Ore dissolving device and method

By designing a ore-soluble device containing multi-layer filters and precipitant, the problem of removing impurities during calcium ion extraction in magnesium slag is solved, and efficient calcium ion extraction and carbon dioxide immobilization is achieved, reducing energy consumption and land occupation, and improving Product purity and absorption rate.

CN117660770BActive Publication Date: 2024-11-15YUANCHU TECH (BEIJING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311616103.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-29
Publication Date
2024-11-15
Estimated Expiration
2043-11-29

AI Technical Summary

Technical Problem

In the prior art, when extracting calcium ions from magnesium slag, it is difficult to effectively remove impurities such as iron and aluminum, resulting in a decrease in the purity of calcium ions, and the process cost is high and energy consumption is large. The resources in magnesium slag are not fully utilized, so there is an environment. Pollution problem.

Method used

Design a kind of ore-soluble device, including ore-soluble filter slag area, iron-removing aluminum area and leaching liquid storage area, leaching calcium ions in magnesium slag through ammonium chloride, and use precipitant in the iron-removing aluminum area Remove iron and aluminum impurities, improve the purity and extraction rate of calcium ions, and use top-down structure and multi-layer filter to improve the precipitation effect, reducing energy consumption and land occupation.

Benefits of technology

The extraction rate of calcium ions is achieved to reach more than 95%, the purity and absorption rate of calcium carbonate is improved, energy consumption and land occupation are reduced, and the efficient immobilization of carbon dioxide is achieved without the need for acid or alkali regulators, which reduces safety. The use of hidden dangers and crystal form control agents.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117660770B_ABST
    Figure CN117660770B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of industrial solid waste utilization, and in particular to a ore dissolving device and method, comprising a tank body and an ore dissolving area, an ore dissolving residue removal area, an iron and aluminum removal area, and a leaching solution storage area arranged in sequence from top to bottom in the tank body, the bottom of the ore dissolving area is connected to the ore dissolving residue removal area, a plurality of first overflow pipes are evenly arranged in the ore dissolving residue removal area, and one end of each first overflow pipe is connected to the ore dissolving residue removal area, and the other end is connected to the iron and aluminum removal area; a plurality of second overflow pipes are evenly arranged in the iron and aluminum removal area, and one end of each second overflow pipe is connected to the iron and aluminum removal area, and the other end is connected to the leaching solution storage area; one or more precipitant sprayers are also arranged above the iron and aluminum removal area. The ore dissolving device of the present invention can not only fully leach calcium in magnesium slag, with a calcium extraction rate of more than 90%, but also effectively eliminate impurities such as iron and aluminum in the ore dissolving solution, thereby improving the purity of calcium ions in the leaching solution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of industrial solid waste utilization, and in particular to an ore dissolving device and method for purifying power plant flue gas by utilizing magnesium slag. Background Art

[0002] As an important inorganic chemical raw material, light calcium carbonate is widely used in papermaking, rubber, plastic, coating, medicine, food and other industries, especially as one of the most commonly used fillers in the papermaking industry. At present, the preparation of light calcium carbonate mostly adopts the carbonization method, that is, lime is obtained by calcining limestone, lime is digested to obtain lime slurry, and carbon dioxide produced by calcining limestone is introduced into the lime slurry for carbonization to generate calcium carbonate.

[0003] At present, the flue gas from thermal power plants is mostly discharged directly into the atmosphere after desulfurization, denitrification and dust removal. The flue gas still contains a certain concentration of carbon dioxide that cannot be used, which not only wastes resources but also pollutes the environment. The more stable carbon dioxide fixation method at present is to convert carbon dioxide into carbonate mineral forms such as calcium carbonate and magnesium carbonate.

[0004] For example, CN114933323A discloses a method for preparing high-purity calcium carbonate by treating waste cement powder with ammonium chloride in combination with carbon dioxide. A "leaching-carbonization" cycle process is designed to seal a large amount of carbon dioxide and extract 97.8% pure calcium carbonate from waste cement powder. However, this method requires the addition of ammonia water for pH adjustment, and is only in the pilot stage, and has not yet considered the problem of three wastes treatment during industrial expansion.

[0005] CN109704380A discloses a method for continuously preparing light calcium carbonate filler using power plant flue gas, wherein lime is digested with hot water to obtain a coarse pulp, the coarse pulp is concentrated and then filtered and suspended by a suspension separator to obtain a refined pulp, and then the refined pulp is put into a carbonizing tower, a crystal form control agent is added, and the treated power plant flue gas is introduced into the carbonizing tower after stirring evenly for carbonization, and the pH and conductivity are detected online during the carbonization process, and the carbonization end point is judged by pH and conductivity, and a pH adjusting agent is added to the carbonized cooked pulp, and impurities are removed by a 325 mesh sieve, and finally a light calcium carbonate filler is obtained. However, this method requires the addition of a pH adjusting agent and a crystal form control agent, and the solution is slightly changed and cannot be accurately judged by pH and conductivity, and more storage tanks are needed to store acid and alkali, which has a potential safety hazard. In addition, the crystal form control agent will also adhere to the product, resulting in a decrease in the purity of calcium carbonate.

