Iron-based sky blue glaze and oxidizing atmosphere firing method thereof
By regulating the formulation and firing conditions under an oxidation atmosphere, combined with a specific phase separation structure, the problem of poor stability of traditional sky blue glaze in a reducing atmosphere is solved, and the effect of preparing deep sky blue glaze under an oxidation atmosphere is achieved, reducing the effect of Production costs and equipment requirements.
Patent Information
- Application Number
- CN202311433344.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-10-31
- Publication Date
- 2024-11-29
- Estimated Expiration
- 2043-10-31
AI Technical Summary
Traditional sky blue glaze is poor in firing under a reducing atmosphere and complex process, resulting in low yield and high requirements for equipment and production conditions, making it difficult to control the glaze color.
In an oxidative atmosphere, by regulating the formulation and firing conditions, using the equilibrium characteristics of acid oxide and iron, controlling the presence of divalent iron, combining specific phase separation structures, wet ball milling and spraying glaze methods are used to prepare iron-based sky blue Glaze.
The glaze surface with a deep sky blue effect was successfully fired under an oxidative atmosphere, which reduced the requirements of equipment and production conditions, improved reproducibility and cost-effectiveness, and achieved through the balance control of acid oxide and divalent iron. Controllability of blue tones.
Smart Images

Figure CN117682764B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of ceramic materials, in particular to an iron-based sky blue glaze surface and an oxidizing atmosphere firing method thereof. Background Art
[0002] Ceramic glazes are widely used in the field of ceramic decoration due to their excellent optical decorative effects, mechanical properties and stain resistance. Among them, iron-based colored glazes have been favored and widely used since ancient times because of their varied colors that give ceramic glazes rich artistic decorative effects. The main colors of iron in glazes include light yellow, brown, red, cyan, black and blue. The iron content, firing atmosphere and temperature lead to the valence and existence of iron, and ultimately present precious glazes such as Jianzhan, black glaze, and Jingdezhen Shanqing. Among them, the sky blue glaze, which evolved from "sky blue" and has a sky blue color, is the most fascinating to people because of its deep, elegant and pure coloring effect. Its coloring effect is similar to that of "kiln-changed" blue glaze.
[0003] According to the research on ancient glazes, traditional sky blue glaze is a combination of cobalt, copper, iron, titanium and other metal elements, and is mostly fired in a reducing atmosphere. The reducing atmosphere is mainly achieved by regulating the intake of gas and air, so the overall stability is worse than that of an oxidizing atmosphere. At the same time, the formula is complex, which makes it difficult to control the glaze color and the yield is low. In this regard, it is of positive significance to develop an oxidizing atmosphere sky blue glaze with low cost, stability and reliability, and relatively low requirements for production conditions. Summary of the invention
[0004] In order to solve the above technical problems, the present invention provides an iron-based sky blue glaze and a method for firing it in an oxidizing atmosphere. The present invention successfully fires the sky blue glaze in an oxidizing atmosphere by regulating the formula and firing conditions. Compared with a reducing atmosphere, the present invention has lower requirements on equipment and production conditions, is more reproducible, and has a wide source of raw materials and low cost.
[0005] The specific technical scheme of the present invention is:
[0006] In a first aspect, the present invention provides an iron-based sky blue glaze, which comprises the following mineral raw materials by mass percentage: 10-25% potassium feldspar, 15-30% glass frit, 15-25% calcite, 8-12% wollastonite, 1-8% burned talc, 15-30% quartz powder, and 2-10% iron oxide.
[0007] Since the existing process of preparing sky blue glaze based on reducing atmosphere is relatively complicated, the present invention explores firing sky blue glaze in oxidizing atmosphere. The present invention uses iron as the main coloring component and is prepared in the form of raw glaze. As is known to all, pure ferrous oxide is rarely seen in nature, and most of them exist as a mixture of divalent and trivalent iron. Therefore, the iron in the glaze is Fe 2+ and Fe 3+ They always coexist, but the content of the two valence states of iron ions varies with different conditions. Divalent iron ions make the glaze appear blue or green, while trivalent iron ions make the glaze appear red or brown. Therefore, how to make the iron exist in the glaze in the divalent form in an appropriate amount is one of the key points in preparing the sky blue glaze.
