A method for preparing graphene-reinforced aluminum-based composite material by laser melting deposition
Graphene is mixed into Al-12Si alloy powder through laser fusion deposition technology to prepare high-density graphene-reinforced aluminum-based composite materials, which solves the problems of uneven composition and poor wear resistance of aluminum alloys and achieves excellent mechanical properties. and wear resistance, suitable for the production of complex components.
Patent Information
- Application Number
- CN202311387063.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-25
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2043-10-25
AI Technical Summary
The traditional casting process results in uneven aluminum alloy composition and coarse grains, resulting in poor wear resistance and low hardness. The production of complex components is also costly and takes a long time, which limits its further development in aerospace and other fields.
Using laser fusion deposition technology, graphene is mixed into Al-12Si alloy powder, and graphene-reinforced aluminum-based composite materials are prepared through laser fusion deposition printing. The graphene is ensured to be evenly dispersed through vacuum ball milling and sieving steps, and the printing parameters are adjusted to Obtain high-density composite materials.
The excellent mechanical properties and wear resistance of graphene-reinforced aluminum matrix composites are achieved, with a wear rate as low as 9mg/20min and a Vickers hardness value of 159.3HV, which solves the problems of low strength and poor wear resistance of aluminum alloys in traditional methods.
Smart Images

Figure CN117399639B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of additive manufacturing, and in particular relates to a method for preparing a graphene-reinforced aluminum-based composite material by laser melting deposition. Background Art
[0002] Graphene (GNPs) has special properties different from traditional materials, such as excellent chemical, mechanical and thermal conductivity. It has received widespread attention since its discovery. Studies have found that graphene can be used as a reinforcing phase to strengthen metal-based materials, thereby preparing composite materials with better performance. Aluminum and aluminum alloys are widely used in aerospace, rail transportation and other industries due to their low density, high strength, good plasticity and corrosion resistance. However, conventional casting processes usually have uneven composition and coarse grains, resulting in poor wear resistance, low hardness and other problems. In addition, when producing complex aluminum alloy components, the cost is high and the production cycle is long, which greatly limits its further development. Summary of the invention
[0003] In view of the above problems existing in the prior art, the present invention proposes a method for preparing graphene-reinforced aluminum-based composite materials by laser melting deposition.
[0004] To achieve the above object, the present invention provides the following technical solutions:
[0005] A method for preparing a graphene-reinforced aluminum-based composite material by laser melting deposition, wherein the method comprises adding graphene into Al-12Si alloy powder and directly forming the graphene-reinforced aluminum-based composite material by laser melting deposition printing.
[0006] Laser melting deposition (LMD), as a kind of additive manufacturing technology, uses a high-energy laser beam to melt powder and stack it layer by layer. It can not only directly form high-precision and complex metal parts, but also its faster heating and cooling rates can obtain refined structures, solving the problems of existing manufacturing technology development and lengthy forming time, while also reducing the waste of metal materials.
[0007] The preparation of the graphene-reinforced aluminum-based composite material is to use Al-12Si alloy powder as the matrix powder and flake graphene as the reinforcement to prepare the bulk composite material by laser melting deposition, and the specific steps are as follows:
[0008] (1) mixing graphene powder with Al-12Si alloy powder to obtain GNPs / Al-12Si composite powder;
[0009] (2) The parameters of the laser melting deposition printer were adjusted to prepare a GNPs / Al-12Si composite material with high density and uniform graphene dispersion by laser melting deposition.
[0010] Furthermore, the Al-12Si alloy powder is spherical, with a particle size of 53-105 μm, and a chemical composition of 12.02 wt.% Si, 0.144 wt.% Fe, 0.006 wt.% Mn, 0.007 wt.% Zn, and the rest is Al. The graphene powder is a nano-sheet structure.
[0011] Furthermore, the graphene powder is mixed with the Al-12Si alloy powder according to the graphene mass fraction x (wt.%), wherein x=0.25-1, preferably x=0.25, 0.5, 1.
[0012] Furthermore, the GNPs / Al-12Si composite powder needs to be vacuum milled, and the vacuum milling equipment parameters are set as follows: rotation speed 260 rpm, ball-to-material ratio 10:1, and milling time 2 hours. The obtained composite powder also needs to be sieved and dried in a vacuum drying oven at 80° C. for 4 hours.
