Glaze for obtaining low-roughness glaze effect and preparation method of light-colored ceramic rock plate
By adding fluorescent screen glass slag and melted material powder to the ceramic glaze formula, and adopting specific firing and processing technology, the problem of difficult to reduce the roughness of the ceramic glaze surface is solved, and ceramic rock with low roughness and stable texture is achieved The plate preparation avoids the occurrence of glaze defects.
Patent Information
- Application Number
- CN202311431033.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2043-10-31
AI Technical Summary
Existing ceramic glaze products are difficult to break through 1.20μm when reducing roughness, resulting in the surface texture being not delicate enough and prone to defects such as pinholes, making it difficult to achieve the unity of low roughness and stable texture.
Add the fluorescent screen glass slag produced by color TV imaging tubes and melted material powder to the glaze formula, and control the glaze roughness to 0.5~1.5μm through specific firing and processing steps, and use batch ball milling and inkjet printing. Process to ensure the fineness and flatness of the glaze surface.
The glaze surface roughness is achieved at a low roughness effect of 0.5 to 1.5μm, the feel is smooth and round, close to the fluff effect, and the production is stable and controllable, avoiding defects such as bubble pinholes, and having good flatness and tone stability.
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of building ceramics, and in particular relates to a glaze for obtaining a low-roughness glaze effect and a method for preparing a light-colored ceramic rock slab. Background Art
[0002] With the continuous development of the building ceramics industry, the texture of ceramic glaze has become diversified. In the terminal market where market competition is extremely fierce, in order to show differentiated product characteristics, different manufacturers usually promote ceramic glazed tiles with a certain type of products with similar texture to gain market recognition, such as the "delicate glaze", "velvet", "skin glaze" and other products popular in the current building ceramics market. Since the products are usually expressed in analogical or descriptive language, different people have different senses and it is difficult to unify the qualitative description, which has caused chaos in the market. In the field of technology, it is also difficult to express the glaze texture in an objective way when developing glazes, and the subjective expression of products brings difficulties in stable control to technology research and development and production.
[0003] CN116023171A discloses a ceramic plate with a skin-friendly texture, a preparation method and an application thereof. The technical solution is: made of a body layer and a skin glaze layer arranged on the surface of the body layer, the skin glaze layer includes a base glaze layer, a surface glaze layer and a transparent protective glaze layer arranged in sequence away from the body layer; the surface gloss of the ceramic plate is 16 to 25°, and the surface roughness Ra of the ceramic plate is 10 to 15 μm. The invention adopts a design in which multiple glaze layers cooperate with each other to achieve a matte effect of 16 to 25° on the surface of the ceramic plate, with a soft and comfortable visual effect, and at the same time achieves a surface roughness of Ra = 10 to 15 μm. The surface is as delicate and smooth as baby skin, and has an ergonomic skin-friendly texture. However, in fact, when the roughness Ra = 10 to 15 μm, the surface roughness is relatively strong and cannot achieve the described "surface as delicate and smooth as baby skin". According to the surface roughness detection of glazes with different formulas and different textures, when Ra﹤2.0μm, the glaze texture is relatively delicate and smooth, that is to say, the lower the surface roughness of the product, the more delicate and smooth it is. However, according to the formula structure of the matte delicate glaze, while reducing the glaze roughness, it is easy to have glaze defects such as surface pinholes. According to information collected, the roughness Ra of most glazed products in the current building ceramics industry is difficult to break through below 1.20μm. Summary of the invention
[0004] In view of the problems existing in the above-mentioned prior art, the technical problem solved by the present invention is to provide a method for adding fluorescent screen glass slag and molten material powder formed by the production of color TV picture tubes into the formula, so that the glaze has a smooth and fine texture and good flatness after firing. The glaze surface roughness Ra of the product after firing is 0.5-1.5μm, with a low-roughness glaze effect and stable color, and is suitable for glazes with a wide firing range. Another technical problem solved by the present invention is to provide a glaze for obtaining a low-roughness glaze effect, the product glaze surface roughness Ra is 0.50-1.50μm, the glaze surface feels smooth and round, the texture is close to the fluff effect, the production is stable and controllable, and there is no defects such as bubbles and pinholes. The light-colored ceramic rock plate preparation method.