[0006] CN111214938A discloses a carbon dioxide mineralization reaction device and a carbon dioxide fixation method, which can capture carbon dioxide from exhaust gas without a separate carbon dioxide capture process, and convert carbon dioxide into carbonate mineral form with high efficiency and purity, and minimize the volume of process equipment, improve space efficiency, and convert carbon dioxide into carbonate mineral form with high conversion rate even at normal temperature and pressure. However, the device needs to prepare hydrochloric acid by electrolysis for later mineralization, which consumes a lot of electricity and has a high carbon fixation cost.

[0007] Magnesium slag is an industrial waste residue produced by silicon thermal magnesium smelting. According to statistics, the production of 1 ton of primary magnesium will produce 5.5-10 tons of magnesium reduction slag. At present, magnesium smelters mainly treat magnesium slag waste by landfilling or dumping at fixed locations. These unreasonable disposal methods will not only cause environmental pollution problems such as air and soil, but also waste a lot of resources and materials.

[0008] In recent years, with the rapid development of my country's magnesium smelting industry, the annual output of primary magnesium and magnesium alloys has increased year by year, and the amount of magnesium slag discharged has also increased. Magnesium slag has high content of silicon, magnesium and calcium, which can be used to absorb carbon dioxide in flue gas and generate economically beneficial calcium magnesium carbonate. While achieving emission reduction, it is also of great significance to solve the pollution problem of magnesium reduction slag.

[0009] For example, CN116282116A discloses a circulation process for mineralizing carbon dioxide from magnesium slag, which leaches magnesium slag with ammonium chloride, and uses the leachate to seal carbon dioxide in situ to prepare high-purity calcium carbonate and magnesium carbonate products. The process can process magnesium slag solid waste such as steel slag and carbide slag and carbon dioxide in factory tail gas, and simultaneously prepare high value-added products such as calcium carbonate and magnesium carbonate, and the ammonium chloride solution is also repeatedly recycled, and no wastewater and waste gas are generated in the process. However, this method has not yet considered the impact of impurities such as iron and aluminum in magnesium slag on the mineralization effect of carbon dioxide.

[0010] In view of this, the present invention is proposed. Summary of the invention

[0011] The object of the present invention is to provide a ore dissolving device and method, which can not only fully leach calcium in magnesium slag, with a calcium extraction rate of more than 95%, but also effectively eliminate impurities such as iron and aluminum in the molten ore solution, thereby improving the purity of calcium ions in the leaching solution.

[0012] In a first aspect, the present invention provides an ore dissolving device, comprising a tank body and an ore dissolving area, an ore dissolving and slag removing area, an iron and aluminum removing area and a leaching liquid storage area arranged in sequence from top to bottom inside the tank body,

[0013] The bottom of the ore dissolution zone is connected to the ore dissolution removal and slag filtering zone.

[0014] A plurality of first overflow pipes are evenly arranged in the desolventizing slag area, and one end of each of the first overflow pipes is connected to the desolventizing slag area, and the other end is connected to the iron and aluminum removal area;

[0015] A plurality of second overflow pipes are evenly arranged in the iron removal and aluminum removal area, and one end of each of the second overflow pipes is connected to the iron removal and aluminum removal area, and the other end is connected to the leaching liquid storage area;

[0016] One or more precipitant sprayers are also arranged above the iron and aluminum removal zone.

[0017] As a preferred embodiment of the present technical solution, the bottoms of the ore dissolution zone, the ore dissolution slag removal zone and the iron and aluminum removal zone are all in a conical structure, and the bottoms of the ore dissolution zone, the ore dissolution slag removal zone and the iron and aluminum removal zone are respectively provided with a first mixed liquid outlet, a second mixed liquid outlet and a third mixed liquid outlet;

[0018] The second mixed liquor outlet is communicated with the upper part of the ore dissolution and slag removal zone through a first pipeline, and the third mixed liquor outlet is communicated with the upper part of the iron and aluminum removal zone through a second pipeline.

[0019] As a preferred embodiment of the present technical solution, the first pipe and the second pipe are respectively provided with a first filter and a second filter.

[0020] As a preferred embodiment of the present technical solution, a plurality of sedimentation wedge assemblies are provided inside the ore dissolution and slag removal zone and the iron and aluminum removal zone, and the sedimentation wedge assemblies include a plurality of first sedimentation wedges inclined inwardly and a plurality of second sedimentation wedges inclined outwardly, and the second sedimentation wedges are arranged above the first sedimentation wedges.

