Proton exchange membrane for fuel cell based on metal bipolar plate and preparation method thereof
Through the compounding technology of modified polyvinyl alcohol, carbon nanotubes, nano-silica, POSS and chitosan, a proton exchange membrane with high water absorption and low swelling rate is prepared, which solves the problem of hydrophilicity in the existing technology. It achieves excellent mechanical properties and proton conductivity by solving the problems of polymer material loss and poor electrical conductivity in aqueous environments.
Patent Information
- Application Number
- CN202311346313.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-10-18
AI Technical Summary
Existing proton exchange membranes suffer from slow loss of hydrophilic polymer materials and poor electrical conductivity when operating in a water environment, resulting in insufficient water resistance, mechanical properties and stability, and cannot meet market demand.
It adopts the compounding technology of modified polyvinyl alcohol with carbon nanotubes, nano-silica, glycidyl oxypropyl caged polysilsesquioxane (POSS) and chitosan and other raw materials, and opens the ring through epoxy compounds. , O-alkylation and esterification reactions to prepare proton exchange membranes with high water absorption and low swelling rate.
It significantly improves the mechanical properties, proton conductivity and stability of the membrane, while maintaining a high water absorption rate, significantly reducing the swelling rate, and meeting the performance requirements of fuel cells for proton exchange membranes.
Smart Images

Figure BDA0004498821790000021 
Figure BDA0004498821790000031 
Figure BDA0004498821790000091
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of fuel cells, and in particular relates to a proton exchange membrane for a fuel cell based on a metal bipolar plate and a preparation method thereof. Background Art
[0002] Proton exchange membrane fuel cells have the advantages of low operating temperature, fast start-up, high specific power, simple structure, and easy operation. They are recognized as the preferred energy source for electric vehicles, fixed power stations, etc. Inside the fuel cell, the proton exchange membrane provides a channel for the migration and transportation of protons, allowing protons to pass through the membrane from the anode to the cathode, forming a loop with the electron transfer of the external circuit, and providing current to the outside world. Therefore, the performance of the proton exchange membrane plays a very important role in the performance of the fuel cell, and its quality directly affects the service life of the battery.
[0003] The patent with application number CN201811272802.2 provides a cross-linked proton exchange membrane for vanadium batteries and a preparation method thereof. The invention first prepares sulfonated graphene powder by surface grafting, and then synthesizes sulfonated polybenzimidazole by polymerization reaction, and then mixes polyvinyl alcohol, sulfonated polybenzimidazole, and sulfonated graphene powder for cross-linking reaction, flows into film, and dries to obtain the cross-linked proton exchange membrane provided by the invention. The cross-linked proton exchange membrane not only has good proton conductivity and can reduce the permeability of vanadium ions, but also has good chemical stability and mechanical properties, and has low water absorption; the patent with application number 202110390109.0 provides a proton exchange membrane, a preparation method thereof, and an environmentally friendly fuel cell. The invention mixes carbon nanotube dispersion, silica sol, chitosan solution, and polyvinyl alcohol solution evenly, and then flows into film, dries, and then soaks in alkali solution and introduces ionic liquid and phosphotungstic acid, washes and dries to obtain a hybrid membrane, and then chitosan and polyethylene The enol mixed solution is coated on the surface of the hybrid membrane and immersed in a cross-linking agent solution for cross-linking to obtain a proton exchange membrane. The proton exchange membrane provided by the invention has good proton conductivity, mechanical properties and stability, and its preparation method is simple, the raw material cost is low, it is environmentally friendly, and it is conducive to industrial production; the above patents all add polyvinyl alcohol when preparing the proton exchange membrane. Polyvinyl alcohol has been widely used in polymer electrolyte films due to its potential charge transfer ability, alcohol resistance and excellent film-forming performance, but polyvinyl alcohol is a hydrophilic polymer material with strong water solubility, and fuel cells need to operate in the presence of water. The hydrophilic polymer material will slowly lose with the operation of the battery. In addition, polyvinyl alcohol also has problems such as poor conductivity and easy swelling. When it is made into a membrane material, because its molecular structure contains a large number of hydrophilic hydroxyl groups and has the characteristics of high crystallinity, the water resistance, mechanical properties and stability of the polyvinyl alcohol membrane material are poor, which cannot meet market demand. Summary of the invention
[0004] In view of the deficiencies in the prior art, the object of the present invention is to provide a proton exchange membrane for a fuel cell based on a metal bipolar plate, which has the characteristics of high water absorption and low swelling rate, and also has excellent mechanical properties, proton conductivity and stability; the present invention also provides a method for preparing the proton exchange membrane.
