PIN-PMN-PT ceramic crystals to prepare homogeneous and adjustable ferroelectric microcrystalline optical fiber materials through tube-rod drawing. The continuous length of the optical fiber core reaches more than meters and is easy to mass produce. The selection of materials can meet the preparation requirements of this composite optical fiber. The quartz glass used as the optical fiber cladding has a glass softening temperature of more than 1400°C, and the tail cone is left to reduce the drawing temperature as much as possible. The PIN-PMN-PT microcrystalline glass used as the optical fiber core has a melting point of less than 1400°C.
[0014] (2) The ferroelectric microcrystalline glass optical fiber of the present invention, with the help of efficient optical fiber drawing, can obtain a standard optical fiber with a length of kilometers and a diameter of about 125 μm, and the core diameter is controllable; the main matrix of the glass optical fiber material is quartz glass, and its transmittance in the visible light band of 0.5 to 2 μm is as high as 80-99%, and the optical fiber has good flexibility and thermodynamic stability.
[0015] (3) The nonlinearity of the small-core ferroelectric optical fiber of the present invention can reach hundreds of times that of quartz optical fiber, and can be fused with standard quartz optical fiber. It is suitable for all-fiber waveguide transmission in nonlinear optical devices in the visible to near-infrared light band, and has high nonlinearity and low loss. BRIEF DESCRIPTION OF THE DRAWINGS
[0016] Figure 1 The present invention is a flowchart of a preparation method according to an embodiment of the present invention.
[0017] Figure 2 These are photos of the core glass and optical fiber of Examples 1 and 2 of the present invention.
[0018] Figure 3 This is a diagram of the light transmittance of the core glass of Examples 1 and 2 of the present invention. DETAILED DESCRIPTION
[0019] In order to better understand the present invention, the technical solution of the present invention is further explained below in conjunction with examples, but the implementation methods of the present invention are not limited thereto. For process parameters not particularly described, conventional techniques can be used.
[0020] Example 1, a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber, the composite optical fiber cladding material is quartz glass, the core material is 0.2Pb (In 1 / 2 Nb 1 / 2 )O3–0.5Pb(Mg 1 / 3 Nb 2 / 3 )O3–0.3PbTiO3(PIN-PMN-PT) glass-ceramics.
[0021] like Figure 1 As shown, a method for preparing a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber comprises the following steps:
[0022] 1) Core glass melting and processing: Synthesized 0.2PIN-0.5PMN-0.3PT ferroelectric ceramic powder and raw material SiO2 powder (5N) were mixed evenly at a mass ratio of 5:1, melted and quenched at 1400℃, and annealed at 550℃ to produce glass; the glass photo is shown in the figure. Figure 2 The glass in the middle left picture shows that the optical fiber has good light transmittance, and then the glass is processed into a thin rod of microcrystalline glass with a fiber core;
[0023] 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame or drawing tower to heat and draw a cone to seal one end of the center hole of the quartz glass tube, leaving a slender tail cone, and then fill the core microcrystalline glass thin rod into the center hole of the glass tube to form an optical fiber preform;
[0024] 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. During the heating process, argon gas is passed through the drawing furnace for protection. The drawing temperature of the traction tail cone is 1930°C. At this temperature, the glass of the fiber preform is in a viscous flow state, while the core microcrystalline glass in the center hole of the glass tube is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PIN-PMN-PT microcrystalline optical fiber. The fiber diameter is adjusted by the glass tube feeding speed and the fiber traction wheel speed parameters.
[0025] An application of a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber is suitable for single-mode transmission of all-fiber waveguides in various nonlinear optical devices, or preparation of optical fiber devices; the light transmittance of the optical fiber core glass in this embodiment is as follows Figure 3 As shown, it can be seen that the light transmittance in the 0.5 to 2 μm band is greater than 90%, and the measured nonlinearity is more than 100 times that of quartz optical fiber. It is expected to be used in the transmission of visible to infrared light and nonlinear applications.
[0026] The beneficial effects of this embodiment are as follows: PIN-PMN-PT microcrystalline glass can be melted in one step with high efficiency index, and then composited with quartz and drawn into microcrystalline glass optical fiber, and the process is easy to mass produce. The light transmittance in the 0.5 to 2μm band is greater than 90%, indicating that the optical fiber has good light transmittance. At the same time, the nonlinearity measured is more than 100 times that of quartz optical fiber, which is expected to promote the application of PIN-PMN-PT microcrystalline glass optical fiber in the transmission of visible to infrared light and nonlinear applications.