[0021] As a preferred embodiment of the present technical solution, a feed port, a liquid replenishment port and an exhaust gas discharge port are provided on the top of the ore dissolution zone, a feed discharge mechanism is provided on the feed port, and an iron removal component is provided at one end of the feed discharge mechanism close to the feed port.

[0022] As a preferred embodiment of the present technical solution, a stirring mechanism is provided inside the ore dissolving zone, and a circulating water heating layer is provided outside the ore dissolving zone.

[0023] As a preferred embodiment of the present technical solution, an online liquid level meter is provided inside the ore dissolution zone, and an online viscosity detector is installed at the outlet of the first mixed liquid;

[0024] An leaching liquid outlet is provided at the bottom of the leaching liquid storage area, and an online calcium ion monitor and a flow meter are installed at the leaching liquid outlet;

[0025] The valves at the first mixed liquid outlet and the leaching liquid outlet are both pneumatic regulating valves.

[0026] In a second aspect, the present invention further discloses a method for dissolving ore using the above-mentioned ore dissolving device, comprising the following steps:

[0027] S1, magnesium slag enters the ore dissolution area through the feeding mechanism, and the magnesium slag is leached by ammonium chloride, and the obtained ore dissolution liquid enters the ore dissolution and slag removal area through the first mixed liquid outlet;

[0028] S2, in the ore removal residue removal area, the ore removal solution is settled by the settling wedge assembly and then enters the first filter through the second mixed liquid outlet, and the obtained filtrate returns to the ore removal residue removal area again; the supernatant in the ore removal residue removal area overflows to the iron and aluminum removal area through multiple first overflow pipes;

[0029] S3. In the iron and aluminum removal area, the precipitant sprayer sprays the precipitant on the surface of the overflow liquid. After the mixed liquid is settled by the settling wedge assembly, it enters the second filter through the third mixed liquid outlet, and the obtained filtrate returns to the iron and aluminum removal area again; the supernatant in the iron and aluminum removal area overflows to the leaching liquid storage area through multiple second overflow pipes and is discharged from the leaching liquid outlet.

[0030] As a preferred embodiment of the present technical solution, in step S1, the feeding rate of magnesium slag is 550-700 kg / h, the mass ratio of magnesium slag to ammonium chloride is 1:(1.0-1.2), wherein the mass concentration of ammonium chloride is 6-12%.

[0031] As a preferred embodiment of the present technical solution, in step S3, the precipitant includes any one or more of ammonia water, sodium hydroxide, sodium carbonate and ammonium bicarbonate, and the volume of the precipitant to the overflow liquid is 1:(10-15), wherein the molar concentration of the precipitant is 0.01-0.02 mol / L.

[0032] Compared with the prior art, the ore dissolving device and method of the present invention have at least the following effects:

[0033] 1. The ore dissolving device of the present invention is provided with an ore dissolving area, an ore dissolving residue removal area, an iron and aluminum removal area, and a leaching solution storage area in sequence from top to bottom. In the ore dissolving area, ammonium chloride is used to leach calcium ions in magnesium slag, and the leached ore solution enters the ore dissolving residue removal area; after impurities such as calcium carbonate and silicon dioxide in the ore dissolving solution are precipitated and filtered out in the ore dissolving residue removal area, the supernatant overflows to the iron and aluminum removal area; in the iron and aluminum removal area, impurities such as iron and aluminum in the mixed solution are removed by a precipitant, and the supernatant further overflows to the leaching solution storage area. Therefore, the ore dissolving device of the present invention can not only fully leach calcium in magnesium slag under the interaction of the ore dissolving area, the ore dissolving residue removal area, the iron and aluminum removal area, and the leaching solution storage area, with a calcium extraction rate of more than 90%, but can also effectively eliminate impurities such as iron and aluminum in the ore dissolving solution, thereby improving the purity of calcium ions in the leaching solution;

[0034] 2. When the leaching solution prepared by the ore dissolving device of the present invention is used for carbon dioxide mineralization absorption, high-purity calcium carbonate can be obtained, and the carbon dioxide absorption rate can reach more than 95%. In addition, during the operation, it is not necessary to add acid or alkali to adjust the pH, and it is not necessary to add a crystal form control agent. According to tests, the calcium carbonate obtained by this method is 200-300% more efficient than the heavy calcium carbonate used in power plant desulfurization, and does not require grinding, which greatly reduces energy consumption;

[0035] 3. The ore dissolving device of the present invention reduces the floor space, comprehensively utilizes the space, reduces the water transportation in the absorption and separation units, improves the process efficiency, reduces the process energy consumption, and has low operating costs;

[0036] 4. The ore dissolving device of the present invention has a simple process. Through the online calcium ion monitor, ammonia concentration monitor, viscosity detector and conductivity detector, the reaction process can be automatically controlled by PLC to achieve fully automated production;