[0005] The technical solution adopted by the present invention to achieve the above-mentioned purpose is:
[0006] A proton exchange membrane for a fuel cell based on a metal bipolar plate comprises the following raw materials in parts by weight: 1-2 parts of carbon nanotubes, 5-15 parts of nano-silicon dioxide, 4-9 parts of glycidyloxypropyl cage-like polysilsesquioxane (POSS), 150-200 parts of chitosan, and 60-120 parts of modified polyvinyl alcohol; the preparation method of the modified polyvinyl alcohol is as follows:
[0007] S1. Disperse epoxybutyltrimethoxysilane in 2-methyltetrahydrofuran, add 2-pyridin-3-yl-3H-benzimidazole-5-carboxylic acid and chromium acetate in sequence, raise the temperature to 75-85° C., stir and react for 6-10 hours, filter, take the filtrate, distill under reduced pressure, and dry to obtain intermediate 1;
[0008] S2, dispersing the intermediate 1 obtained in step S1 in 2-methyltetrahydrofuran, adding 4-bromobutyric acid, potassium hydroxide, and benzyltriethylammonium chloride in sequence, heating to 55-70°C, stirring for reaction for 4-7h, cooling to room temperature, adjusting the pH to 6-7, filtering, taking the filtrate, distilling under reduced pressure, and drying to obtain intermediate 2;
[0009] S3, dispersing polyvinyl alcohol in dimethyl sulfoxide, heating to 85-100°C, stirring for 1-2h, cooling to 75-90°C, adding intermediate 2 obtained in step S2 and p-toluenesulfonic acid in sequence, continuing stirring for 5-9h, cooling to room temperature, separating the solid from the liquid, taking the solid, washing and drying, and obtaining the modified polyvinyl alcohol;
[0010] The synthetic route of modified polyvinyl alcohol is as follows:
[0011]
[0012]
[0013] The invention uses epoxybutyltrimethoxysilane and 2-pyridin-3-yl-3H-benzimidazole-5-carboxylic acid as starting materials, and under the action of chromium acetate, an epoxide compound undergoes a ring-opening reaction to obtain an intermediate 1; the intermediate 1 contains a hydroxyl structure, and under the action of potassium hydroxide and benzyltriethylammonium chloride, an O-alkylation reaction occurs with 4-bromobutyric acid to obtain an intermediate 2; under the action of p-toluenesulfonic acid, the intermediate 2 further undergoes an esterification reaction with polyvinyl alcohol to obtain modified polyvinyl alcohol.
[0014] In order to obtain modified polyvinyl alcohol and ensure the consistency of the product, the molar ratio of epoxybutyltrimethoxysilane, 2-pyridin-3-yl-3H-benzimidazole-5-carboxylic acid and chromium acetate in step S1 is 1.1-1.2:1:0.013-0.020, and the amount of epoxybutyltrimethoxysilane added to 2-methyltetrahydrofuran is 0.12-0.26 g / mL; the intermediate 1, 4-bromobutyric acid, hydroxide The molar ratio of potassium hydroxide and benzyltriethylammonium chloride is 1:0.8-1.0:0.7-1.2:0.04-0.08, and the amount of intermediate 1 added to 2-methyltetrahydrofuran is 0.1-0.3 g / mL; the mass ratio of polyvinyl alcohol, intermediate 2, and p-toluenesulfonic acid in step S3 is 10:0.8-1.5:0.1-0.2, and the amount of polyvinyl alcohol added to dimethyl sulfoxide is 0.08-0.16 g / mL.