[0027] Example 2, a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber, the composite optical fiber cladding material is quartz glass, the core material is 0.2Pb (In 1 / 2 Nb 1 / 2 )O3–0.5Pb(Mg 1 / 3 Nb 2 / 3 )O3–0.3PbTiO3(PIN-PMN-PT) glass-ceramics.
[0028] A method for preparing a PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber comprises the following steps:
[0029] 1) Core glass melting and processing: Synthesized 0.2PIN-0.5PMN-0.3PT ferroelectric ceramic powder and raw material SiO2 powder (5N) were mixed evenly in a mass ratio of 6:1, melted and quenched at 1300℃, and annealed at 550℃ to produce glass; the glass photo is shown in the figure. Figure 2 The glass in the middle right picture shows that the optical fiber has good light transmittance, and then the glass is processed into a thin rod of microcrystalline glass with a fiber core;
[0030] 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame or drawing tower to heat and draw a cone to seal one end of the center hole of the quartz glass tube, leaving a slender tail cone, and then fill the core microcrystalline glass thin rod into the center hole of the glass tube to form an optical fiber preform;
[0031] 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. During the heating process, argon gas is passed through the drawing furnace for protection. The drawing temperature of the traction tail cone is 1900°C. At this temperature, the glass of the fiber preform is in a viscous flow state, while the core microcrystalline glass in the center hole of the glass tube is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PIN-PMN-PT microcrystalline optical fiber. The optical fiber diameter is adjusted by the glass tube feeding speed and the optical fiber traction wheel speed parameters.
[0032] An application of a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber is suitable for single-mode transmission of all-fiber waveguides in various nonlinear optical devices, or preparation of optical fiber devices; the light transmittance of the optical fiber core glass in this embodiment is as follows Figure 3 As shown, it can be seen that the core glass has high transmittance (up to 80%) in the 0.5 to 2 μm band, and the measured nonlinearity is more than 100 times that of silica fiber. It is expected to be used for transmission of visible to infrared light and high nonlinear applications.
[0033] The beneficial effects of this embodiment are as follows: the beneficial effects of Embodiment 2 are similar to those of Embodiment 1.
[0034] Example 3, a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber, the composite optical fiber cladding material is quartz glass, the core material is 0.3Pb (In 1 / 2 Nb 1 / 2 )O3–0.4Pb(Mg 1 / 3 Nb 2 / 3 )O3–0.3PbTiO3(PIN-PMN-PT) glass-ceramics.
[0035] A method for preparing a PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber comprises the following steps:
[0036] 1) Fiber core glass melting and processing: using the synthesized 0.3PIN-0.4PMN-0.3PT ferroelectric ceramic powder and the raw material SiO2 powder (5N), the mixture is uniformly mixed in a mass ratio of 5.5:1, melted and quenched at 1350°C, annealed at 550°C to obtain glass, and then processed into a fiber core microcrystalline glass rod;
[0037] 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame or drawing tower to heat and draw a cone to seal one end of the center hole of the quartz glass tube, leaving a slender tail cone, and then fill the core microcrystalline glass thin rod into the center hole of the glass tube to form an optical fiber preform;
[0038] 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. During the heating process, argon gas is passed through the drawing furnace for protection. The drawing temperature of the traction tail cone is 1950°C. At this temperature, the glass of the fiber preform is in a viscous flow state, while the core microcrystalline glass in the center hole of the glass tube is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PIN-PMN-PT microcrystalline optical fiber. The fiber diameter is adjusted by the glass tube feeding speed and the fiber traction wheel speed parameters.
[0039] The application of a PIN-PMN-PT ferroelectric microcrystalline glass composite optical fiber is suitable for the transmission of all-fiber waveguides in various nonlinear optical devices or the preparation of highly nonlinear optical fiber devices.
[0040] The beneficial effects of this embodiment are as follows: the beneficial effects of Embodiment 3 are similar to those of Embodiment 1.
Claims
1. A PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber, characterized in that: The composite optical fiber cladding material is quartz glass, and the core material is (0.2+x)Pb(In 1 / 2 Nb 1 / 2 )O3– (0.5-x)Pb(Mg 1 / 3 Nb 2 / 3 )O3– 0.3PbTiO3(PIN-PMN-PT) glass-ceramics, 0≤x≤0.
1.
2. The method for preparing a PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber according to claim 1, characterized in that: The following steps are involved: 1) Fiber core glass melting and processing: Use PIN-PMN-PT ferroelectric ceramic powder and raw material SiO2 powder, mix them evenly according to (5-6): 1, melt, quench, and heat-treat the microcrystalline glass at 1300℃-1400℃, and then process them into fiber core thin rods; 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame or drawing tower to heat and draw a cone to seal one end of the center hole of the quartz glass tube, leaving a slender tail cone, and then fill the core microcrystalline glass thin rod into the center hole of the glass tube to form an optical fiber preform; 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. During the heating process, argon gas is passed through the furnace for protection. The temperature is 1900-1950°C when the tail cone is drawn to obtain a continuous glass-clad microcrystalline glass optical fiber. The fiber diameter is adjusted by the glass tube feeding speed and the fiber traction wheel speed parameters.
