A method for preparing the back structure of an N-type SE-TOPCon battery by PECVD

By setting the auxiliary heat switch on in the vacuum step and adjusting the deposition parameters of the phosphorus-doped amorphous silicon layer in the PECVD method, the problems of high marking ratio of graphite boats and uneven oxide layer are solved, and the N-type SE-TOPCon is improved The preparation efficiency and yield of the back structure of the battery reduce costs.

CN117626232BActive Publication Date: 2024-11-05合肥大恒智慧能源科技有限公司
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202311613582.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-11-05
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

When preparing the back structure of the N-type SE-TOPCon battery, the PECVD method has problems such as high graphite boat dot printing ratio, low product yield, and uneven oxide layer thickness, resulting in high cost and low efficiency.

Method used

By setting the auxiliary heat switch on in the PECVD deposition furnace in the vacuum step and adjusting the three-step deposition parameters of the phosphorus-doped amorphous silicon layer, the fit of the silicon wafer heating process and the uniformity of the oxide layer are improved, and the uniformity of the oxide layer is reduced. Phosphorus expansion and dark film generation improve production line efficiency.

Benefits of technology

The thickness and uniformity of the oxide layer in which the graphite boat and the silicon wafer are contacted is improved, the cost of the product and the generation of dark sheets is reduced, and the yield and efficiency of the product are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117626232B_ABST
    Figure CN117626232B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a back structure of an N-type SE-TOPCon battery by a PECVD method, comprising the following steps: putting in a boat: inserting a silicon wafer that has been cleaned and textured, first subjected to boron diffusion to prepare PN and SE, then subjected to boron oxidation, and subjected to alkali polishing into a graphite boat, and sending the wafer to a PECVD deposition furnace; heating: closing a furnace door of the PECVD deposition furnace, and raising the temperature in the furnace to a set temperature by heating and temperature control; evacuating: evacuating the PECVD deposition furnace, and simultaneously turning on auxiliary heat at the bottom and top of the furnace tube; leak detection: detecting gas leakage; pre-ventilation-constant pressure: performing pre-ventilation to maintain a constant pressure in the PECVD deposition furnace; tunneling layer deposition: performing pre-ventilation to deposit the same gas at a constant pressure before depositing different film layers. The invention sets the auxiliary heat on at the vacuuming step, and the setting improves the fit between the silicon wafer heating process and the graphite boat, and deposits a thin tunneling layer at a low deposition rate to improve the oxide layer thickness and uniformity at the contact point between the graphite boat and the silicon wafer, thereby improving the EL yield of the product.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of solar cells, and in particular to a method for preparing a back structure of an N-type SE-TOPCon cell using a PECVD method. Background Art

[0002] The tunnel oxide contact (TOPCon) battery technology based on N-type silicon substrate uses a stacked structure of ultra-thin oxide layer and doped polysilicon layer (Poly-Si) for back surface passivation. The tunnel oxide layer structure effectively realizes carrier selectivity by allowing minority carriers to penetrate and majority carriers to be blocked, thereby greatly reducing the recombination rate of minority carriers and thereby improving the conversion efficiency of the battery.

[0003] The core of the TOPCon cell is a very thin oxide layer and phosphorus-doped polysilicon layer on the back. The methods for preparing this structure can be divided into PECVD (plasma enhanced chemical vapor deposition) and LPCVD (low pressure chemical vapor deposition). LPCVD is to deposit a tunneling oxide layer and an amorphous silicon film on the same machine, and then dope the film by ion implantation or phosphorus diffusion to form phosphorus-doped polysilicon (poly-si). The PECVD method is to complete the tunneling oxide layer and the phosphorus-doped amorphous silicon layer on the same machine, and then form polysilicon (poly-si) through high temperature annealing and crystallization.

[0004] At present, LPCVD technology is relatively mature, but the auxiliary material quartz tube used in it has a short life and high consumables cost. The carrier used by PECVD is a graphite boat, which has a lower cost. Based on cost and production capacity considerations, all new lines in the market currently use the PECVD technology route. However, the PECVD route also has many problems: for example, the high proportion of graphite boat point printing leads to low product yield. The tubular PECVD method uses nitrous oxide ionization deposition to prepare the tunneling layer. The activity of nitrous oxide is relatively high. The temperature and the atmosphere of the cavity will affect its uniformity, especially the thickness of the oxide layer at the position where the graphite boat contacts the silicon wafer. At the same time, the overall thickness of the oxide layer will also affect the thickness of the oxide layer at the position where the graphite boat contacts the silicon wafer. Therefore, a method for preparing the back structure of an N-type SE-TOPCon battery by PECVD is needed to solve the above problems. Summary of the invention

[0005] The object of the present invention is to provide a method for preparing a back structure of an N-type SE-TOPCon battery by a PECVD method, so as to solve the problems existing in the prior art mentioned in the above background technology.