[0037] 5. The present invention utilizes magnesium slag to purify the flue gas of a power plant. On the basis of reducing the exhaust gas emission, the magnesium slag discharged from the metal magnesium plant is used to recycle the carbon dioxide in the exhaust gas. During the reaction, the leaching liquid is used for carbon fixation, the generated ammonium chloride and washing water can be recycled, the water vapor in the flue gas can be used as production water after cooling, the flue gas heat can be used as a heat source for the ore dissolution reaction, the tail gas generated during the production process contains ammonia, which can enter the denitrification system through the pipeline, and the waste slag generated during the production process can be used as a raw material for the cement plant. Therefore, the present invention can make full use of the three wastes, and has good economic and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] In order to more clearly illustrate the specific implementation methods of the present invention or the technical solutions in the prior art, the drawings required for use in the specific implementation methods or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are some implementation methods of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0039] Figure 1 It is a schematic diagram of the structure of the ore dissolving device of the present invention;

[0040] Figure 2 It is the principle diagram of the ore dissolving device of the present invention;

[0041] Figure 3 The present invention is a flow chart of using magnesium slag to purify flue gas from a power plant.

[0042] Reference numerals:

[0043] 1: ore dissolution area; 2: ore dissolution and slag removal area; 3: iron and aluminum removal area; 4: leachate storage area; 5: first overflow pipe; 6: second overflow pipe; 7: precipitant sprayer; 8: first mixed liquid outlet; 9: second mixed liquid outlet; 10: third mixed liquid outlet; 11: first pipeline; 12: second pipeline; 13: first filter; 14: second filter; 15: first sedimentation wedge; 16: second sedimentation wedge; 17: feed inlet; 18: liquid replenishment inlet; 19: tail gas discharge outlet; 20: feed discharge mechanism; 21: iron removal component; 22: stirring mechanism; 23: circulating water heating layer; 24: leachate outlet. DETAILED DESCRIPTION

[0044] It should be noted that the following detailed descriptions are illustrative and are intended to provide further explanation of the present application. Unless otherwise specified, all technical and scientific terms used herein have the same meanings as those commonly understood by those skilled in the art to which the present application belongs.

[0045] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form also includes the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this description, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0046] The technical solution of the present invention will be clearly and completely described below in conjunction with the embodiments. Obviously, the described embodiments are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0047] Example 1

[0048] like Figure 1-2 As shown, this embodiment provides a ore dissolving device, including a tank body and an ore dissolving area 1, an ore dissolving and slag removing area 2, an iron and aluminum removing area 3 and a leaching liquid storage area 4 which are sequentially arranged inside the tank body from top to bottom.

[0049] The bottom of the ore dissolution zone 1 is connected with the ore dissolution residue removal zone 2, that is, the ore dissolution solution obtained in the ore dissolution zone 1 can directly enter the ore dissolution residue removal zone 2; a plurality of first overflow pipes 5 are evenly arranged in the ore dissolution residue removal zone 2, and one end of each first overflow pipe 5 is connected with the ore dissolution residue removal zone 2, and the other end is connected with the iron-aluminum removal zone 3, that is, the supernatant after sedimentation and separation in the ore dissolution residue removal zone 2 can overflow to the iron-aluminum removal zone 3 through the first overflow pipe 5 to further remove impurities such as iron and aluminum in the ore dissolution solution; a plurality of second overflow pipes 6 are evenly arranged in the iron-aluminum removal zone 3, and one end of each second overflow pipe 6 is connected with the iron-aluminum removal zone 3, and the other end is connected with the leaching liquid storage zone 4; one or more precipitant sprayers 7 are also arranged above the iron-aluminum removal zone 3, and the iron and aluminum ions in the ore dissolution solution can be effectively precipitated by spraying the precipitant on the overflow liquid surface through the precipitant sprayer 7.

[0050] In the ore dissolution area 1 of the present embodiment, ammonium chloride is used to leach calcium ions in magnesium slag, and the leached ore solution enters the ore dissolution filter residue removal area 2; after impurities such as calcium carbonate and silicon dioxide in the ore dissolution solution are precipitated and filtered out in the ore dissolution filter residue removal area 2, the supernatant overflows to the aluminum and iron removal area; in the iron and aluminum removal area 3, impurities such as iron and aluminum in the mixed solution are removed by a precipitant, and the obtained supernatant further overflows to the leaching solution storage area 4, and can be used for carbon dioxide mineralization absorption.

[0051] Therefore, the ore dissolving device of the present invention can not only fully leach calcium in magnesium slag under the interaction of ore dissolving area 1, ore dissolving slag removal area 2, iron and aluminum removal area 3 and leaching solution storage area 4, with the calcium extraction rate reaching more than 95%, but also effectively eliminate impurities such as iron and aluminum in the ore dissolving solution, thereby improving the purity of calcium ions in the leaching solution.