3. A PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber, characterized in that: The composite optical fiber cladding material is quartz glass, and the core material is 0.2Pb (In 1 / 2 Nb 1 / 2 )O3– 0.5Pb(Mg 1 / 3 Nb 2 / 3 )O3– 0.3PbTiO3(PIN-PMN-PT) glass-ceramics.
4. The method for preparing a PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber according to claim 3, characterized in that: The following steps are involved: 1) Core glass melting and processing: Use the synthesized 0.2PIN-0.5PMN-0.3PT ferroelectric ceramic powder and raw material SiO2 powder, mix them evenly in a mass ratio of 5:1, melt and quench at 1400℃, and anneal at 550℃ to obtain microcrystalline glass, which is then processed into core glass thin rods; 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame or drawing tower to heat and draw a cone to seal one end of the center hole of the quartz glass tube, leaving a slender tail cone, and then fill the core microcrystalline glass thin rod into the center hole of the glass tube to form an optical fiber preform; 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. During the heating process, argon gas is passed through the furnace for protection. The temperature is 1900°C when the tail cone is pulled for drawing. At this temperature, the glass of the fiber preform is in a viscous flow state, while the core microcrystalline glass in the center hole of the glass tube is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PIN-PMN-PT microcrystalline optical fiber.
5. The method for preparing a PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber according to claim 3, characterized in that: The following steps are involved: 1) Core glass melting and processing: Use the synthesized 0.2PIN-0.5PMN-0.3PT ferroelectric ceramic powder and raw material SiO2 powder, mix them evenly in a mass ratio of 6:1, melt and quench at 1300℃, and anneal at 550℃ to obtain microcrystalline glass, which is then processed into core glass thin rods; 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame or drawing tower to heat and draw a cone to seal one end of the center hole of the quartz glass tube, leaving a slender tail cone, and then fill the core microcrystalline glass thin rod into the center hole of the glass tube to form an optical fiber preform; 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. Argon gas is passed through the furnace for protection during the heating process. The temperature is 1900°C when the tail cone is drawn. At this temperature, the glass of the fiber preform is in a viscous flow state, while the core microcrystalline glass in the center hole of the glass tube is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PIN-PMN-PT microcrystalline optical fiber. The fiber diameter is adjusted by the glass tube feeding speed and the fiber traction wheel speed parameters.
6. A PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber, characterized in that: The composite optical fiber cladding material is quartz glass, and the core material is 0.3Pb (In 1 / 2 Nb 1 / 2 )O3– 0.4Pb(Mg 1 / 3 Nb 2 / 3 )O3– 0.3PbTiO3(PIN-PMN-PT) glass-ceramics.
7. The method for preparing a PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber according to claim 6, characterized in that: The following steps are involved: 1) Core glass melting and processing: Use the synthesized 0.3PIN-0.4PMN-0.3PT ferroelectric ceramic powder and raw material SiO2 powder, mix them evenly at a mass ratio of 5.5:1, melt and quench at 1350℃, anneal at 550℃ to obtain microcrystalline glass, and then process the glass into core glass thin rods; 2) Assembly of optical fiber preform: Use hydrogen-oxygen flame or drawing tower to heat and draw a cone to seal one end of the center hole of the quartz glass tube, leaving a slender tail cone, and then fill the core microcrystalline glass thin rod into the center hole of the glass tube to form an optical fiber preform; 3) Fiber drawing: The assembled fiber preform is placed in a graphite furnace drawing tower for drawing. Argon gas is passed through the furnace for protection during the heating process. The temperature is 1950°C when the tail cone is drawn. At this temperature, the glass of the fiber preform is in a viscous flow state, while the core microcrystalline glass in the center hole of the glass tube is in a molten state. After hot drawing, the optical fiber is naturally cooled and solidified to form a continuous glass cladding and PIN-PMN-PT microcrystalline optical fiber. The fiber diameter is adjusted by the glass tube feeding speed and the fiber traction wheel speed parameters.
8. Application of a PIN-PMN-PT ferroelectric glass-ceramic composite optical fiber as claimed in claim 1, 3 or 6, characterized in that: It is suitable for single-mode transmission of all-fiber waveguides in various nonlinear optical devices, or for the preparation of optical fiber devices.