[0015] The present invention also provides a method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate, comprising the following steps:
[0016] (1) dispersing carbon nanotubes in deionized water to obtain a carbon nanotube dispersion; dispersing nanosilica in deionized water to obtain a nanosilica dispersion; dispersing glycidyloxypropyl caged polysilsesquioxane (POSS) in ethanol to obtain a POSS dispersion; dispersing acetic acid in deionized water, mixing uniformly, and then adding chitosan, stirring and dissolving to obtain a chitosan solution; dispersing modified polyvinyl alcohol in deionized water to obtain a modified polyvinyl alcohol solution;
[0017] (2) mixing a carbon nanotube dispersion, a nanosilica dispersion, and a POSS dispersion, and stirring at room temperature for 3-7 hours to obtain a mixed solution 1; mixing a chitosan solution and a modified polyvinyl alcohol solution, and stirring at 55-70° C. for 5-10 hours to obtain a mixed solution 2; mixing the mixed solution 1 with the mixed solution 2, and continuing to stir at 55-65° C. for 2-5 hours, pouring into a mold to form a cast film, and drying to obtain a hybrid film;
[0018] (3) Soaking the hybrid membrane obtained in step (2) in an alkaline solution for 0.5-1.5 hours, taking it out, cleaning it, and drying it, and then soaking it in an ionic liquid for 10-15 hours, taking it out, cleaning it, and drying it.
[0019] The carbon nanotube has a highly delocalized large π bond, so that the addition of the carbon nanotube can expand the proton transmission channel and promote the proton conductivity. The present invention uses glycidyl ether oxypropyl caged polysilsesquioxane (POSS) as a dispersant or cosolvent for nanomaterials such as carbon nanotubes and nanosilica to enhance the dispersibility of the nanomaterials. By compounding with carbon nanotubes, nanosilica, chitosan and modified polyvinyl alcohol, the reinforcing effect can be fully exerted, and the inorganic particles can also be used as a bridge between organic polymers to improve the compatibility of the inorganic particles and the organic polymers, thereby improving the mechanical properties, thermal stability and proton conductivity of the product.
[0020] Furthermore, the mass fraction of the carbon nanotube dispersion in step (1) is 2-7%, the mass fraction of the nano-silicon dioxide dispersion is 1-6%, the mass fraction of the POSS dispersion is 0.2-2%, the mass ratio of acetic acid to chitosan in the chitosan solution is 0.7-1.4:1, the mass fraction of chitosan in the chitosan solution is 1-4%, and the mass fraction of the modified polyvinyl alcohol solution is 1-4%; the alkali solution in step (3) is a sodium hydroxide or potassium hydroxide aqueous solution, the mass fraction of the alkali solution is 20-40%, and the ionic liquid is 1-butyl-3-methylimidazole bistrifluoromethanesulfonimide.
[0021] The present invention has the following beneficial effects:
[0022] (1) The present invention synthesizes modified polyvinyl alcohol through the ring-opening reaction of epoxy compounds, O-alkylation reaction and esterification reaction in sequence, introduces ester groups, siloxanes, pyridine and benzimidazole into the side chains of polyvinyl alcohol, reduces the hydrophilic groups on the polyvinyl alcohol molecular chain, and significantly increases the intermolecular forces through π-π interactions, introduction of side chains, etc., thereby improving the mechanical properties and water resistance of the modified polyvinyl alcohol. In addition, the introduction of pyridine and benzimidazole structures also improves the conductivity and stability of the modified polyvinyl alcohol.