[0008] Furthermore, the present invention has found through research that the decomposition pressure of Fe2O3 reaches 0.1MPa at 1475°C, and even reaches 1MPa at 1575°C. That is to say, even pure Fe2O3 will partially decompose and release oxygen to generate divalent iron under high-temperature calcination. At the same time, the acid-base oxide content in the glaze will also significantly affect the balance between divalent and trivalent iron, among which acidity is more conducive to the presence of divalent iron. In this regard, the present invention utilizes the characteristics of the instability of trivalent iron oxides under high temperature and the influence of the acid-base oxide content of the glaze on its valence balance, and finally successfully obtains a sky blue glaze by adjusting the formula composition and firing conditions.
[0009] Specifically, in terms of formula regulation, the present invention finds that although acidic oxides are conducive to the conversion of iron to divalent, they will also increase the high-temperature viscosity of the glaze, which is not conducive to the decomposition of iron. In addition, the increase in the iron content in the formula will affect the balance of decomposition, and too high an iron content under the same matrix is not conducive to the appearance of a blue effect. Therefore, the present invention finally provides the above formula after a series of optimizations to regulate the content of acidic and alkaline oxides and iron. Through the above formula design, the glaze can have an ideal divalent iron content after firing in an oxidizing atmosphere, so that the glaze surface appears sky blue.
[0010] Preferably, the iron-based sky blue glaze comprises the following mineral raw materials by mass percentage: potassium feldspar 13-17%, glass frit 17-23%, calcite 17-23%, wollastonite 8-12%, burned talc 1.5-2.5%, quartz powder 25-30%, and iron oxide 3-5%.
[0011] Most preferably, the iron-based sky blue glaze comprises the following mineral raw materials by mass percentage: 15% potassium feldspar, 20% glass frit, 20% calcite, 10% wollastonite, 2% burned talc, 29% quartz powder, and 4% iron oxide.
[0012] Preferably, the glass frit comprises the following chemical compositions in mass percentage: SiO2 65-75%, Al2O3 1.5-2.5%, CaO 7.5-8.5%, MgO 3.5-4.5%, K2O 0.2-0.6%, Na2O 10-15%, and Fe2O3 0.1-0.5%.
[0013] Further preferably, the glass frit comprises the following chemical compositions in mass percentage: SiO2 68-72%, Al2O3 1.6-1.8%, CaO 7.8-8.2%, MgO 3.8-4.2%, K2O 0.3-0.5%, Na2O 12.5-13.5%, and Fe2O3 0.2-0.4%.
[0014] Most preferably, the glass frit comprises the following chemical composition in mass percentage: SiO2 70.48%, Al2O3 1.75%, CaO 8.08%, MgO 4.02%, K2O 0.39%, Na2O 13.07%, and Fe2O3 0.29%.
[0015] In a second aspect, the present invention provides an iron-based sky blue glaze, which comprises the following chemical components by mass percentage: SiO2 77-81%, Al2O3 3-5%, CaO 2-4%, MgO 0.5-1.5%, K2O 1.5-3.5%, Na2O 4-6%, and Fe2O3 4-8%.
[0016] Preferably, the iron-based sky blue glaze comprises the following chemical components by mass percentage: SiO2 79%, Al2O3 4%, CaO 3%, MgO 1%, K2O 2%, Na2O 5%, and Fe2O36%.
[0017] In a third aspect, the present invention provides an oxidizing atmosphere firing method for an iron-based sky blue glaze, comprising the following steps:
[0018] (1) Weigh the raw materials according to the ratio;
[0019] (2) wet ball milling the raw materials to obtain glaze slurry;
[0020] (3) Adjust the density and flow rate of the glaze slurry;
[0021] (4) applying glaze slurry to the surface of the body;
[0022] (5) The glazed body is fired in an oxidizing atmosphere to obtain an iron-based sky blue glaze.
[0023] Preferably, in step (2), the particle size of the glaze slurry is D50≤5 μm.
[0024] In addition, the present invention also found that the phase structure in the glaze is also important for obtaining sky blue glaze. If there are a large number of spherical, quasi-spherical and multiple quasi-spherical stacked phase structures in a specific particle size range (about 100nm) in the glaze, the blue tone of the physical color will be presented due to Rayleigh scattering, and the chemical coloring of divalent iron will work together to make the glaze surface obtain a better "sky" deep blue decorative effect. Therefore, the particle size of the glaze slurry is more important for the final firing to form an ideal phase structure. Finally, the present invention found that controlling the glaze slurry particle size within the above range is more conducive to the formation of the target phase structure.