[0052] When the above leaching solution is used for carbon dioxide mineralization absorption, the whiteness and purity of calcium carbonate can be significantly improved, the added value of the product can be increased, the carbon dioxide absorption rate can reach more than 95%, and during the operation, the ammonia generated by magnesium slag and ammonium chloride can form a buffer solution with ammonium chloride. Therefore, during the mineralization process, there is no need to add acid or alkali to adjust the pH, and there is no need to add a crystal control agent. According to tests, the calcium carbonate obtained by this method is 200-300% more efficient than the heavy calcium carbonate used in power plant desulfurization, and no grinding is required, which greatly reduces energy consumption.

[0053] On the basis of the above technical scheme, it is further preferred that the bottoms of the ore dissolution zone 1, the ore dissolution slag zone 2 and the iron-aluminum removal zone 3 are all of a conical structure to improve the precipitation effect of the ore dissolution solution in each zone, and the slag is enriched at the bottom of the ore dissolution slag zone 2 and the iron-aluminum removal zone 3, and the bottoms of the ore dissolution zone 1, the ore dissolution slag zone 2 and the iron-aluminum removal zone 3 are respectively provided with a first mixed liquor outlet 8, a second mixed liquor outlet 9 and a third mixed liquor outlet 10; the ore dissolution zone 1 enters the ore dissolution slag zone 2 through the first mixed liquor outlet 8, the second mixed liquor outlet 9 is connected with the top of the ore dissolution slag zone 2 through the first pipeline 11, so as to transport the mixture of the filtrate and slag of the ore dissolution slag zone 2 back to the ore dissolution slag zone 2 for further sedimentation, and the third mixed liquor outlet 10 is connected with the top of the iron-aluminum removal zone 3 through the second pipeline 12, so as to transport the mixture of the filtrate and slag of the iron-aluminum removal zone 3 back to the iron-aluminum removal zone 3 for further sedimentation.

[0054] In this embodiment, in order to timely filter out the residues produced in the ore dissolution removal residue zone 2 and the iron and aluminum removal zone 3, a first filter 13 and a second filter 14 are respectively arranged on the first pipeline 11 and the second pipeline 12. The filtrate after being filtered by the first filter 13 and the second filter 14 respectively enters the ore dissolution removal residue zone 2 and the iron and aluminum removal zone 3 for further sedimentation and separation. Among them, the residues produced by the first filter 13 can be transported to the cement plant as a raw material for cement production, and the residues produced by the second filter 14 can be directly transported to the steel plant.

[0055] On the basis of the above technical solution, in order to further improve the sedimentation effect of the ore removal residue area 2 and the iron and aluminum removal area 3, a plurality of sedimentation wedge assemblies are arranged inside the ore removal residue area 2 and the iron and aluminum removal area 3, and the present invention does not strictly limit the structure and arrangement of the sedimentation wedge assembly. Specifically, the sedimentation wedge assembly may include a plurality of first sedimentation wedges 15 inclined inwardly and a plurality of second sedimentation wedges 16 inclined outwardly, wherein the second sedimentation wedges 16 are arranged above the first sedimentation wedges 15. Therefore, the second sedimentation wedges 16 and the first sedimentation wedges 15 can sequentially sediment and separate the molten ore solution.

[0056] In this embodiment, a feed port 17, a liquid replenishment port 18 and an exhaust gas discharge port 19 are sequentially opened on the top of the ore dissolution zone 1, wherein a feeding mechanism 20 is provided on the feed port 17, and an iron removal component 21 is provided at one end of the feeding mechanism 20 close to the feed port 17, and magnesium slag is injected into the ore dissolution zone 1 through the feeding mechanism 20. While feeding, the iron removal component 21 can remove the magnetic iron element or iron oxide compounds in the magnesium slag; the liquid replenishment port 18 is mainly used for replenishing ammonium chloride solution; the exhaust gas discharge port 19 is mainly used for discharging waste gas generated in the ore dissolution process, and the waste gas generated is connected with the exhaust gas emission generated by the mineralization reaction device, and enters the denitrification system of the power plant in a unified manner.

[0057] Specifically, a stirring mechanism 22 is provided inside the ore dissolution area 1 to increase the disturbance degree of the leaching system and improve the leaching efficiency. In addition, a circulating water heating layer 23 is also provided outside the ore dissolution area 1 to heat the leaching system. A circulating water inlet and a circulating water outlet are provided on the circulating water heating layer 23. The circulating water is mainly provided by the flue gas cooling tower of the power plant. One pipe of the cooling tower outlet pipe supplies the circulating water heating layer 23, and the other is connected to the circulating water system. The obtained condensed water is stored in a water tank.