[0005] The technical solution of the present invention is the glaze for obtaining a low-roughness glaze effect, and its special feature is that the glaze is composed of the following components by weight: 10 to 22 parts of fluorescent screen glass slag, 1 to 5 parts of wollastonite, 15 to 25 parts of potassium feldspar, 5 to 10 parts of kaolin, 0 to 2 parts of celestite, and 40 to 50 parts of molten material powder.
[0006] Preferably, the glaze for obtaining the low-roughness glaze effect is composed of the following components by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of lapis lazuli, and 46 parts of molten material powder.
[0007] Preferably, the fluorescent screen glass slag is the recycled waste slag of fluorescent screen glass produced in the production of color television picture tubes, and its chemical composition consists of the following components by weight: 53.02 parts of SiO2, 17.62 parts of Al2O3, 0.14 parts of Fe2O3, 0.05 parts of TiO2, 7.6 parts of CaO, 4.46 parts of MgO, 3.3 parts of K2O, 4.48 parts of Na2O, 0.08 parts of PbO, 3.6 parts of BaO, and 5.65 parts of SrO.
[0008] As a preferred option: in order to make the glaze obtain the set quality transparency and stable color, the selected fluorescent screen glass slag should not have too heavy color cast. The a* value range of -2.5 to +2 and the b* value range of -2 to +1.5 detected by a colorimeter are qualified materials in terms of color tone. When introduced into the formula, the fineness of the fluorescent screen glass slag is controlled at 200 to 300 mesh, which is beneficial to the glaze processing and at the same time increases the degree of participation of the fluorescent screen glass slag in the reaction in the formula.
[0009] Preferably, the molten material powder is composed of the following components by weight:
[0010] 5 parts of zinc oxide ore, 2 parts of barium carbonate, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin, and 10 parts of coal gangue;
[0011] Its chemical composition is composed of the following components by weight:
[0012] SiO2 51.73 parts, Al2O3 17.34 parts, CaO 7.89 parts, MgO 4.05 parts, K2O1.22 parts, Na2O 4.43 parts, B2O3 0.31 parts, ZnO 6.08 parts, BaO 1.98 parts, SrO 4.97 parts;
[0013] As a preferred method: Preparation of molten material powder:
[0014] ⑴ Weigh the raw materials according to the formula of the melting material powder.
[0015] ⑵Mix evenly,
[0016] ⑶ Use a rotary kiln to calcine and melt the materials, the calcination temperature is 1200-1300℃, the calcination time is 30min,
[0017] ⑷ Cooling,
[0018] (5) Use a double-roll crusher to crush the material. The particle size range after crushing is: all pass through a 40-mesh sieve to obtain molten material powder;
[0019] Furthermore, in step (1), the materials for the melting material powder formula are introduced in the form of dry materials with a fineness of 150 to 250 mesh.
[0020] Another technical solution of the present invention is the method for preparing a glaze for obtaining a low-roughness glaze effect, which is special in that it includes the following steps: weighing materials according to the glaze formula for obtaining a low-roughness glaze effect, adding 0.3 parts of sodium carboxymethyl cellulose and 0.5 parts of sodium tripolyphosphate and 40 parts of water, and ball milling by intermittent ball milling, ball milling until the glaze fineness is 0.4-0.8% on a 325-mesh sieve, the glaze particle grading distribution span is span﹤3, the Eng viscosity is 40-50s, the specific gravity is 1.82-1.85, and slurrying is performed to obtain a glaze for obtaining a low-roughness glaze effect.