[0023] (2) The modified polyvinyl alcohol provided by the present invention has good compatibility with the various components of the raw materials. The modified polyvinyl alcohol and chitosan act synergistically to enhance the water retention, mechanical properties, and proton conductivity of the membrane product. The modified polyvinyl alcohol is then compounded with raw materials such as glycidyl ether oxypropyl cage polysilsesquioxane (POSS), carbon nanotubes, nano-silica, and ionic liquids. Through blending and cross-linking, the various components are combined in the form of chemical bonds or hydrogen bonds, which significantly improves the bonding strength between the components, thereby improving the mechanical properties, proton conductivity, and stability of the membrane product, and ensuring that the membrane product has a certain water absorption rate while significantly reducing its swelling rate. DETAILED DESCRIPTION
[0024] The following will be combined with the embodiments of the present application to clearly and completely describe the technical solutions in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this application.
[0025] Carbon nanotubes, multi-walled, purity 98%, tube diameter 15-25nm, purchased from Dazhan Nano (Guangdong) Co., Ltd.; nano-silicon dioxide, model CT-101, content 98%, specific surface area 185-205m 2 / g, purchased from Shouguang Changtai New Materials Co., Ltd.; glycidyl ether oxypropyl caged polysilsesquioxane (POSS), purity 99%, purchased from Xi'an Qiyue Biotechnology Co., Ltd.; chitosan, content 85-95%, deacetylation degree 85-95%, purchased from Shandong Fengtai Biotechnology Co., Ltd.; polyvinyl alcohol, model 17-99, viscosity 54-66mPa.s, purchased from Henan Yaoze Chemical Products Co., Ltd.; 1-butyl-3-methylimidazole bistrifluoromethanesulfonimide, density 1.44g / cm 3 , purchased from Jinan Xinda Chemical Co., Ltd.; the raw materials used in the following examples are all common commercially available products.
[0026] Example 1
[0027] A method for preparing modified polyvinyl alcohol comprises the following steps:
[0028] S1. Disperse epoxybutyltrimethoxysilane in 2-methyltetrahydrofuran, add 2-pyridin-3-yl-3H-benzimidazole-5-carboxylic acid and chromium acetate in sequence, heat to 80°C, stir to react for 7h, filter, take the filtrate, remove 2-methyltetrahydrofuran by vacuum distillation under reduced pressure, and dry under vacuum at 55°C for 24h to obtain intermediate 1, wherein the molar ratio of epoxybutyltrimethoxysilane, 2-pyridin-3-yl-3H-benzimidazole-5-carboxylic acid and chromium acetate is 1.1:1:0.015, and the amount of epoxybutyltrimethoxysilane added to 2-methyltetrahydrofuran is 0.15g / mL;
[0029] S2, dispersing the intermediate 1 obtained in step S1 in 2-methyltetrahydrofuran, adding 4-bromobutyric acid, potassium hydroxide, and benzyltriethylammonium chloride in sequence, heating to 60°C, stirring and reacting for 4-7h, cooling to room temperature, adjusting the pH to 6-7 with 98% concentrated sulfuric acid, filtering, taking the filtrate, removing 2-methyltetrahydrofuran by vacuum distillation under reduced pressure, and drying at 55°C in vacuo for 24h to obtain intermediate 2, wherein the molar ratio of intermediate 1, 4-bromobutyric acid, potassium hydroxide, and benzyltriethylammonium chloride is 1:0.9:0.8:0.07, and the amount of intermediate 1 added to 2-methyltetrahydrofuran is 0.2g / mL;
[0030] The NMR results of intermediate 2 are: 1 H NMR (300MHz, DMSO-d6) δ12.56 (s, 1H), 12.01 (s, 1H), 9.24 (s, 1H), 8.70 (d, 1H), 8.42(d, 1H), 8.13(s, 1H), 7.92(d, 1H), 7.74(d, 1H), 7.50-7.55(m, 1H) , 4.47-4.51(m, 1H), 4.20-4.25(m, 1H), 3.78-3.82(m, 1H), 3.55(s, 9H), 3. 35(t, 2H), 2.30(t, 2H), 1.70-1.77(m, 2H), 1.35-1.39(m, 2H), 0.56(t, 2H);
[0031] S3, disperse polyvinyl alcohol in dimethyl sulfoxide, heat to 95°C, stir for 1.5h, cool to 85°C, add intermediate 2 obtained in step S2 and p-toluenesulfonic acid in sequence, continue stirring for 7h, cool to room temperature, separate solid and liquid, take solid, wash with ether, and vacuum dry at 45°C for 24h to obtain modified polyvinyl alcohol, wherein the mass ratio of polyvinyl alcohol, intermediate 2, and p-toluenesulfonic acid is 10:0.9:0.12. The amount of polyvinyl alcohol added to the dimethyl sulfoxide is 0.12g / mL.