[0025] Preferably, in step (2), the mass ratio of raw material, ball stone and water during wet ball milling is 1:1.8-2.2:0.6-0.8.
[0026] Preferably, in step (4), the glaze slurry is applied to the surface of the body by spraying or pouring glaze. The density of the sprayed glaze slurry is 1.48-1.60 g / cm 3 , flow rate is 5-20s / 100mL; glaze slurry density is 1.70-1.80g / cm 3 , flow rate is 20-35s / 100mL.
[0027] Preferably, in step (5), the sintering process specifically includes: heating to 1300-1340°C at 18-22°C / min, sintering for 18-22 minutes, cooling to 580-620°C at a rate of 23-27°C / min immediately after the insulation, and finally cooling naturally.
[0028] It should be noted that the selection of firing temperature and holding time in the firing conditions is particularly important for the divalent iron content. The present invention finds that if the temperature is too low, it is not conducive to the price reduction of iron ions, and if the temperature is too high, it will damage the glaze quality beyond the firing range of the glaze. In addition, the firing temperature and holding time are also very critical for the phase separation structure of the glaze finished product. If the temperature is improperly controlled, the ideal target phase separation structure of the present invention cannot be obtained. At the same time, the rapid cooling after firing can increase the viscosity of the glaze layer rapidly, thereby preventing the divalent iron from being oxidized during the cooling process.
[0029] Compared with the prior art, the beneficial effects of the present invention are:
[0030] (1) The present invention successfully fired a deep sky blue glaze with a "sky-like" look in an oxidizing atmosphere. Compared with a reducing atmosphere, the present invention has lower requirements on equipment and production conditions, is more reproducible, and has a wide source of raw materials at a low cost.
[0031] (2) The present invention finds a balance between "acidic oxide-divalent iron content-firing temperature" by adjusting the formula and firing conditions, thereby obtaining a sky blue glaze with adjustable blue tone.
[0032] (3) The present invention further combines the physical coloring of a specific phase structure with the chemical coloring of divalent iron. Under the combined effect of the two aspects, the glaze surface can obtain a better "sky" deep blue decorative effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 This is an optical photograph of the iron-based sky blue glaze prepared in Example 1;
[0034] Figure 2 This is the XRD pattern of the iron-based sky blue glaze prepared in Example 1;
[0035] Figure 3 This is a scanning electron microscope image of the iron-based sky blue glaze prepared in Example 1 ((a) low magnification, (b) high magnification). DETAILED DESCRIPTION
[0036] The present invention will be further described below in conjunction with the embodiments.
[0037] Overall embodiment
[0038] An iron-based sky blue glaze comprises the following mineral raw materials by mass percentage: potassium feldspar 10-25%, glass frit 15-30%, calcite 15-25%, wollastonite 8-12%, calcined talc 1-8%, quartz powder 15-30%, and iron oxide 2-10%. The glass frit comprises the following chemical composition by mass percentage: SiO2 65-75%, Al2O3 1.5-2.5%, CaO 7.5-8.5%, MgO 3.5-4.5%, K2O 0.2-0.6%, Na2O 10-15%, and Fe2O3 0.1-0.5%.
[0039] Preferably, the iron-based sky blue glaze comprises the following mineral raw materials by mass percentage: potassium feldspar 13-17%, glass frit 17-23%, calcite 17-23%, wollastonite 8-12%, calcite 1.5-2.5%, quartz powder 25-30%, and iron oxide 3-5%. The glass frit comprises the following chemical composition by mass percentage: SiO2 68-72%, Al2O3 1.6-1.8%, CaO 7.8-8.2%, MgO 3.8-4.2%, K2O 0.3-0.5%, Na2O 12.5-13.5%, and Fe2O3 0.2-0.4%.
