A heavy metal capture agent and its preparation method and application

By preparing hemihydrate calcium sulfate whiskers on phosphogypsum and carrying out modification reactions, a heavy metal capture agent containing amino and sulfhydryl groups was formed, which solved the problem of restricted application of phosphogypsum in water treatment, achieved efficient removal of heavy metals, and promoted the promotion of The advancement of phosphogypsum resource utilization and water treatment technology.

CN117813265BActive Publication Date: 2024-11-12GUANGDONG BRUNP RECYCLING TECH CO LTD +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202380011839.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-19
Publication Date
2024-11-12
Estimated Expiration
2043-11-19

AI Technical Summary

Technical Problem

The resource utilization of phosphogypsum has problems such as complex impurities, large storage volume, low added value, immature and unstable technology, and its application in water treatment is limited, due to the solubleness and porosity of the hemihydrate calcium sulfate whiskers. This leads to the inability to effectively remove heavy metal ions.

Method used

Calcium sulfate hemihydrate whiskers are prepared by treating phosphogypsum, and amino and thiol groups are introduced through primary and secondary modification reactions to form a heavy metal capture agent, and thiol compounds are grafted using thiol-alkenyl click chemical reaction. Improve the adsorption performance of capture agents.

Benefits of technology

It has achieved efficient removal of heavy metals such as nickel, cobalt, manganese, etc. in water, expanded the scope of application of phosphogypsum in water treatment, provided new resource utilization ideas, and met the policy requirements of energy conservation, emission reduction, and low-carbon and environmental protection.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The present disclosure provides a heavy metal capture agent and a preparation method and application thereof, belonging to the field of water treatment technology. The present disclosure first prepares phosphogypsum into hemihydrate calcium sulfate whiskers, grafts silane amino groups on the hydroxyl groups of the hemihydrate calcium sulfate whiskers through primary modification, then introduces double bonds through secondary modification, and then grafts thiol compounds through thiol-ene click chemistry reaction to obtain a heavy metal capture agent, which contains hydroxyl groups, amino groups and thiol groups at the same time, so that the heavy metal capture agent can adsorb heavy metals in heavy metal wastewater through physical and chemical adsorption to achieve the purpose of removing heavy metals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of water treatment, and in particular to a heavy metal scavenger and a preparation method and application thereof. Background Art

[0002] As a by-product in the production process of wet phosphoric acid, phosphogypsum produces about 4-5 tons of phosphogypsum for every ton of phosphoric acid produced. Among them, the main hazards to the environment are phosphides and fluorides with strong acidity. my country's "three phosphorus" (phosphate mines, phosphorus chemicals, and phosphogypsum depots) are densely distributed in the middle and upper reaches of the Yangtze River, and many phosphogypsum depots are distributed along the river, which is an important reason for the excessive total phosphorus in the Yangtze River Basin. According to data from the China Phosphate and Compound Fertilizer Industry Association, the production of phosphogypsum in 2022 was 77 million tons, and the comprehensive utilization of phosphogypsum in 2022 was 38.8 million tons. Although it reached 50%, nearly 50% of the phosphogypsum is still not utilized.

[0003] The main problems with the resource utilization of phosphogypsum are complex impurities, large storage volume, low added value, immature and unstable technology, etc. In the main markets for the comprehensive utilization of phosphogypsum, the products are highly homogeneous, highly competitive, and have low added value, and it is also very difficult to open up the market. At the same time, since phosphogypsum is a by-product of the chemical industry, people still have some misunderstandings and distrust of phosphogypsum products. In terms of storage, the design of the phosphogypsum warehouse has a certain lifespan, and the inventory of phosphogypsum is high, resulting in some phosphogypsum being stored for a long time and corroding the yard, causing varying degrees of pollution to groundwater, rivers, soil, etc. The investment in the production of gypsum comprehensive utilization products is large, the start-up rate is low, and most of them are in a loss-making state. Therefore, there is a serious conflict between the "quality" and "quantity" of comprehensive utilization of phosphogypsum.

[0004] At present, the resource utilization products based on phosphogypsum in the market are mainly in the construction, agricultural and chemical industries, among which the consumption of phosphogypsum in construction materials accounts for the vast majority, and there are mature processes that can make phosphogypsum into gypsum powder that meets the standards of "Building Gypsum". However, affected by the real estate market, cost competition and traffic radius, the market for building gypsum is currently saturated, so it is necessary to actively seek other technical methods for the consumption of phosphogypsum.