[0013] Furthermore, the 6063 aluminum alloy is used as a substrate, the substrate is cleaned and sandblasted, and the composite powder is poured into a powder feeding tank.
[0014] Furthermore, a three-dimensional model of the aluminum-based composite material to be prepared is constructed, the slicing software is imported, the number of prints and their placement is set, and the laser melting deposition printing parameters are set as follows: the spot diameter is 50 μm, the substrate is a 6063 aluminum alloy substrate with a size of 150 mm × 150 mm × 20 mm, the laser power is 800 W, the scanning speed is 360 mm / min, the scanning spacing is 0.8 mm, the layer thickness is 0.35 mm, and the path offset is 1 mm. The scanning strategy is strip scanning. During printing, each layer is rotated 45° and sliced, and then imported into the equipment software, the equipment molding chamber is closed and argon gas is introduced for deoxygenation so that the oxygen concentration in the molding chamber is less than 100 ppm, the laser is turned on, and printing begins after the laser is stabilized. The laser melting deposition is carried out in a laser additive manufacturing device.
[0015] The present invention also provides a graphene-reinforced aluminum-based composite material prepared by the method.
[0016] Compared with the prior art, the present invention has the following advantages and technical effects:
[0017] The present invention uses graphene as a reinforcing phase. When the composite material is subjected to external stress, graphene bears most of the stress, and interacts with the matrix in the form of a second phase in the matrix, which can effectively prevent dislocation movement, that is, a dislocation strengthening mechanism. In addition, the addition of graphene can significantly refine the matrix alloy structure, which can not only better block the occurrence of dislocations, but also effectively prevent the initiation and expansion of cracks. The present invention uses graphene as a reinforcing phase and mixes it into Al-12Si alloy powder. By strictly controlling the graphene addition amount, ball milling parameters and laser melting deposition printing parameters, the prepared composite material solves the problems of long forming time and material waste, and also obtains a forming material with excellent mechanical properties and wear resistance, and its wear rate can be as low as 9mg / 20min, and the Vickers hardness value can reach 159.3HV. The problem of low strength and poor wear resistance of aluminum alloys prepared by the current traditional method is solved. BRIEF DESCRIPTION OF THE DRAWINGS
[0018] The drawings constituting a part of the present application are used to provide a further understanding of the present application. The illustrative embodiments and descriptions of the present application are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0019] Figure 1 This is a schematic diagram of the working principle of the laser deposition melting forming equipment used in the present invention;
[0020] Figure 2 The microstructure morphology of the GNPs / Al-12Si composite material powder in Example 1;
[0021] Figure 3 The microstructure morphology of the GNPs / Al-12Si composite material in Comparative Example 1;
[0022] Figure 4 The microstructure morphology of the GNPs / Al-12Si composite material in Comparative Example 2;
[0023] Figure 5 The microstructure morphology of the GNPs / Al-12Si composite material in Comparative Example 3;
[0024] Figure 6 The microstructure morphology of the GNPs / Al-12Si composite material powder in Example 2;
[0025] Figure 7 The microstructure morphology of the GNPs / Al-12Si composite material powder in Example 3;
[0026] Figure 8 The microstructure morphology of the GNPs / Al-12Si composite material powder in Example 4;
[0027] Fig. 9 is the microstructure diagram of the GNPs / Al-12Si composite material in Example 1;
[0028] Fig.10 is the microstructure diagram of the GNPs / Al-12Si composite material in Example 2;
[0029] Fig.11 is the microstructure diagram of the GNPs / Al-12Si composite material in Example 3;
[0030] Fig.12 is the microstructure diagram of the GNPs / Al-12Si composite material in Example 4;
[0031] Fig.13 EBSD image of the GNPs / Al-12Si composite material in Example 1;
[0032] Fig.14 EBSD image of the GNPs / Al-12S composite material in Example 2;
[0033] Fig.15 is the Vickers hardness value of the GNPs / Al-12Si composite material in Examples 1-4;
[0034] Fig.16 is the wear rate of the GNPs / Al-12Si composite material in Examples 1-4. DETAILED DESCRIPTION
[0035] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.
[0036] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.