[0040] Further preferably, the iron-based sky blue glaze comprises the following mineral raw materials by mass percentage: potassium feldspar 15%, glass frit 20%, calcite 20%, wollastonite 10%, calcite 2%, quartz powder 29%, and iron oxide 4%. The glass frit comprises the following chemical composition by mass percentage: SiO2 70.48%, Al2O3 1.75%, CaO 8.08%, MgO 4.02%, K2O 0.39%, Na2O 13.07%, and Fe2O3 0.29%.
[0041] An iron-based sky blue glaze comprises the following chemical components by mass percentage: SiO2 77-81%, Al2O3 3-5%, CaO 2-4%, MgO 0.5-1.5%, K2O 1.5-3.5%, Na2O4-6%, Fe2O3 4-8%. Preferably, the iron-based sky blue glaze comprises the following chemical components by mass percentage: SiO2 79%, Al2O3 4%, CaO 3%, MgO 1%, K2O 2%, Na2O5%, Fe2O3 6%.
[0042] An oxidizing atmosphere firing method for an iron-based sky blue glaze comprises the following steps:
[0043] (1) Weigh the raw materials according to the ratio.
[0044] (2) The raw materials are wet ball-milled, and the mass ratio of the raw materials, ball stones and water is 1:1.8-2.2:0.6-0.8. After ball milling, a glaze slurry with a particle size of D50≤5μm is obtained.
[0045] (3) Adjust the density and flow rate of the glaze slurry.
[0046] (4) Apply glaze slurry to the surface of the body by spraying or pouring glaze. The density of the sprayed glaze slurry is 1.48-1.60g / cm 3 , flow rate is 5-20s / 100mL; glaze slurry density is 1.70-1.80g / cm 3 , flow rate is 20-35s / 100mL.
[0047] (5) firing the glazed body in an oxidizing atmosphere, wherein the firing process specifically includes: heating to 1300-1340° C. at 18-22° C. / min, firing for 18-22 min, then immediately cooling to 580-620° C. at 23-27° C. / min, and finally cooling naturally to obtain an iron-based sky blue glaze.
[0048] Example 1
[0049] The iron-based sky blue glaze of this embodiment is composed of the following mineral raw materials by weight: 15% potassium feldspar, 20% glass frit, 20% calcite, 10% wollastonite, 2% calcite, 29% quartz powder, and 4% iron oxide. The chemical composition of the glass frit is: SiO270.48%, Al2O31.75%, CaO 8.08%, MgO 4.02%, K2O 0.39%, Na2O 13.07%, and Fe2O30.29%.
[0050] The specific preparation steps are:
[0051] (1) weighing the raw materials according to the above formula, adding water and ball milling (the weight ratio of raw materials to water is 100:45) for 2 hours to obtain a glaze slurry with a particle size D50 = 4.2 μm;
[0052] (2) Add water to adjust the density of the glaze slurry to 1.73 g / cm 3 , flow rate is 24s / 100mL;
[0053] (3) applying glaze slurry to the surface of the blank by pouring glaze;
[0054] (4) The dried glazed body is fired in a shuttle kiln. Firing schedule: heating to 1320°C at 20°C / min, firing for 20 min, then immediately cooling to 600°C at 25°C / min, then cooling naturally.
[0055] The glaze obtained in this case has a deep sky blue glaze similar to the sky, and its L*a*b* are: L*=27.97, a*=1.45, b*=-12.51 respectively.
[0056] Example 2
[0057] The iron-based sky blue glaze of this embodiment is composed of the following mineral raw materials by weight: 12% potassium feldspar, 26% glass frit, 15% calcite, 9% wollastonite, 4% calcined talc, 27% quartz powder, and 7% iron oxide. The chemical composition of the glass frit is the same as that of Embodiment 1.
[0058] The specific preparation steps are:
[0059] (1) weighing the raw materials according to the above formula, adding water and ball milling (the weight ratio of raw materials to water is 100:45) for 2 hours to obtain a glaze slurry with a particle size D50 = 4.5 μm;
[0060] (2) Add water to adjust the density of the glaze slurry to 1.75g / cm 3 , flow rate is 28s / 100mL;
[0061] (3) applying glaze slurry to the surface of the blank by pouring glaze;
[0062] (4) The dried glazed body is fired in a shuttle kiln. Firing schedule: heating to 1320°C at 20°C / min, firing for 20 min, then immediately cooling to 600°C at 25°C / min, then cooling naturally.