[0006] To achieve the above object, the present invention provides the following technical solutions:

[0007] A method for preparing a back structure of an N-type SE-TOPCon battery by a PECVD method comprises the following steps:

[0008] S1: Putting into the boat: inserting the silicon wafer after cleaning and texturing, front boron diffusion to make PN and SE, back boron oxidation, and alkaline polishing into the graphite boat and sending it to the PECVD deposition furnace;

[0009] S2: Heating: Close the door of the PECVD deposition furnace and raise the temperature inside the furnace to the set temperature through heating and temperature control;

[0010] S3: Evacuate: Evacuate the PECVD deposition furnace and turn on the auxiliary heat at the bottom and top of the furnace tube at the same time;

[0011] S4: Leak detection: detect gas leakage;

[0012] S5: Pre-ventilation-constant pressure: Pre-ventilation is performed to maintain a constant pressure in the PECVD deposition furnace;

[0013] S6: Tunneling layer deposition: Before depositing different film layers, pre-deposit the same gas of the layer at a constant pressure, and then evacuate;

[0014] S7: Pre-ventilation-constant pressure: Pre-ventilation is performed again to maintain a constant pressure in the PECVD deposition furnace;

[0015] S8: phosphorus-doped amorphous silicon deposition, after which vacuum treatment and pre-ventilation constant pressure treatment are performed;

[0016] S9: preparing a mask;

[0017] S10: Vacuum and purge, and after back pressure, take the graphite boat out of the deposition furnace to complete the preparation.

[0018] Preferably, the temperature in S2 is set to 400-430 degrees Celsius, and the heating time is set to 300-500 seconds.

[0019] Preferably, the auxiliary heating temperature in S3 is 400-430 degrees Celsius, and the auxiliary heating start time is 450-600s.

[0020] Preferably, in S6, the deposition thickness is 1.5-2.0 nm, the deposition time is 80-115 s, the nitrous oxide flow rate is 8000-11000 sccm, and the RF power is 8500-11000 W.

[0021] Preferably, the specific steps of depositing phosphorus-doped amorphous silicon in S8 are:

[0022] The deposition is divided into three steps. The parameters for the first step are as follows: deposition time of 100-200s, silane flow rate of 2400-3300sccm, hydrogen flow rate of 9200-9900sccm, phosphine flow rate of 250-600sccm, and RF power of 9000-13000W; the parameters for the second step are as follows: deposition time of 50-200s, silane flow rate of 2200-3000sccm, hydrogen flow rate of 8300-9000sccm, phosphine flow rate of 350-550sccm, and RF power of 11000-15000W; the parameters for the third step are as follows: deposition time of 350-550s, silane flow rate of 2000-3000sccm, hydrogen flow rate of 8300-9000sccm, phosphine flow rate of 350-550sccm, and RF power of 12000-15000W.

[0023] Preferably, the total film thickness of the phosphorus-doped amorphous silicon deposition is 95-120 nm.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The present invention sets the auxiliary heat on at the vacuum step, which improves the fit between the silicon wafer and the graphite boat during the heating process, and deposits a thin tunneling layer at a low deposition rate to improve the thickness and uniformity of the oxide layer at the contact point between the graphite boat and the silicon wafer, thereby improving the EL yield of the product.

[0026] 2. The present invention adjusts the thickness of each layer of the three-step deposition of the doped poly-Si layer, reduces phosphorus internal diffusion, reduces the generation of dark films, improves production line efficiency, and thus reduces product costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0027] Figure 1 This is a picture of the product prepared in Comparative Example 1 of the present invention.

[0028] Figure 2 This is a picture of the product prepared in Example 2 of the present invention.

[0029] Figure 3 This is a picture of the product prepared in Example 3 of the present invention. DETAILED DESCRIPTION

[0030] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0031] See also Figure 1-3 , the present invention provides the following technical solutions:

[0032] A method for preparing the back structure of an N-type SE-TOPCon battery by PECVD. The N-type silicon wafer information used in the following embodiments is as follows: the thickness is 130 microns, the resistivity is 0.4-1.6 ohm-cm, and the silicon wafer is processed in the same manner before depositing a tunneling oxide layer / phosphorus-doped amorphous silicon on the back.