[0021] Another technical solution of the present invention is a method for preparing a light-colored ceramic rock plate using a glaze for obtaining a low-roughness glaze effect, which is special in that it includes the following steps:
[0022] ⑴ Body pressing: After the body is pressed and dried, the difference in oil absorption rate at different positions of the body is less than 1.8%. In order to meet the requirement of low roughness effect of the product glaze, the pressed body is bisque fired. It is required that there are no fine particles on the surface of the body, the roughness of the surface Ra is less than 5μm, and the optimal range of the roughness of the surface after firing is 1.5μm<Ra<3μm; the low roughness surface provides a good foundation for the flatness of the glaze surface later;
[0023] ⑵Body drying: Maximum drying temperature: 170-180℃, drying time: 20min;
[0024] ⑶ Base glaze: The glossiness of single base glaze after firing is in the range of 4 to 9°, and the best roughness range of base glaze on the body is 1.0μm<Ra<2.5μm;
[0025] The chemical composition of the base glaze is composed of the following components by weight:
[0026] SiO2 56.28 parts, Al2O3 19.84 parts, Fe2O3 0.73 parts, CaO 3.36 parts, MgO 1.17 parts, K2O 1.88 parts, Na2O 5.15 parts, B2O3 0.13 parts, ZnO 1.39 parts, TiO2 0.09 parts, BaO 4.67 parts, ZrO 1.03 parts;
[0027] ⑷Inkjet printing: light color, total grayscale of ink <100;
[0028] ⑸ Glaze with low roughness: Use bell jar glaze to get low roughness glaze, the glaze amount is 500g / m 2 ;
[0029] (6) Firing: The maximum firing temperature is 1180℃, the high temperature holding time is 5-8min, and the firing cycle is 68min. After firing, the glaze gloss is 13-25°, the surface roughness Ra is 0.50-1.50μm, and the glaze of the product feels smooth and round, with a texture close to the fluff effect.
[0030] ⑺ Brush polishing: Use a 320-mesh abrasive brush to brush the glaze surface with a brush pressure of 1 to 2 kg. Brush polishing does not change the state of the glaze surface, but can remove kiln dirt or fallen dirt, further improving the surface flatness of the low-roughness glaze surface.
[0031] Preferably, step (1) further comprises: since the green body is pressed from powder, in order to avoid obvious granularity on the green body surface, a press back-beating method is adopted to improve the fineness of the green body surface; at the same time, after the green body is pressed, a green body surface is pre-treated by a polishing machine, and a 300-mesh sponge brush grinding block is used to polish the green body surface to improve the flatness of the green body surface.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] (1) The present invention discloses a glaze formula for obtaining a low-roughness glaze effect. By adding fluorescent screen glass slag formed in the production of color television picture tubes into the formula, a large amount of strontium-containing silicate components are introduced, which is beneficial to reducing the viscosity of the glaze and making the glaze smoother and finer after firing. At the same time, the fluorescent screen glass slag is melted at a high temperature of 1500-1700°C, and the carbonates and sulfates in the raw materials have been fully decomposed, with less impurities, forming a unified molten body. The use of this raw material in the glaze formula can enable the glaze to maintain the advantages of the fluorescent screen glass, such as good radiation protection performance, light weight, clear image and small deformation.
[0034] (2) The present invention provides a glaze formula for obtaining a low-roughness glaze effect. The molten material powder in the formula is calcined at 1200-1300° C. in a rotary kiln to eliminate moisture and carbon volatiles in the raw materials, thereby reducing excessive volatiles during the firing process of the glaze for obtaining a low-roughness glaze effect and avoiding defects such as bubbles and pinholes. DETAILED DESCRIPTION
[0035] The present invention will be further described in detail below in conjunction with embodiments:
[0036] The glaze for obtaining a low-roughness glaze effect consists of the following components in parts by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestine, and 46 parts of molten material powder; the fluorescent screen glass slag is waste slag recycled from fluorescent screen glass used in the production of color television picture tubes, and its chemical composition consists of the following components in parts by weight: 53.02 parts of SiO2, 17.62 parts of Al2O3, 0.14 parts of Fe2O3, 0.05 parts of TiO2, 7.6 parts of CaO, 4.46 parts of MgO, 3.3 parts of K2O, 4.48 parts of Na2O, 0.08 parts of PbO, 3.6 parts of BaO, and 5.65 parts of SrO.