[0032] Example 2
[0033] A proton exchange membrane for a fuel cell based on a metal bipolar plate comprises the following raw materials in parts by weight: 1 part of carbon nanotubes, 8 parts of nano-silicon dioxide, 5 parts of glycidyloxypropyl cage-like polysilsesquioxane (POSS), 180 parts of chitosan, and 90 parts of modified polyvinyl alcohol.
[0034] A method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate comprises the following steps:
[0035] (1) dispersing carbon nanotubes in deionized water to obtain a carbon nanotube dispersion with a mass fraction of 1%; dispersing nanosilica in deionized water to obtain a nanosilica dispersion with a mass fraction of 2%; dispersing glycidyl ether oxypropyl caged polysilsesquioxane-POSS in ethanol to obtain a POSS dispersion with a mass fraction of 1.5%; dispersing acetic acid in deionized water, mixing evenly, and then adding chitosan, stirring and dissolving to obtain a chitosan solution, wherein the mass ratio of acetic acid to chitosan in the chitosan solution is 0.8:1, and the mass fraction of chitosan in the chitosan solution is 3%; dispersing modified polyvinyl alcohol in deionized water to obtain a modified polyvinyl alcohol solution with a mass fraction of 3%;
[0036] (2) mixing a carbon nanotube dispersion, a nano-silica dispersion, and a POSS dispersion, and stirring at room temperature for 4 hours to obtain a mixed solution 1; mixing a chitosan solution and a modified polyvinyl alcohol solution, and stirring at 65° C. for 7 hours to obtain a mixed solution 2; mixing the mixed solution 1 with the mixed solution 2, and continuing to stir at 60° C. for 4 hours, pouring into a mold to form a cast film, and drying to obtain a hybrid film;
[0037] (3) The hybrid membrane obtained in step (2) is immersed in a sodium hydroxide aqueous solution (the mass fraction of the sodium hydroxide aqueous solution is 25%) for 1 hour, washed with deionized water after being taken out, and vacuum dried at 60° C. for 6 hours, and then immersed in 1-butyl-3-methylimidazole bistrifluoromethanesulfonyl imide ionic liquid for 12 hours, washed with deionized water after being taken out, and vacuum dried at 60° C. for 12 hours to obtain a proton exchange membrane with a membrane thickness of 65 μm.
[0038] Example 3
[0039] A proton exchange membrane for a fuel cell based on a metal bipolar plate comprises the following raw materials in parts by weight: 1 part of carbon nanotubes, 8 parts of nano-silicon dioxide, 5 parts of glycidyl ether oxypropyl cage-like polysilsesquioxane (POSS), 180 parts of chitosan, and 60 parts of modified polyvinyl alcohol; the difference from Example 2 is that the parts by weight of the modified polyvinyl alcohol are changed.
[0040] Example 4
[0041] A proton exchange membrane for a fuel cell based on a metal bipolar plate comprises the following raw materials in parts by weight: 1 part of carbon nanotubes, 8 parts of nano-silicon dioxide, 5 parts of glycidyloxypropyl caged polysilsesquioxane (POSS), 180 parts of chitosan, and 120 parts of modified polyvinyl alcohol; the difference from Example 2 is that the parts by weight of the modified polyvinyl alcohol are changed.