[0033] Comparative Example 1

[0034] S1: Putting into the boat: inserting the silicon wafer after cleaning and texturing, front boron diffusion to make PN and SE, back boron oxidation, and alkaline polishing into the graphite boat and sending it to the PECVD deposition furnace;

[0035] S2: Heating: Close the door of the PECVD deposition furnace, and raise the temperature in the furnace to the set temperature through heating temperature control. The set temperature is 420 degrees Celsius, and the heating time is set to 650s. At the same time, turn on the auxiliary heating at the bottom and top of the furnace tube to assist in rapid heating and improve the temperature distribution in the tube so that all parts of the graphite boat are heated evenly. The auxiliary heating temperature is 420 degrees Celsius and the auxiliary heating start time is 600s.

[0036] S3: Evacuate: Evacuate the PECVD deposition furnace for 300 seconds;

[0037] S4: Leak detection: detect gas leakage;

[0038] S5: Pre-ventilation-constant pressure: Pre-ventilation is performed to maintain a constant pressure in the PECVD deposition furnace;

[0039] S6: Tunneling layer deposition: Before depositing different film layers, the same gas of the same layer is pre-deposited at a constant pressure, and then evacuated. The purpose of evacuation is to remove the remaining unreacted or reactant to facilitate the deposition of other films in the next step. The deposition thickness is 2nm, the deposition time is 110s, the laughing gas flow rate is 8500sccm, and the RF power is 11000W;

[0040] S7: Pre-ventilation-constant pressure: Pre-ventilation is performed again to maintain a constant pressure in the PECVD deposition furnace;

[0041] S8: Deposition of phosphorus-doped amorphous silicon. After completion, vacuum treatment and pre-ventilation constant pressure treatment are carried out. The specific steps of phosphorus-doped amorphous silicon deposition are: it is divided into three steps of deposition. The first step parameters are deposition time of 150s, silane flow rate of 2400sccm, hydrogen flow rate of 9500sccm, phosphine flow rate of 250sccm, and RF power of 10000W; the second step parameters are deposition time of 200s, silane flow rate of 2400sccm, hydrogen flow rate of 8300sccm, and phosphine flow rate of The parameters for the third step are deposition time of 350s, silane flow rate of 2400sccm, hydrogen flow rate of 8300sccm, phosphine flow rate of 450sccm, RF power of 12000W, and the total film thickness of phosphorus-doped amorphous silicon deposition is 95nm; the first and second steps are both lightly doped, and the third step is heavily doped, the purpose of which is to reduce the phosphorus content in the deposited layer in contact with the tunneling layer, reduce the internal expansion of phosphorus, and thereby reduce parasitic absorption.

[0042] S9: prepare a mask, prepare an oxide layer mask to protect the poly-si layer in the subsequent cleaning process;

[0043] S10: Vacuum and purge, and after back pressure, take the graphite boat out of the deposition furnace to complete the preparation.

[0044] The preparation method adopts the traditional auxiliary heat setting method, and sets the auxiliary heat on in the temperature rise step of step S2. The program parameter product mass black spots and graphite boat card point printing ratio is 5%, of which mass black spots account for the majority. Figure 1 shown.

[0045] Example 1

[0046] S1: Putting into the boat: inserting the silicon wafer after cleaning and texturing, front boron diffusion to make PN and SE, back boron oxidation, and alkaline polishing into the graphite boat and sending it to the PECVD deposition furnace;

[0047] S2: Heating: Close the door of the PECVD deposition furnace, and raise the temperature in the furnace to the set temperature through heating temperature control. The set temperature is 420 degrees Celsius, and the heating time is set to 430 seconds;

[0048] S3: Evacuate: Evacuate the PECVD deposition furnace for 650 seconds, and turn on the auxiliary heat at the bottom and top of the furnace tube to assist in rapid temperature rise and improve the temperature distribution in the tube so that all parts of the graphite boat are heated evenly. The auxiliary heat temperature is 420 degrees Celsius and the auxiliary heat start time is 550 seconds.