[0037] In order to ensure that the glaze has the set quality transparency and stable color, the selected fluorescent screen glass slag should not have too heavy color cast. The colorimeter is used to detect the a* value range of -2.5 to +2, and the b* value range of -2 to +1.5 is the qualified color tone material. When introduced into the formula, the fineness of the fluorescent screen glass slag is controlled at 200 to 300 mesh, which is conducive to glaze processing and at the same time increases the degree of participation of the fluorescent screen glass slag in the reaction in the formula.
[0038] The molten material powder consists of the following components by weight:
[0039] 5 parts of zinc oxide ore, 2 parts of barium carbonate, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin, and 10 parts of coal gangue;
[0040] Its chemical composition is composed of the following components by weight:
[0041] SiO2 51.73 parts, Al2O3 17.34 parts, CaO 7.89 parts, MgO 4.05 parts, K2O 1.22 parts, Na2O 4.43 parts, B2O3 0.31 parts, ZnO 6.08 parts, BaO 1.98 parts, SrO 4.97 parts
[0042] Preparation of molten material powder: weigh the raw materials according to the formula of molten material powder, mix them evenly, and then use a rotary kiln to calcine and melt the materials. The calcination temperature is 1200-1300°C and the calcination time is 30 minutes. After cooling, use a double-roll crusher to crush the materials. The particle size range after crushing is: all pass through a 40-mesh sieve to obtain molten material powder; wherein the materials of the molten material powder formula are introduced in the form of dry materials with a fineness of 150-250 meshes.
[0043] The method for preparing a glaze for obtaining a low-roughness glaze effect comprises the following steps: weighing materials according to a glaze formula for obtaining a low-roughness glaze effect, adding 0.3 parts of sodium carboxymethyl cellulose and 0.5 parts of sodium tripolyphosphate and 40 parts of water, and ball milling by an intermittent ball milling method until the glaze fineness is 0.4-0.8% of the residue on a 325-mesh sieve, the glaze particle grading distribution span is less than 3, the Eng viscosity is 40-50s, the specific gravity is 1.82-1.85, and slurrying is performed to obtain a glaze for obtaining a low-roughness glaze effect.
[0044] A method for preparing a light-colored ceramic rock plate using a glaze for obtaining a low-roughness glaze effect comprises the following steps:
[0045] ⑴ Body pressing: adopt the method of reverse pressing by the press. After the body is pressed, the body surface is pre-treated by a polishing machine, and the body surface is polished by a 300-mesh sponge brush grinding block. There are no fine particles on the body surface. After the body is pressed and formed and dried, the difference in oil absorption rate at different positions of the body is less than 1.6%. The pressed body is bisque fired, and the roughness range of the body surface after firing is 1.6μm<Ra<2.5μm; providing a good foundation for the flatness of the glaze surface later;
[0046] ⑵Body drying: Maximum drying temperature: 170-180℃, drying time: 20min;
[0047] ⑶ Base glaze: The glossiness of single base glaze after firing is in the range of 4 to 9°, and the best roughness range of base glaze on the body is 1.0μm<Ra<2.5μm;
[0048] The chemical composition of the base glaze is composed of the following components by weight:
[0049] SiO2 56.28 parts, Al2O3 19.84 parts, Fe2O3 0.73 parts, CaO 3.36 parts, MgO 1.17 parts, K2O 1.88 parts, Na2O 5.15 parts, B2O3 0.13 parts, ZnO 1.39 parts, TiO2 0.09 parts, BaO 4.67 parts, ZrO 1.03 parts;
[0050] ⑷Inkjet printing: light color, total grayscale of ink <100;
[0051] ⑸ Glaze with low roughness: Use bell jar glaze to get low roughness glaze, the glaze amount is 500g / m 2 ;
[0052] (6) Firing: The maximum firing temperature is 1180℃, the high temperature holding time is 7min, and the firing cycle is 68min. After firing, the glaze gloss is 15-18°, the surface roughness Ra is 0.75-1.25μm, and the glaze feels smooth and round, with a texture close to the fluff effect.