[0063] The glaze obtained in this case also has a deep sky blue glaze similar to the sky, and its L*a*b* are: L*=23.72, a*=-4.12, b*=-10.66 respectively.
[0064] Example 3
[0065] The iron-based sky blue glaze of this embodiment is composed of the following mineral raw materials in weight fractions: 15% potassium feldspar, 20% glass frit, 20% calcite, 10% wollastonite, 2% calcite, 29% quartz powder, and 4% iron oxide. The chemical composition of the glass frit is the same as that of Example 1.
[0066] The specific preparation steps are:
[0067] (1) weighing the raw materials according to the above formula, adding water and ball milling (the weight ratio of raw materials to water is 100:45) for 2 hours to obtain a glaze slurry with a particle size D50 = 4.2 μm;
[0068] (2) Add water to adjust the density of the glaze slurry to 1.73 g / cm 3 , flow rate is 24s / 100mL;
[0069] (3) applying glaze slurry to the surface of the blank by pouring glaze;
[0070] (4) The dried glazed body is fired in a shuttle kiln. Firing schedule: heating to 1300°C at 20°C / min, firing for 20 min, then immediately cooling to 600°C at 25°C / min, then cooling naturally.
[0071] The glaze obtained in this case has a deep sky blue glaze similar to the sky, and its L*a*b* are: L*=27.50, a*=5.09, b*=-7.48 respectively.
[0072] Comparative Example 1
[0073] The formula and preparation method of the iron-based glaze of this comparative example refer to those of Example 1, except that the ball milling time in step (1) is controlled to be 20 minutes, thereby obtaining a glaze slurry with a particle size D50 = 15.3 μm.
[0074] The glaze surface obtained in this comparative example has a deep sky blue glaze surface similar to the sky, and L*a*b* are respectively: L*=18.27, a*=3.45, b*=-9.09.
[0075] Comparative Example 2
[0076] The preparation method of the iron-based glaze in this comparative example refers to Example 1, the main difference being that the content of alkali metals and alkaline earth metals in the formula is increased, while the content of quartz is reduced. The specific formula is: 20% potassium feldspar, 25% glass frit (same as Example 1), 15% calcite, 10% wollastonite, 5% burnt talc, 20% quartz powder, and 4% iron oxide.
[0077] The glaze obtained in this comparative example failed to obtain a blue effect, and L*a*b* were respectively: L*=28.15, a*=7.45, b*=-1.18.
[0078] Comparative Example 3
[0079] The preparation method of the iron-based glaze of this comparative example refers to Example 1, the main difference being that the content of iron oxide in the formula is 8%.
[0080] The glaze blue effect obtained in this comparative example is not good, and L*a*b* are respectively: L*=25.11, a*=-5.94, b*=-2.07.
[0081] Comparative Example 4
[0082] The preparation method of the iron-based glaze of this comparative example refers to Example 1, the main difference being that the content of iron oxide is 12%.
[0083] The glaze obtained in this comparative example failed to obtain a blue effect, and L*a*b* were respectively: L*=15.05, a*=-3.25, b*=1.16.
[0084] Comparative Example 5
[0085] The formula and preparation method of the iron-based glaze of this comparative example refer to Example 1, the main difference being that the firing temperature is 1280°C.
[0086] The glaze blue effect obtained in this comparative example is not good, and L*a*b* are respectively: L*=29.55, a*=4.40, b*=-2.36.
[0087] Comparative Example 6
[0088] The preparation method of the iron-based glaze in this comparative example refers to Example 1, the main difference being that the firing temperature is 1340°C.
[0089] The glaze surface obtained in this comparative example was not smooth enough due to over-firing, and the L*a*b* values were: L*=10.12, a*=-3.25, b*=-4.66 respectively.