[0005] The main component of phosphogypsum is calcium sulfate, which can be obtained by removing impurities, roasting, and atmospheric pressure acidification to obtain hemihydrate calcium sulfate whiskers. Hemihydrate calcium sulfate whiskers are used as water treatment agents. On the one hand, hemihydrate calcium sulfate whiskers are easily soluble in water, which increases the concentration of calcium ions in water and introduces new impurities. On the other hand, the pores between calcium sulfate whiskers are large and their affinity with heavy metal ions is poor, which limits the application of hemihydrate calcium sulfate whiskers in water treatment. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and provide a heavy metal scavenger and a preparation method and application thereof. The heavy metal scavenger is used in water treatment to remove nickel, cobalt and manganese heavy metal ions in water.

[0007] To achieve the above objectives, the technical solution adopted by the present disclosure is as follows: In a first aspect, a method for preparing a heavy metal scavenger is provided, comprising the following steps:

[0008] Preparation of calcium sulfate hemihydrate whiskers: treating phosphogypsum with hydrochloric acid and then aging to obtain calcium sulfate hemihydrate whiskers;

[0009] Preparation of a primary modified product: after evenly mixing calcium sulfate hemihydrate whiskers and a first alcohol solvent, adjusting the pH of the solution to 2-5 to obtain a first solution; after evenly mixing γ-aminopropyltriethoxysilane and a second alcohol solvent, adjusting the pH of the solution to 2-5 to obtain a second solution; dropping the first solution into the second solution for reaction to obtain a primary modified product;

[0010] Prepare a secondary modified product; after uniformly mixing maleimide and a polar solvent, adjust the pH of the solution to 7-7.5 to obtain a third solution; add the primary modified product to the third solution for reaction to obtain a secondary modified product;

[0011] Preparation of heavy metal scavenger: after uniformly dispersing a mixture of a secondary modified substance, a photoinitiator, a thiol compound, and a third alcohol solvent, performing a photocuring reaction to obtain a heavy metal scavenger;

[0012] Wherein, the thiol compound is at least one of trimethylolpropane-3-mercaptopropionate, 3-mercaptopropionic acid ethyl ester, and 3-mercapto-1-propanol; the mass ratio of the secondary modified product to the thiol modified product is (1:0.65)-(1:0.85).

[0013] In one embodiment, the mass ratio of the secondary modified product to the mercapto modified product is (1:0.7)-(1:0.85).

[0014] In one embodiment, the mass ratio of the calcium sulfate hemihydrate whiskers to γ-aminopropyltriethoxysilane is (0.75:1)-(1.1:1).

[0015] In one embodiment, the mass ratio of the maleimide to the primary modified product is (0.6:1)-(1.2:1).

[0016] In one embodiment, the mass ratio of the secondary modified product to the photoinitiator is (50:1)-(60:1).

[0017] In one embodiment, the pH of the first solution and the second solution are each independently selected from 2.5-5.

[0018] In one embodiment, the specific surface area of ​​the calcium sulfate hemihydrate whiskers is 40-130 m 2 / g, aspect ratio is 80-110.

[0019] In one embodiment, in the preparation of the primary modified product, the reaction temperature is 20-40° C. and the reaction time is 0.5-3 h.

[0020] In one embodiment, in the preparation of the secondary modified product, the reaction time is 10-12 hours.

[0021] In one embodiment, in the preparation of the heavy metal capture agent, ultrasonic oscillation is used for dispersion, and the time of ultrasonic oscillation is 10-30 minutes.

[0022] In one embodiment, the solid-to-liquid ratio of the phosphogypsum and hydrochloric acid is 0.1-0.2 g / mL; and / or the treatment temperature is 110-130° C., and the treatment time is 10-30 min; and / or the mass fraction of the hydrochloric acid is 21%-98%; and / or the aging time is 5-8 h.

[0023] In one embodiment, the alcohol solvent is at least one of ethanol, methanol, propanol and n-butanol.

[0024] In one embodiment, the polar solvent is at least one of dimethyl sulfoxide, N,N'-dimethylformamide, and N,N'-dimethylacetamide.

[0025] In one embodiment, the photoinitiator is benzoin and its derivatives.

[0026] In a second aspect, a heavy metal capture agent is provided, wherein the heavy metal capture agent is prepared by the above-mentioned preparation method of the heavy metal capture agent.

[0027] In one embodiment, the grafting rate of the thiol compound in the heavy metal scavenger is 19-55%.

[0028] In a third aspect, the invention provides application of the heavy metal scavenger in water treatment.