[0053] ⑺ Brush polishing: Use a 320-mesh abrasive brush to brush the glaze surface with a brush pressure of 1kg. Brush polishing does not change the state of the glaze surface, but can remove kiln dirt or fallen dirt, and further improve the surface flatness of the low-roughness glaze surface.
[0054] The above description is only a preferred embodiment of the present invention. All equivalent changes and modifications made within the scope of the claims of the present invention should fall within the scope of the claims of the present invention.
Claims
1. A glaze for obtaining a low-roughness glaze effect, characterized in that: The glaze is composed of the following components by weight: 10-22 parts of fluorescent screen glass slag, 1-5 parts of wollastonite, 15-25 parts of potassium feldspar, 5-10 parts of kaolin, 0-2 parts of celestite, and 40-50 parts of molten material powder; The fluorescent screen glass slag is the fluorescent screen glass recycled waste slag produced in the production of color television picture tubes, and its chemical composition is composed of the following components by weight: 53.02 parts of SiO2, 17.62 parts of Al2O3, 0.14 parts of Fe2O3, 0.05 parts of TiO2, 7.6 parts of CaO, 4.46 parts of MgO, 3.3 parts of K2O, 4.48 parts of Na2O, 0.08 parts of PbO, 3.6 parts of BaO, and 5.65 parts of SrO; The chemical composition of the molten material powder is composed of the following components by weight: SiO2 51.73 parts, Al2O3 17.34 parts, CaO 7.89 parts, MgO 4.05 parts, K2O 1.22 parts, Na2O 4.43 parts, B2O3 0.31 parts, ZnO 6.08 parts, BaO 1.98 parts, SrO 4.97 parts.
2. The glaze for obtaining a low-roughness glaze effect according to claim 1, characterized in that: The glaze is further composed of the following components by weight: 20 parts of fluorescent screen glass slag, 5 parts of wollastonite, 20 parts of potassium feldspar, 8 parts of kaolin, 2 parts of celestite, and 46 parts of molten material powder.
3. The glaze for obtaining a low-roughness glaze effect according to claim 1, characterized in that: In order to ensure that the glaze has the set quality transparency and stable color, the selected fluorescent screen glass slag should not have too heavy color cast. The colorimeter is used to detect the a* value range of -2.5 to +2, and the b* value range of -2 to +1.5 is the qualified color tone material. When introduced into the formula, the fineness of the fluorescent screen glass slag is controlled at 200 to 300 mesh, which is conducive to glaze processing and at the same time increases the degree of participation of the fluorescent screen glass slag in the reaction in the formula.
4. The glaze for obtaining a low-roughness glaze effect according to claim 1, characterized in that: The molten material powder consists of the following components by weight: 5 parts of zinc oxide ore, 2 parts of barium carbonate, 12 parts of potassium feldspar, 36 parts of sodium feldspar, 15 parts of dolomite, 3 parts of ultrafine quartz, 11 parts of kaolin, and 10 parts of coal gangue.
5. The glaze for obtaining a low-roughness glaze effect according to claim 4, characterized in that: The preparation of the molten material powder comprises the following steps: ⑴Weigh the raw materials according to the formula of the melting material powder; ⑵Mix evenly; ⑶ Use a rotary kiln to calcine and melt the materials, the calcination temperature is 1200-1300℃, and the calcination time is 30min; (4) Cooling; ⑸ Use a double-roll crusher to crush, and the particle size range after crushing is: all pass through a 40-mesh sieve to obtain molten material powder; Furthermore, the molten material powder formula materials in step (1) are introduced in the form of dry materials with a fineness of 150 to 250 mesh.