[0058] On the basis of the above technical solution, it is further preferred that an online level meter is also provided inside the ore dissolution zone 1, through which the amount of liquid in the ore dissolution zone 1 can be monitored in real time, and the metering pump is controlled by the PLC to replenish the liquid from the ammonium chloride tank, and the ammonium chloride used here is the ammonium chloride produced in the carbon dioxide mineralization reaction, so the ammonium chloride can be recycled in this device. In addition, an online viscosity detector is also installed at the first mixed liquid outlet 8, and the flow rate of the valve flowing into the ore dissolution slag removal zone 2 is automatically adjusted by the PLC controller.

[0059] An extraction liquid outlet 24 is provided at the bottom of the extraction liquid storage area 4, and an online calcium ion monitor and a flow meter are installed at the extraction liquid outlet 24. The flow rate is adjusted by the calcium ion concentration to connect the extraction liquid to the carbon dioxide mineralization device, and the carbon dioxide conversion rate is calculated by the PLC controller to automatically control the flow entering the mineralization device.

[0060] The valves at the first mixed liquid outlet 8 and the leaching liquid outlet 24 are preferably pneumatic regulating valves.

[0061] like Figure 3 As shown, the leaching solution obtained in this embodiment can be directly pumped into the carbon dioxide absorption and mineralization device to absorb the carbon dioxide in the flue gas of the power plant. The flue gas of the power plant is dehydrated and impurities are removed by a cooling tower and a filter tower. The cooled water is used to prepare the product slurry. The treated flue gas is passed through a compressor into the carbon dioxide absorption and mineralization device. An online carbon dioxide concentration analyzer is installed at the flue gas inlet and outlet. The flow rate of the leaching solution is automatically adjusted by the PLC controller according to the changes in carbon dioxide and calcium ion concentrations. Since magnesium slag and ammonium chloride generate ammonia and form a buffer solution with ammonium chloride, there is no need to add a pH regulator during the mineralization reaction. After the mineralized liquid enters the sedimentation tank for precipitation, the bottom slurry is pumped into a filter press for filtration, and the filtrate enters the ammonium chloride concentration equipment. The concentrated solution is returned to the ammonium chloride storage tank, and the condensed water returns to the water tank. The filter cake is prepared into a slurry according to the density of 1180-1250kg / m 3, enters the desulfurization system through pipelines, the dilution water comes from the water tank, the tail gas from the ore dissolution process and the mineralization process enters the denitrification system through pipelines, and the ammonia concentration is measured by an online monitoring ammonia analyzer to reduce the use of urea in the denitrification system. Therefore, the ore dissolution device in this embodiment is applied to solve the problem of carbon dioxide emissions in power plants, which not only improves the absorption rate of carbon dioxide, but also the device can be automated throughout the production process, reducing labor costs.

[0062] Example 2

[0063] The magnesium slag discharged from a magnesium metal plant was treated using the most preferred ore dissolving device, and its main composition was determined by melt X-ray fluorescence spectrometry. The results are shown in Table 1.

[0064] Table 1 XRF composition analysis of magnesium slag

[0065]

[0066] The specific steps include:

[0067] S1, magnesium slag enters the ore dissolution zone 1 through the feeding mechanism 20, the feeding speed is 550kg / h, the ammonium chloride solution is replenished from the ammonium chloride tank through the PLC-controlled metering pump, the concentration of the ammonium chloride solution is 10%, the mass ratio of magnesium slag to ammonium chloride solution is 1:1.2, the mineralization temperature is controlled at 50°C, and the obtained ore dissolution solution enters the ore dissolution and slag removal zone 2 through the first mixed solution outlet 8;

[0068] S2, in the ore removal residue removal zone 2, the molten ore is settled by the settling wedge assembly, and then enters the first filter 13 through the second mixed liquid outlet 9, and the obtained filtrate returns to the ore removal residue removal zone 2 again, and the obtained residue is transported to the cement plant; the supernatant of the ore removal residue removal zone 2 overflows to the iron and aluminum removal zone 3 through multiple first overflow pipes 5;

[0069] S3. In the iron and aluminum removal zone 3, the precipitant sprayer 7 sprays sodium hydroxide with a molar concentration of 0.01-0.02 mol / L on the surface of the overflow liquid, and the volume of sodium hydroxide to the overflow liquid is 1:(10-15). After the mixed liquid is settled by the settling wedge assembly, it enters the second filter 14 through the third mixed liquid outlet 10, and the obtained filtrate returns to the iron and aluminum removal zone 3 again, and the obtained filter residue is transported to the steel plant; the supernatant of the iron and aluminum removal zone 3 overflows to the leaching liquid storage area 4 through multiple second overflow pipes 6 and is discharged from the leaching liquid outlet 24.