[0037] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.
[0038] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.
[0039] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.
[0040] The "room temperature" and "normal temperature" mentioned in the present invention are all calculated as 25±2°C unless otherwise specified.
[0041] The graphene-reinforced aluminum-based composite material prepared by laser melting deposition in the present invention has excellent dimensional accuracy and wear resistance. After testing, it was found that its Vickers hardness value at room temperature can reach up to 159.3HV, and the lowest wear rate is 9mg / 20min. The present invention solves the problem of low strength and poor wear resistance of aluminum alloys, and provides a new idea for the strengthening and further application of aluminum alloys.
[0042] In the embodiment of the present invention, the matrix powder is Al-12Si powder from Beijing Sanspuruixin Company, with a particle size of 53-105 μm, spherical powder particles, good fluidity, and the chemical composition of the powder by mass fraction is Si12.02wt.%, Fe 0.144wt.%, Mn 0.006wt.%, and Zn 0.007wt.%. The reinforcing phase is graphene from Changzhou Sixth Element Company, and its structure is a nano-sheet structure.
[0043] The present invention provides a method for preparing a graphene-enhanced aluminum-based composite material by laser melting deposition, wherein graphene is added to Al-12Si alloy powder, and the graphene-enhanced aluminum-based composite material is directly formed by laser melting deposition printing. The specific steps are as follows:
[0044] (1) mixing graphene powder with Al-12Si alloy powder to obtain GNPs / Al-12Si composite powder;
[0045] (2) vacuum ball milling, sieving and drying the obtained GNPs / Al-12Si composite powder;
[0046] (3) The parameters of the laser melting deposition printer were adjusted to prepare a GNPs / Al-12Si composite material with high density and uniform graphene dispersion by laser melting deposition.
[0047] In one embodiment of the present invention, the addition amount of the graphene powder is x (wt.%) of the total mass of (Al-12Si alloy powder + graphene powder), wherein x=0-1, preferably x=0, 0.25, 0.5, 1, and more preferably 0.5.
[0048] In one embodiment of the present invention, the vacuum ball mill is a MiQi YXQM-2L vacuum ball mill, and the ball milling parameters are: ball-to-material ratio 10:1; rotation speed 260 rpm, and ball milling time 2 h.
[0049] In one embodiment of the present invention, the laser additive manufacturing method is laser melting deposition (LMD), and its working principle is as follows: Figure 1 As shown. The BLT-C400 equipment (Xi'an, Bolit) equipped with a 1000WIPG fiber laser generator was used, the laser spot diameter was set to 50μm, the substrate was a 6063 aluminum alloy substrate with a size of 150mm×150mm×20mm, the laser power was 800W, the scanning speed was 360mm / min, and the scanning spacing and layer thickness were kept constant at 0.8mm and 0.35mm respectively. The scanning strategy was strip scanning, and each layer was rotated 45° during printing.
[0050] In the embodiment of the present invention, the density of the sample is measured by the Archimedes drainage method.
[0051] The following examples serve as further illustrations of the technical solutions of the present invention.
[0052] Example 1
[0053] Preparation of graphene reinforced aluminum matrix composites:
[0054] (1) The Al-12Si alloy powder was sieved through 300 mesh and 1000 mesh sieves to obtain a sample with an average particle size between 53 and 105 μm as a raw material. The graphene powder was mixed with the sieved Al-12Si alloy powder using a vacuum ball mill (the graphene addition amount was 0.5 wt.% of the total mass of (Al-12Si alloy powder + graphene powder)). The ball milling parameters were: ball-to-material ratio 10:1; rotation speed 260 rpm, ball milling time 2 h, to obtain a composite material powder;
[0055] (2) The composite material powder obtained in step (1) was sieved through 300 mesh and 1000 mesh sieves to ensure that the powder particle size used in the printing process was between 53 and 105 μm. After the sieving was completed, the sieved powder was placed in a glass container, which was placed in an oven and baked at 80° C. for 4 hours;
[0056] (3) Construct a three-dimensional model of the aluminum-based composite material to be prepared, import the slicing software, set the number of prints and their placement, and set the laser melting deposition printing parameters as follows: spot diameter 50μm, substrate selection 6063 aluminum alloy substrate with a size of 150mm×150mm×20mm, laser power 800W, scanning speed 360mm / min, scanning spacing 0.8mm, layer thickness 0.35mm, path offset 1mm. The scanning strategy is strip scanning, and each layer rotates 45° during printing. After the settings are completed, slices are performed, and then imported into the equipment software, the equipment molding chamber is closed and argon gas is introduced to deoxygenate so that the oxygen concentration in the molding chamber is less than 100ppm, the laser is turned on, and printing is started after the laser is stable, and finally a graphene-reinforced aluminum-based composite material is obtained.