6. A method for preparing a glaze for obtaining a low-roughness glaze effect according to claim 1, characterized in that: The following steps are involved: Weigh the materials according to the glaze formula for obtaining a low-roughness glaze effect, add 0.3 parts of sodium carboxymethyl cellulose, 0.5 parts of sodium tripolyphosphate and 40 parts of water, and use intermittent ball milling to perform ball milling until the glaze fineness is 0.4-0.8% on a 325-mesh sieve, the glaze particle grading distribution span is span﹤3, the Eng viscosity is 40-50s, the specific gravity is 1.82-1.85, and then slurry is released to obtain a glaze for obtaining a low-roughness glaze effect.
7. A method for preparing a light-colored ceramic rock plate using the glaze for obtaining a low-roughness glaze effect as claimed in claim 1, characterized in that: The following steps are involved: ⑴ Body pressing: After the body is pressed and dried, the difference in oil absorption rate at different positions of the body is less than 1.8%. In order to meet the requirement of low roughness effect of the product glaze, the pressed body is bisque fired. It is required that there are no fine particles on the body surface, the roughness of the body surface Ra is less than 5μm, and the roughness range of the body surface after firing is: 1.5μm<Ra<3μm; the low roughness body surface provides a good foundation for the flatness of the subsequent glaze surface; (2) Drying of green body: Maximum drying temperature is 170-180℃, and the drying time is 20min; ⑶ Base glaze: The glossiness of single base glaze after firing is in the range of 4 to 9 degrees, and the roughness of base glaze on the body is in the range of 1.0μm<Ra<2.5μm; ⑷Inkjet printing: light color, total grayscale of ink <100; ⑸ Glaze with low roughness: Use bell jar glaze to get low roughness glaze, the glaze amount is 500g / m 2 ; (6) Firing: The maximum firing temperature is 1180℃, the high temperature holding time is 5-8min, and the firing cycle is 68min. After firing, the glaze gloss of the product is 13-25°, the surface roughness Ra is 0.50-1.50μm, and the glaze of the product feels smooth and round, with a texture close to the fluff effect. ⑺ Brush polishing: Use a 320-mesh abrasive brush to brush the glaze surface with a brush pressure of 1 to 2 kg. Brush polishing does not change the state of the glaze surface, but removes kiln dirt or fallen dirt to further improve the surface flatness of the low-roughness glaze surface.
8. The method for preparing a light-colored ceramic rock plate using a glaze for obtaining a low-roughness glaze effect according to claim 7, characterized in that: The step (1) further includes: since the green body is pressed from powder, in order to avoid obvious granularity on the green body surface, a press back-beating method is used to improve the fineness of the green body surface. At the same time, after the green body is pressed, a green body surface is pre-treated by a polishing machine, and a 300-mesh sponge brush grinding block is used to polish the green body surface to improve the flatness of the green body surface.
9. The method for preparing a light-colored ceramic rock plate using a glaze for obtaining a low-roughness glaze effect according to claim 7, characterized in that: The step (3) further comprises: the base glaze chemical composition is composed of the following components by weight: SiO2 56.28 parts, Al2O3 19.84 parts, Fe2O3 0.73 parts, CaO 3.36 parts, MgO 1.17 parts, K2O 1.88 parts, Na2O 5.15 parts, B2O3 0.13 parts, ZnO 1.39 parts, TiO2 0.09 parts, BaO 4.67 parts, ZrO 1.03 parts.
Citation Information
Patent Citations
Ceramic plate with skin-friendly texture as well as preparation method and application of ceramic plate
CN116023171A
Domestic ceramic product not easy to smudge and preparation method thereof
CN111410424A
Gray black polished thin rock plate prepared from double-peak grading glaze and glaze preparation method
CN114956871A
Preparation method of ultra-smooth ceramic glaze
CN115893844A