[0042] Comparative Example 1
[0043] A proton exchange membrane for a fuel cell based on a metal bipolar plate comprises the following raw materials in parts by weight: 1 part of carbon nanotubes, 8 parts of nano-silicon dioxide, 5 parts of glycidyl ether oxypropyl cage-shaped polysilsesquioxane-POSS, 180 parts of chitosan, and 90 parts of polyvinyl alcohol.
[0044] The proton exchange membranes for fuel cells based on metal bipolar plates described in Examples 3-4 and Comparative Example 1 were prepared according to the method described in Example 2.
[0045] Comparative Example 2
[0046] A proton exchange membrane for a fuel cell based on a metal bipolar plate comprises the following raw materials in parts by weight: 1 part of carbon nanotubes, 8 parts of nano-silica, 5 parts of glycidyloxypropyl caged polysilsesquioxane (POSS), 180 parts of chitosan, 90 parts of polyvinyl alcohol, and 8 parts of 2-pyridine-3-yl-3H-benzimidazole-5-carboxylic acid; the difference from Example 2 is that the modified polyvinyl alcohol is replaced by a blend of polyvinyl alcohol and 2-pyridine-3-yl-3H-benzimidazole-5-carboxylic acid.
[0047] A method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate comprises the following steps:
[0048] (1) dispersing carbon nanotubes in deionized water to obtain a carbon nanotube dispersion with a mass fraction of 1%; dispersing nanosilica in deionized water to obtain a nanosilica dispersion with a mass fraction of 2%; dispersing glycidyloxypropyl caged polysilsesquioxane-POSS in ethanol to obtain a POSS dispersion with a mass fraction of 1.5%; dispersing acetic acid in deionized water, mixing evenly, and then adding chitosan, stirring and dissolving to obtain a chitosan solution, wherein the mass ratio of acetic acid to chitosan in the chitosan solution is 0.8:1, and the mass fraction of chitosan in the chitosan solution is 3%; dispersing polyvinyl alcohol and 2-pyridin-3-yl-3H-benzimidazole-5-carboxylic acid in deionized water to obtain a polyvinyl alcohol solution, wherein the mass fraction of polyvinyl alcohol in the polyvinyl alcohol solution is 3%;
[0049] (2) mixing a carbon nanotube dispersion, a nano-silica dispersion, and a POSS dispersion, and stirring at room temperature for 4 hours to obtain a mixed solution 1; mixing a chitosan solution and a polyvinyl alcohol solution, and stirring at 65° C. for 7 hours to obtain a mixed solution 2; mixing the mixed solution 1 with the mixed solution 2, and continuing to stir at 60° C. for 4 hours, pouring into a mold to form a cast film, and drying to obtain a hybrid film;
[0050] (3) The hybrid membrane obtained in step (2) is immersed in a sodium hydroxide aqueous solution (the mass fraction of the sodium hydroxide aqueous solution is 25%) for 1 hour, washed with deionized water after being taken out, and vacuum dried at 60° C. for 6 hours, and then immersed in 1-butyl-3-methylimidazole bistrifluoromethanesulfonyl imide ionic liquid for 12 hours, washed with deionized water after being taken out, and vacuum dried at 60° C. for 12 hours to obtain a proton exchange membrane with a membrane thickness of 65 μm.