[0057] Figure 2 This is a microstructure morphology diagram of the composite material powder obtained in Example 1. It can be seen from the figure that the mixed composite material powder has good sphericity and graphene is evenly adhered to its surface.
[0058] Example 2
[0059] Same as Example 1, except that the amount of graphene added is 0wt.% of the total mass of (Al-12Si alloy powder+graphene powder).
[0060] Example 3
[0061] Same as Example 1, except that the amount of graphene added is 0.25wt.% of the total mass of (Al-12Si alloy powder+graphene powder).
[0062] Example 4
[0063] Same as Example 1, except that the amount of graphene added is 1.0 wt.% of the total mass of (Al-12Si alloy powder+graphene powder).
[0064] Comparative Example 1
[0065] Same as Example 1, except that the vacuum ball milling time is 1 h.
[0066] Figure 3The microstructure morphology of the composite material prepared in this comparative example. The vacuum ball milling time determines the dispersion degree of graphene in the Al-12Si matrix powder and the sphericity of the powder. As in this comparative example, when the ball milling time is too short, the graphene cannot be evenly distributed in the Al-12Si. Since graphene has high strength, high absorptivity and high thermal conductivity, the temperature field of the molten pool is unevenly distributed and the flow of the molten pool is turbulent during the LMD forming process. Therefore, subsequent printing and performance testing of different graphene addition amounts were not carried out.
[0067] Comparative Example 2
[0068] Same as Example 1, except that the vacuum ball milling time is 3 h.
[0069] Comparative Example 3
[0070] Same as Example 1, except that the vacuum ball milling time is 4 h.
[0071] Figure 4 This is a microstructure morphology of the composite material prepared in Comparative Example 2. Figure 5 The microstructure morphology of the composite material prepared in Comparative Example 3. It can be found that when the ball milling time is too long, the impact of the grinding balls causes the powder to change from a spherical shape to an elliptical shape and develop into an irregular shape, and the powder fluidity is greatly reduced, which seriously affects the uniformity of the powder melting to fill the molten pool. Therefore, subsequent printing and performance testing with different graphene addition amounts were not carried out.
[0072] Effect verification:
[0073] 1. The composite material powders obtained in Examples 1-4 were subjected to electron microscopic morphology analysis. Figure 2 as well as Figure 6-8 , it can be seen that when the graphene addition amount is 0.5wt.%, the graphene is distributed relatively evenly in the Al-12Si powder.
[0074] The block samples prepared in Examples 1-4 were coarsely ground with #400, #800, and #1500 sandpapers, respectively, and then the sample surfaces were polished. The polished samples were ultrasonically cleaned with alcohol, and the treated samples were analyzed.
[0075] 2. Figure 9-12 The microstructure images of the composite materials prepared in Examples 1 to 4 are shown in FIG. 1 . As can be seen from the figure, the addition of graphene significantly refines the structure, and the refinement effect is particularly obvious when the addition amount of graphene is 0.5 wt.%.
[0076] 3. Fig.13 This is the electron backscatter diffraction (EBSD) image of the bulk composite material prepared in Example 1. Fig.14This is an EBSD image of the bulk composite material prepared in Example 2. As can be seen from the figure, the grains of the composite material with a graphene addition amount of 0.5wt.% are refined.
[0077] 4. The bulk composite material prepared in Example 1-4 was subjected to a Vickers hardness test. The Vickers hardness value was measured by a HXD-1000 microhardness tester with a load of 15 g and a holding time of 10 s. The test results are shown in FIG. Fig.15 It can be seen that the addition of graphene increases the hardness of the composite material, and the Vickers hardness value of the composite material with a graphene addition of 0.5 wt.% in Example 1 is as high as 159.3 HV.