[0049] S4: Detect gas leakage;

[0050] S5: Pre-ventilation-constant pressure: Pre-ventilation is performed to maintain a constant pressure in the PECVD deposition furnace;

[0051] S6: Tunneling layer deposition, before depositing different film layers, the same gas of the same layer is pre-deposited at a constant pressure, and then evacuated. The purpose of evacuation is to remove the remaining unreacted or reactant to facilitate the next step of depositing other films. The deposition thickness is 2nm, the deposition time is 110s, the laughing gas flow rate is 8500sccm, and the RF power is 11000W;

[0052] S7: Pre-ventilation-constant pressure: Pre-ventilation is performed again to maintain a constant pressure in the PECVD deposition furnace;

[0053] S8: Deposition of phosphorus-doped amorphous silicon. After completion, vacuum treatment and pre-ventilation constant pressure treatment are carried out. The specific steps of phosphorus-doped amorphous silicon deposition are: it is divided into three steps of deposition. The first step parameters are deposition time of 150s, silane flow rate of 2400sccm, hydrogen flow rate of 9500sccm, phosphine flow rate of 250sccm, and RF power of 10000W; the second step parameters are deposition time of 200s, silane flow rate of 2400sccm, hydrogen flow rate of 8300sccm, and phosphine flow rate of The parameters of the third step are deposition time of 350s, silane flow rate of 2400sccm, hydrogen flow rate of 8300sccm, phosphine flow rate of 450sccm, RF power of 12000W, and the total film thickness of phosphorus-doped amorphous silicon deposition is 100nm; the first and second steps are both lightly doped, and the third step is heavily doped, the purpose of which is to reduce the phosphorus content in the deposited layer in contact with the tunneling layer, reduce the internal expansion of phosphorus, and thereby reduce parasitic absorption.

[0054] S9: preparing a mask, preparing an oxide layer mask to protect the poly-si layer during the subsequent cleaning process;

[0055] S10: Vacuum and purge, and after back pressure, take the graphite boat out of the deposition furnace to complete the preparation.

[0056] The product of this program parameter has almost no black spots, and the proportion of graphite boat card point printing is 0.5-0.7%. Figure 2 shown.

[0057] Example 2

[0058] S1: Entering the boat: insert the silicon wafer that has been cleaned and textured, front boron diffusion to make PN and SE, back boron oxidation, and alkali polishing into the graphite boat and sent to the PECVD deposition furnace;

[0059] S2: Heating: Close the door of the PECVD deposition furnace, and raise the temperature in the furnace to the set temperature through heating temperature control. The set temperature is 420 degrees Celsius, and the heating time is set to 430 seconds;

[0060] S3: Evacuate: Evacuate the PECVD deposition furnace for 650 seconds, and turn on the auxiliary heat at the bottom and top of the furnace tube to assist in rapid temperature rise and improve the temperature distribution in the tube so that all parts of the graphite boat are heated evenly. The auxiliary heat temperature is 420 degrees Celsius and the auxiliary heat start time is 550 seconds.

[0061] S4: Detect gas leakage;

[0062] S5: Pre-ventilation-constant pressure: Pre-ventilation is performed to maintain a constant pressure in the PECVD deposition furnace;

[0063] S6: Tunneling layer deposition, before depositing different film layers, the same gas of the same layer is pre-deposited at a constant pressure, and then evacuated. The purpose of evacuation is to remove the remaining unreacted or reactant to facilitate the next step of depositing other films. The deposition thickness is 1.5nm, the deposition time is 100s, the laughing gas flow rate is 9000sccm, and the RF power is 10000W;

[0064] S7: Pre-ventilation-constant pressure: Pre-ventilation is performed again to maintain a constant pressure in the PECVD deposition furnace;

[0065] S8: phosphorus-doped amorphous silicon deposition, after which vacuum treatment and pre-ventilation constant pressure treatment are performed. The specific steps of phosphorus-doped amorphous silicon deposition are: a total of three steps of deposition, the first step parameters are deposition time of 130s, silane flow rate of 2700sccm, hydrogen flow rate of 9900sccm, phosphine flow rate of 280sccm, and RF power of 10000W; the second step parameters are deposition time of 70s, silane flow rate of 2700sccm, hydrogen flow rate of 8500sccm, phosphine flow rate of 540sccm, RF power is 14000W; the parameters for the third step are deposition time of 420s, silane flow rate of 2700sccm, hydrogen flow rate of 8500sccm, phosphine flow rate of 540sccm, RF power of 14000W, and the total film thickness of phosphorus-doped amorphous silicon deposition is 120nm; the first and second steps are both lightly doped, and the third step is heavily doped, the purpose of which is to reduce the phosphorus content in the deposition layer in contact with the tunneling layer, reduce the internal expansion of phosphorus, and thereby reduce parasitic absorption.