[0051] The following are related performance tests of the proton exchange membranes prepared in Examples 2-4 and Comparative Examples 1-2. The tensile performance test was carried out in accordance with GB / T1040-2006 "Test Method for Tensile Performance of Plastics", and the mechanical performance test was carried out by a universal mechanical testing machine, and the test conditions were: the tensile speed was 5 mm / min, the test temperature was 25°C, and each group of tests was repeated 3 times, and the average value was taken; the proton conductivity test was carried out in accordance with GB / T20042.3-2009 "Proton Exchange Membrane Fuel Cell Part 3: Test Method for Proton Exchange Membrane", and the test conditions were: temperature 60°C, 80°C, 100°C, humidity 70%, and each group of tests was repeated 3 times, and the average value was taken; the water absorption rate and swelling rate test were carried out in accordance with GB / T20042.3-2009 "Proton Exchange Membrane Fuel Cell Part 3: Test Method for Proton Exchange Membrane", and the test temperature was 80°C, and each group of tests was repeated 3 times, and the average value was taken; the chemical stability test was carried out by exposing the sample to Fenton reagent (containing 8ppm Fe at 70°C) 2+ The samples were soaked in a 30wt% hydrogen peroxide solution for 12 hours, taken out for cleaning, dried, weighed and calculated for weight retention, weight retention = (membrane weight after soaking - membrane weight before soaking) / membrane weight before soaking × 100%, each test was repeated 3 times, and the average value was taken; the test results are shown in Table 1. It can be seen from the table that the tensile strength, elongation at break and weight retention of the proton exchange membrane prepared in Example 2-4 are significantly better than those in Comparative Example 2; at 60°C, 80°C and 100°C, the proton conductivity of the proton exchange membrane prepared in Example 2-4 is significantly higher than that of Comparative Example 1-2; compared with Comparative Example 1-2, the proton exchange membrane prepared in Example 2-4 greatly reduces the linear swelling rate of the membrane material while the water absorption rate is basically not affected, so that the membrane material has both high water absorption rate and low swelling rate. The invention compounds modified polyvinyl alcohol with carbon nanotubes, nano-silica, glycidyloxypropyl caged polysilsesquioxane-POSS, chitosan, ionic liquid and other raw materials to obtain a proton exchange membrane having excellent mechanical properties, proton conductivity and chemical stability, and at the same time, the membrane material also has the characteristics of high water absorption and low swelling rate.
[0052] Table 1 Proton exchange membrane related performance test results
[0053]
[0054] Although the embodiments of the present application have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present application, and that the scope of the present application is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate, characterized in that: The following steps are involved: (1) dispersing carbon nanotubes in deionized water to obtain a carbon nanotube dispersion; dispersing nanosilica in deionized water to obtain a nanosilica dispersion; dispersing glycidyloxypropyl caged polysilsesquioxane in ethanol to obtain a POSS dispersion; dispersing acetic acid in deionized water, mixing well, and then adding chitosan, stirring and dissolving to obtain a chitosan solution; dispersing the modified polyvinyl alcohol in deionized water to obtain a modified polyvinyl alcohol solution; (2) Mix the carbon nanotube dispersion, nano-silica dispersion and glycidyl ether oxypropyl caged polysilsesquioxane dispersion, and stir at room temperature for 3-7 hours to obtain a mixed solution 1; mix the chitosan solution and the modified polyvinyl alcohol solution, and stir at 55-70°C for 5-10 hours to obtain a mixed solution 2; mix the mixed solution 1 with the mixed solution 2, continue stirring at 55-65°C for 2-5 hours, pour into a mold to cast a film, and obtain a hybrid film after drying; (3) Soaking the hybrid membrane obtained in step (2) in an alkaline solution for 0.5-1.5 hours, taking it out, cleaning it, and drying it, and then soaking it in an ionic liquid for 10-15 hours, taking it out, cleaning it, and drying it, thereby obtaining the