[0070] The results showed that the concentration of calcium ions in the leaching solution was 0.7 mol / L, the concentration of iron ions was 0.001 mol / L, the concentration of aluminum ions was 0.001 mol / L, and the extraction rate of calcium ions in the magnesium slag was 92%.

[0071] Control the flow rate of the leaching liquid to 1.5-2m 3 / h, after the leaching liquid is discharged to the carbon dioxide absorption and mineralization device, online carbon dioxide detectors are installed at the gas inlet and outlet to detect the carbon dioxide concentration. The calculated carbon dioxide absorption rate is 92%, the whiteness of the obtained calcium carbonate is 98.5, and the purity is 99%.

[0072] Comparative Example 1

[0073] The device in Example 1 is used, but the supernatant in the ore dissolution and slag filtering zone 2 overflows to the leaching liquid storage tank through multiple first overflow pipes 5, without passing through the iron and aluminum removal zone, to treat the magnesium slag in Example 1. The specific treatment method is as follows:

[0074] S1, magnesium slag enters the ore dissolution zone 1 through the feeding mechanism 20, the feeding speed is 550kg / h, the ammonium chloride solution is replenished from the ammonium chloride tank through the PLC-controlled metering pump, the concentration of the ammonium chloride solution is 10%, the mass ratio of magnesium slag to ammonium chloride solution is 1:1.2, the mineralization temperature is controlled at 50°C, and the obtained ore dissolution solution enters the ore dissolution and slag removal zone 2 through the first mixed solution outlet 8;

[0075] S2, in the desolventizing filter residue area 2, the molten ore solution is settled by the settling wedge assembly, and then enters the first filter 13 through the second mixed liquid outlet 9, and the obtained filtrate returns to the desolventizing filter residue area 2 again, and the obtained filter residue is transported to the cement plant; the supernatant of the desolventizing filter residue area 2 overflows to the leaching liquid storage tank through multiple first overflow pipes 5;

[0076] The results showed that the calcium ion concentration in the leaching solution was 0.6 mol / L, the iron ion concentration was 0.1 mol / L, the aluminum ion concentration was 0.05 mol / L, and the extraction rate of calcium ions in the magnesium slag was 85%.

[0077] Control the flow rate of the leaching liquid to 1.5-2m 3 / h, after the leaching liquid is discharged to the carbon dioxide absorption and mineralization device, online carbon dioxide detectors are installed at the gas inlet and outlet to detect the carbon dioxide concentration. The carbon dioxide absorption rate is calculated to be 90%, and the whiteness of the obtained calcium carbonate is 88.4 and the purity is 92%.

[0078] Comparative Example 2

[0079] The magnesium slag in Example 1 was treated using a conventional stirred reactor type ore dissolving device. The specific treatment method is as follows:

[0080] S1. Add 500 kg of the above magnesium slag powder and 6 t of 10% ammonium chloride solution into a reactor with a stirring device, control the mineralization temperature to 40°C, and react for 2 hours;

[0081] S2. After the reaction is completed, the leaching liquid is discharged through the discharge port and then filtered;

[0082] The results showed that the calcium ion concentration in the leaching solution was 0.5 mol / L, the iron ion concentration was 0.2 mol / L, the aluminum ion concentration was 0.08 mol / L, and the extraction rate of calcium ions in the magnesium slag was 80%.

[0083] Control the flow rate of the leaching liquid to 1.5-2m 3 / h, after the leaching liquid is discharged to the carbon dioxide absorption and mineralization device, online carbon dioxide detectors are installed at the gas inlet and outlet to detect the carbon dioxide concentration. The carbon dioxide absorption rate is calculated to be 85%, and the whiteness of the obtained calcium carbonate is 83.5 and the purity is 87.

[0084] The treatment effects of Example 2 and Comparative Example 1 on magnesium slag are shown in Table 2.

[0085] Table 2 Treatment effects of Example 2 and Comparative Example 1

[0086]

[0087] In summary, the ore dissolving device of the present invention is used to leach magnesium slag, and the leaching solution is used to purify the flue gas of the power plant, which can not only fully leach the calcium in the magnesium slag with a calcium extraction rate of more than 90%, but also effectively eliminate impurities such as iron and aluminum in the ore dissolving solution, thereby improving the whiteness and purity of calcium carbonate.

[0088] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.