[0066] S9: preparing a mask, preparing an oxide layer mask to protect the poly-si layer during the subsequent cleaning process;

[0067] S10: Vacuum and purge, and after back pressure, take the graphite boat out of the deposition furnace to complete the preparation.

[0068] The product of this program parameter has almost no black spots, and the proportion of graphite boat card point printing is 0.1%. Figure 3 shown.

[0069] It can be concluded from the test results of Examples 1, 2 and Comparative Example 1 that by setting the auxiliary heat on in the vacuum step and depositing a thinner tunneling layer at a low deposition rate, the thickness and uniformity of the oxide layer at the stuck point where the graphite boat contacts the silicon wafer are improved, thereby improving the EL yield of the product.

[0070] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a back structure of an N-type SE-TOPCon battery by PECVD, characterized in that: The following steps are involved: S1: Putting into the boat: inserting the silicon wafer after cleaning and texturing, front boron diffusion to make PN and SE, back boron oxidation, and alkaline polishing into the graphite boat and sending it to the PECVD deposition furnace; S2: Heating: Close the door of the PECVD deposition furnace and raise the temperature inside the furnace to the set temperature through heating and temperature control; S3: Evacuate: Evacuate the PECVD deposition furnace and turn on the auxiliary heat at the bottom and top of the furnace tube at the same time; S4: Leak detection: detect gas leakage; S5: Pre-ventilation-constant pressure: Pre-ventilation is performed to maintain a constant pressure in the PECVD deposition furnace; S6: Tunneling layer deposition: before depositing different film layers, pre-deposit the same gas of the layer at a constant pressure, and then evacuate; S7: Pre-ventilation-constant pressure: Pre-ventilation is performed again to maintain a constant pressure in the PECVD deposition furnace; S8: phosphorus-doped amorphous silicon deposition, after which vacuum treatment and pre-ventilation constant pressure treatment are performed. The specific steps of phosphorus-doped amorphous silicon deposition are as follows: The deposition is divided into three steps. The first step parameters are as follows: deposition time is 100-200s, silane flow rate is 2400-3300sccm, hydrogen flow rate is 9200-9900sccm, phosphine flow rate is 250-600sccm, and RF power is 9000-13000W; the second step parameters are as follows: deposition time is 50-200s, silane flow rate is 2200-3000sccm, hydrogen flow rate is 8300-9000sccm, phosphine flow rate is 350-550sccm, and RF power is 11000-15000W; the third step parameters are as follows: deposition time is 350-550s, silane flow rate is 2000-3000sccm, hydrogen flow rate is 8300-9000sccm, phosphine flow rate is 350-550sccm, and RF power is 12000-15000W; S9: preparing a mask; S10: Vacuum and purge, and after back pressure, take the graphite boat out of the deposition furnace to complete the preparation.

2. The method for preparing the back structure of an N-type SE-TOPCon battery by a PECVD method according to claim 1, characterized in that: The temperature in S2 is set to 400-430 degrees Celsius, and the heating time is set to 300-500s.

3. The method for preparing the back structure of an N-type SE-TOPCon battery by a PECVD method according to claim 1, characterized in that: In S3, the auxiliary heating temperature is 400-430 degrees Celsius, and the auxiliary heating start time is 450-600s.

4. The method for preparing the back structure of an N-type SE-TOPCon battery by a PECVD method according to claim 1, characterized in that: In S6, the deposition thickness is 1.5-2.0 nm, the deposition time is 80-115 s, the nitrous oxide flow rate is 8000-11000 sccm, and the RF power is 8500-11000 W.

5. The method for preparing the back structure of an N-type SE-TOPCon battery by PECVD according to claim 2, characterized in that: The total film thickness of the phosphorus-doped amorphous silicon deposition is 95-120 nm.

Citation Information

Patent Citations

  • PECVD reaction furnace with heat source in furnace and control method thereof

    CN108588684A

  • A coating process of solar polycrystalline cell sheet

    CN109103093A

  • Method for preparing silicon wafer composite film through PECVD and preparation method of TOPCon battery

    CN113675295A

  • Thin film package structure, thin film packaging method and display device

    US20210167325A1