hybrid membrane; The mass fraction of the carbon nanotube dispersion in step (1) is 2-7%, the mass fraction of the nano-silica dispersion is 1-6%, the mass fraction of the glycidyloxypropyl caged polysilsesquioxane dispersion is 0.2-2%, the mass ratio of acetic acid to chitosan in the chitosan solution is 0.7-1.4:1, the mass fraction of chitosan in the chitosan solution is 1-4%, and the mass fraction of the modified polyvinyl alcohol solution is 1-4%; The preparation method of the modified polyvinyl alcohol in step (1) is as follows: S1. Disperse epoxybutyltrimethoxysilane in 2-methyltetrahydrofuran, add 2-pyridin-3-yl-3H-benzimidazole-5-carboxylic acid and chromium acetate in sequence, raise the temperature to 75-85°C, stir and react for 6-10 hours, filter, take the filtrate, distill under reduced pressure, and dry to obtain intermediate 1. The structural formula of intermediate 1 is: ; S2. Disperse the intermediate 1 obtained in step S1 in 2-methyltetrahydrofuran, add 4-bromobutyric acid, potassium hydroxide, and benzyltriethylammonium chloride in sequence, raise the temperature to 55-70° C., stir and react for 4-7 hours, cool to room temperature, adjust the pH to 6-7, filter, take the filtrate, distill under reduced pressure, and dry to obtain intermediate 2. The structural formula of intermediate 2 is: ; S3, dispersing polyvinyl alcohol in dimethyl sulfoxide, heating to 85-100°C, stirring for 1-2h, cooling to 75-90°C, sequentially adding intermediate 2 obtained in step S2 and p-toluenesulfonic acid, continuing stirring for 5-9h, cooling to room temperature, solid-liquid separation, taking solid, washing and drying, and obtaining modified polyvinyl alcohol. The structural formula of the modified polyvinyl alcohol is: 。 2. The method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate according to claim 1, characterized in that: The molar ratio of epoxybutyltrimethoxysilane, 2-pyridin-3-yl-3H-benzimidazole-5-carboxylic acid and chromium acetate in step S1 is 1.1-1.2:1:0.013-0.
020.
3. The method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate according to claim 2, characterized in that: The amount of epoxybutyltrimethoxysilane added to the 2-methyltetrahydrofuran is 0.12-0.26 g / mL.
4. The method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate according to claim 1, characterized in that: The molar ratio of the intermediate 1, 4-bromobutyric acid, potassium hydroxide and benzyltriethylammonium chloride in step S2 is 1:0.8-1.0:0.7-1.2:0.04-0.
08.
5. The method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate according to claim 4, characterized in that: The amount of the intermediate 1 added to the 2-methyltetrahydrofuran is 0.1-0.3 g / mL.
6. The method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate according to claim 1, characterized in that: The mass ratio of polyvinyl alcohol, intermediate 2 and p-toluenesulfonic acid in step S3 is 10:0.8-1.5:0.1-0.
2.
7. The method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate according to claim 6, characterized in that: The amount of polyvinyl alcohol added to the dimethyl sulfoxide is 0.08-0.16 g / mL.
8. The method for preparing a proton exchange membrane for a fuel cell based on a metal bipolar plate according to claim 1, characterized in that: The alkali solution in step (3) is a sodium hydroxide or potassium hydroxide aqueous solution, the mass fraction of the alkali solution is 20-40%, and the ionic liquid is 1-butyl-3-methylimidazole bistrifluoromethanesulfonimide.
9. A proton exchange membrane for a fuel cell based on a metal bipolar plate, characterized in that: The proton exchange membrane for fuel cells is a proton exchange membrane for fuel cells prepared by the method for preparing a proton exchange membrane for fuel cells based on a metal bipolar plate according to any one of claims 1 to 8.
Citation Information
Patent Citations
Cross-linking type proton exchange membrane for vanadium battery and preparation method
CN109411796A
Proton exchange membrane, preparation method thereof and environment-friendly fuel cell
CN113178603A
Crosslinked anion exchange membrane based on polyphenyl ether / polyvinyl alcohol and preparation method
CN111269550A
Preparation method of proton exchange membrane and fuel cell
CN113178604A
Modified polyvinyl alcohol, method for producing the same, electron device using the same and electrophotographic photoreceptor
JP2001106722A