[0078] 5. The block composite materials prepared in Examples 1-4 were subjected to room temperature reciprocating friction and wear tests using a Bruker UMT friction and wear tester. The relevant parameters included: a load of 10 N, a sliding speed of 0.06 m / s, and a test duration of 20 min. The wear rate was calculated by comparing the mass of the block before and after wear. The results are as follows: Fig.16 .from Fig.16 It can be seen that the wear rate of the composite material with a graphene addition amount of 0.5 wt.% in Example 1 is as low as 9 mg / 20 min.
[0079] In summary, the graphene reinforced aluminum-based composites prepared by laser melting deposition technology have excellent hardness and wear resistance.
[0080] Comparative Example 4
[0081] The same as Example 1, except that step (3) is: construct a three-dimensional model of the aluminum-based composite material to be prepared, import the slicing software, set the number of prints and their placement, and set the laser melting deposition printing parameters as follows: spot diameter 50μm, substrate selection 6063 aluminum alloy substrate with a size of 150mm×150mm×20mm, laser power 900W, scanning speed 300mm / min, scanning spacing 0.8mm, layer thickness 0.35mm, path offset 1mm. The scanning strategy is strip scanning, and each layer rotates 67° during printing. After the settings are completed, slices are performed, and then imported into the equipment software, the equipment molding chamber is closed and argon gas is introduced for deoxygenation so that the oxygen concentration in the molding chamber is less than 100ppm, the laser is turned on, and printing is started after the laser is stable, and finally a graphene-enhanced aluminum-based composite material is obtained.
[0082] The performance test method is the same as above. The results show that the wear rate of the composite material prepared in this comparative example is 10.4 mg / 20 min, and the Vickers hardness value is up to 135.3 HV.
[0083] The above are only preferred specific implementations of the present application, but the protection scope of the present application is not limited thereto. Any changes or substitutions that can be easily thought of by a person skilled in the art within the technical scope disclosed in the present application should be included in the protection scope of the present application. Therefore, the protection scope of the present application should be based on the protection scope of the claims.
Claims
1. A method for preparing graphene-reinforced aluminum-based composite materials by laser melting deposition, characterized in that: The method comprises the steps of adding graphene to Al-12Si alloy powder and directly forming a graphene-reinforced aluminum-based composite material by laser melting deposition printing; The graphene addition amount accounts for 0.25-1.0wt.% of the total mass of the raw materials; After the graphene is added to the Al-12Si alloy powder, vacuum ball milling is required, and the ball milling conditions are: rotation speed 260 rpm, ball-to-material ratio 10:1, and ball milling time 2 hours; The laser melting deposition printing parameters are as follows: spot diameter 50 μm, substrate selected 6063 aluminum alloy substrate with a size of 150 mm×150 mm×20 mm, laser power 800 W, scanning speed 360 mm / min, scanning spacing 0.8 mm, layer thickness 0.35 mm, path offset 1 mm, scanning strategy is strip scanning, each layer is rotated 45° during printing, and oxygen concentration is less than 100 ppm.
2. The method for preparing graphene-reinforced aluminum-based composite materials by laser melting deposition according to claim 1, characterized in that: The graphene is flake graphene.
3. The method for preparing graphene-reinforced aluminum-based composite materials by laser melting deposition according to claim 1, characterized in that: The Al-12Si alloy powder is spherical, with a particle size of 53-105 μm and a chemical composition of 12.02 wt.%, 0.144 wt.%, 0.006 wt.%, 0.007 wt.%, and the rest is Al.
4. A graphene-reinforced aluminum-based composite material prepared by the method according to any one of claims 1 to 3.
Citation Information
Patent Citations
Method for preparing graphene-enhanced aluminum matrix composite material by selective laser melting method
CN107299239A
Method for preparing graphene reinforced aluminum alloy material based on laser selective melting technology
CN110257657A
Graphene aluminum-based composite powder used for laser deposition manufacturing, and preparation method and application thereof
CN110666179A
LDM (laser deposition manufacturing) based graphene oxide aluminum matrix composite and preparation method thereof
CN110777277A
Method for improving obdurability of laser melting deposition aluminum alloy forming part
CN114086175A