Claims

1. A ore dissolving device, characterized in that: The invention comprises a tank body and a ore dissolution area (1), an ore dissolution slag removal area (2), an iron and aluminum removal area (3) and a leaching liquid storage area (4) arranged inside the tank body. The ore dissolution zone (1) is connected to the ore dissolution and slag removal zone (2). A plurality of first overflow pipes (5) are evenly arranged in the desolventizing slag zone (2), and one end of each of the first overflow pipes (5) is connected to the desolventizing slag zone (2), and the other end is connected to the iron and aluminum removal zone (3); A plurality of second overflow pipes (6) are arranged in the iron removal and aluminum removal area (3), and one end of each of the second overflow pipes (6) is connected to the iron removal and aluminum removal area (3), and the other end is connected to the leaching liquid storage area (4); One or more precipitant sprayers (7) are also arranged above the iron and aluminum removal zone (3); A plurality of settling wedge assemblies are arranged inside the slag removal zone (2) and the iron and aluminum removal zone (3), wherein the settling wedge assemblies include a plurality of first settling wedges (15) inclined inwardly and a plurality of second settling wedges (16) inclined outwardly, wherein the second settling wedges (16) are arranged above the first settling wedges (15); The method for dissolving ore in the ore dissolving device comprises the following steps: S1, magnesium slag enters the ore dissolution zone (1) through the feeding mechanism (20), the magnesium slag is leached by ammonium chloride, and the resulting ore dissolution solution enters the ore dissolution and slag removal zone (2) through the first mixed solution outlet (8); S2, in the ore removal and slag removal zone (2), the ore removal solution is settled through the settling wedge assembly and then enters the first filter (13) through the second mixed solution outlet (9), and the obtained filtrate is returned to the ore removal and slag removal zone (2) again; the supernatant of the ore removal and slag removal zone (2) overflows to the iron and aluminum removal zone (3) through a plurality of first overflow pipes (5); S3, in the iron removal and aluminum removal zone (3), the precipitant sprayer (7) sprays the precipitant on the surface of the overflow liquid, and the mixed liquid is settled through the settling wedge assembly and enters the second filter (14) through the third mixed liquid outlet (10), and the obtained filtrate returns to the iron removal and aluminum removal zone (3) again; the supernatant of the iron removal and aluminum removal zone (3) overflows to the leaching liquid storage zone (4) through a plurality of second overflow pipes (6) and is discharged from the leaching liquid outlet (24); When the leaching solution is used for mineralization and absorption of carbon dioxide, the whiteness and purity of calcium carbonate can be significantly improved, and the added value of the product can be increased. The absorption rate of carbon dioxide can reach more than 95%, and during the operation, the ammonia generated by magnesium slag and ammonium chloride can form a buffer solution with the ammonium chloride. Therefore, during the mineralization process, there is no need to add acid or alkali to adjust the pH, and there is no need to add a crystal form control agent.

2. The ore dissolving device according to claim 1, characterized in that: The bottoms of the ore dissolution zone (1), the ore dissolution slag removal zone (2) and the iron and aluminum removal zone (3) are either or all of a conical structure, and the bottoms of the ore dissolution zone (1), the ore dissolution slag removal zone (2) and the iron and aluminum removal zone (3) are respectively provided with a first mixed liquid outlet (8), a second mixed liquid outlet (9) and a third mixed liquid outlet (10); The second mixed liquor outlet (9) is connected to the upper part of the desolventizing and slag removal zone (2) through a first pipeline (11), and the third mixed liquor outlet (10) is connected to the upper part of the iron and aluminum removal zone (3) through a second pipeline (12).

3. The ore dissolving device according to claim 2, characterized in that: The first pipe (11) and the second pipe (12) are respectively provided with a first filter (13) and a second filter (14).

4. The ore dissolving device according to claim 1, characterized in that: The top of the ore dissolving area (1) is provided with a feed port (17), a liquid replenishing port (18) and an exhaust gas discharge port (19); a feed discharge mechanism (20) is provided on the feed port (17); and an iron removal component (21) is provided at one end of the feed discharge mechanism (20) close to the feed port (17).

5. The ore dissolving device according to claim 1, characterized in that: A stirring mechanism (22) is arranged inside the ore dissolving area (1), and a circulating water heating layer (23) is arranged outside the ore dissolving area (1).

6. The ore dissolving device according to claim 1, characterized in that: An online liquid level meter is provided inside the ore dissolution zone (1), and an online viscosity detector is installed at the first mixed liquid outlet (8); The bottom of the leachate storage area (4) is provided with an leachate outlet (24), and an online calcium ion monitor and a flow meter are installed at the leachate outlet (24); The valves at the first mixed liquid outlet (8) and the leaching liquid outlet (24) are both pneumatic regulating valves.

7. The ore dissolving device according to claim 1, characterized in that: In step S1, the feeding rate of magnesium slag is 550-700 kg / h, the mass ratio of magnesium slag to ammonium chloride is 1:(1.0-1.2), wherein the mass concentration of ammonium chloride is 6-12%.

8. The ore dissolving device according to claim 1, characterized in that: In step S3, the precipitant includes any one or more of ammonia water, sodium hydroxide, sodium carbonate and ammonium bicarbonate, and the volume of the precipitant to the overflow liquid is 1:(10-15), wherein the molar concentration of the precipitant is 0.01-0.02 mol / L.