[0090] Performance comparison
[0091] Table 1. L*a*b* values of examples and comparative examples
[0092]
[0093]
[0094] Table 1 shows the L*a*b* values of various embodiments and comparative examples (in the L*a*b* color model, L* represents brightness; a* represents the range from magenta to green from positive to negative; b* represents the range from yellow to blue from positive to negative). It can be seen from the table that the best formula is embodiment 1, whose blue color is the most obvious and the red tone is not obvious. Figure 1 This is an optical photograph of the glaze surface obtained in Example 1, which has a deep sky blue glaze surface similar to the sky. Figure 2 This is the XRD diagram of the iron-based sky blue glaze prepared in Example 1, showing that the glaze is entirely amorphous. Figure 3 This is a scanning electron microscope image of the iron-based sky blue glaze prepared in Example 1 ((a) low magnification, (b) high magnification); it shows that there are a large number of spherical, quasi-spherical and multiple quasi-spherical phase structures in the glaze. After particle size statistics, it was found that the median diameter was 102.06nm. At this time, the phase structure presents a blue tone of physical color due to Rayleigh scattering, which works together with the chemical coloring of divalent iron to achieve the decorative effect of the deep blue "sky" of the final sample.
[0095] In contrast, when the ball milling time in Comparative Example 1 is short and a glaze with a large particle size is obtained, the large particle size leads to a slow liquid phase formation rate after firing, and the target phase separation structure cannot be formed, resulting in the final blue tone being slightly worse than that in Example 1. In Comparative Example 2, the proportion of alkali metals and alkaline earth metals in the formula is increased. Due to the increase in the alkali content, a large amount of free oxygen exists in the liquid phase at high temperature, which inhibits the conversion of iron to divalent. The increase in iron content and the lower firing in Comparative Examples 3-5 will also inhibit the conversion of iron to divalent. The excessively high firing temperature in Comparative Example 6 exceeds the firing range of the glaze, resulting in poor quality of the glaze layer.
[0096] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0097] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. An iron-based sky blue glaze, Features: The mineral raw materials include the following by mass percentage: potassium feldspar 13-17%, glass frit 17-23%, calcite 17-23%, wollastonite 8-12%, calcined talc 1.5-2.5%, quartz powder 25-30%, iron oxide 3-5%; The glass frit comprises the following chemical compositions in mass percentage: SiO 2 65-75%, Al 2 O 3 1.5-2.5%, CaO7.5-8.5%, MgO 3.5-4.5%, K 2 O 0.2-0.6%, Na 2 O 10-15%, Fe 2 O 3 0.1-0.5%.
2. The iron-based sky blue glaze according to claim 1, Features: The glass frit comprises the following chemical compositions in mass percentage: SiO 2 68-72%, Al 2 O 3 1.6-1.8%, CaO 7.8-8.2%, MgO 3.8-4.2%, K 2 O 0.3-0.5%, Na 2 O 12.5-13.5%, Fe 2 O 3 0.2-0.4%.
3. The iron-based sky blue glaze according to claim 1, Features: The chemical components by mass percentage include: SiO 2 77-81%, Al 2 O 3 3-5%, CaO 2-4%, MgO 0.5-1.5%, K 2 O 1.5-3.5%, Na 2 O 4-6%, Fe 2 O 3 4-8%.
4. A method for firing the iron-based sky blue glaze in an oxidizing atmosphere as claimed in any one of claims 1 to 3, Features The following steps are involved: (1) Weigh the raw materials according to the ratio; (2) wet ball milling the raw materials to obtain glaze slurry; (3) Adjust the density and flow rate of the glaze slurry; (4) Applying glaze slurry to the surface of the green body; (5) The glazed body is fired in an oxidizing atmosphere to obtain an iron-based sky blue glaze.
5. The method according to claim 4, Features: In step (2), the particle size of the glaze slurry is D50≤5 μm.
6. The method according to claim 4, Features: In step (2), the mass ratio of raw material, ball stone and water during wet ball milling is 1:1.8-2.2:0.6-0.
8.
7. The method according to claim 5, Features: In step (4), the glaze slurry is applied to the surface of the blank by spraying or pouring glaze.
8. The method according to claim 7, Features: In step (4), The density of spray glaze is 1.48-1.60 g / cm 3 , flow rate is 5-20 s / 100 mL; The density of the glaze slurry is 1.70-1.80 g / cm 3 , flow rate is 20-35 s / 100 mL.
9. The method according to claim 5, Features: In step (5), the sintering process specifically includes: heating to 1300-1340°C at 18-22°C / min, sintering for 18-22min, cooling to 580-620°C at 23-27°C / min, and finally cooling naturally.
Citation Information
Patent Citations
formula and preparation method of Sky blue transmutation glaze
CN103964900A