[0029] Compared with the prior art, the present invention has the following beneficial effects:

[0030] (1) In the present disclosure, phosphogypsum is first prepared into hemihydrate calcium sulfate whiskers, which have a needle-like structure. A silane amino group is grafted onto the hydroxyl group of the hemihydrate calcium sulfate whiskers through a primary modification to introduce an amino group. A double bond is then introduced through a secondary modification. Next, a thiol compound is grafted using a thiol-ene click chemistry reaction to introduce a thiol group. A heavy metal scavenger is obtained, which contains hydroxyl groups, amino groups and thiol groups at the same time. The amino group can form a chelate with some heavy metals. On the one hand, the thiol group can reduce the hydrophobicity of the heavy metal scavenger, and on the other hand, the thiol group can form a chelate with heavy metal ions. In addition, after the hemihydrate calcium sulfate whiskers are modified three times, the porosity of the hemihydrate calcium sulfate whiskers is reduced. The above multiple aspects work together to enable the heavy metal scavenger to adsorb heavy metals in heavy metal wastewater through physical and chemical adsorption, thereby achieving the purpose of removing heavy metals.

[0031] (2) The heavy metal capture agent obtained after modification of phosphogypsum is applied to the treatment of heavy metal wastewater, which provides new ideas for the resource utilization of phosphogypsum and achieves waste treatment with waste, responds to the policy call of "zero-waste city" and achieves energy conservation, emission reduction, low carbon and environmental protection. DETAILED DESCRIPTION

[0032] In order to better illustrate the purpose, technical scheme and advantages of the present disclosure, the present disclosure will be further described below in conjunction with specific embodiments and comparative examples, the purpose of which is to understand the content of the present disclosure in detail, rather than to limit the present disclosure. All other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present disclosure. The experimental reagents and instruments involved in the implementation of the present disclosure are all commonly used ordinary reagents and instruments unless otherwise specified.

[0033] To achieve the above objectives, the technical solution adopted by the present disclosure is as follows: In a first aspect, a method for preparing a heavy metal scavenger is provided, comprising the following steps:

[0034] Preparation of calcium sulfate hemihydrate whiskers: treating phosphogypsum with hydrochloric acid and then aging to obtain calcium sulfate hemihydrate whiskers;

[0035] Preparation of a primary modified product: after evenly mixing calcium sulfate hemihydrate whiskers and a first alcohol solvent, adjusting the pH of the solution to 2-5 to obtain a first solution; after evenly mixing γ-aminopropyltriethoxysilane and a second alcohol solvent, adjusting the pH of the solution to 2-5 to obtain a second solution; dropping the first solution into the second solution for reaction to obtain a primary modified product;

[0036] Prepare a secondary modified product; after uniformly mixing maleimide and a polar solvent, adjust the pH of the solution to 8-9 to obtain a third solution; add the primary modified product to the third solution for reaction to obtain a secondary modified product;

[0037] Preparation of heavy metal scavenger: after uniformly dispersing a mixture of a secondary modified substance, a photoinitiator, a thiol compound, and a third alcohol solvent, performing a photocuring reaction to obtain a heavy metal scavenger;

[0038] Wherein, the thiol compound is at least one of trimethylolpropane-3-mercaptopropionate, 3-mercaptopropionic acid ethyl ester, and 3-mercapto-1-propanol; the mass ratio of the secondary modified product to the thiol modified product is (1:0.65)-(1:0.85).

[0039] In the present invention, phosphogypsum is first prepared into calcium sulfate hemihydrate whiskers, which are needle-shaped structures. A silane amino group is grafted onto the hydroxyl group of the calcium sulfate hemihydrate whiskers through a primary modification to introduce an amino group. A double bond is then introduced through a secondary modification. Next, a thiol compound is grafted through a thiol-ene click chemistry reaction to introduce a thiol group. A heavy metal capture agent is obtained, which contains hydroxyl groups, amino groups and thiol groups at the same time. The amino group can form a chelate with part of the heavy metals. On the one hand, the thiol group can reduce the hydrophobicity of the heavy metal capture agent, and on the other hand, the thiol group can form a chelate with the heavy metal ions. In addition, after the calcium sulfate hemihydrate whiskers are modified three times, the porosity of the calcium sulfate hemihydrate whiskers is reduced. The above multiple aspects work together to enable the heavy metal capture agent to adsorb heavy metals in heavy metal wastewater through physical and chemical adsorption, thereby achieving the purpose of removing heavy metals.

[0040] In the present disclosure, the mass ratio of the secondary modified substance to the thiol modified substance is (1:0.65)-(1:0.85), for example, it can be 1:0.65, 1:0.68, 1:0.70, 1:0.72, 1:0.75, 1:0.77, 1:0.80, 1:0.83, 1:0.85 or a range consisting of any two of them, but is not limited to the listed values, and other values ​​not listed within the numerical range are also applicable; the mass ratio of the secondary modified substance to the thiol modified substance is (1:0.65)-(1:0.85), for example, it can be 1:0.65, 1:0.68, 1:0.70, 1:0.72, 1:0.75, 1:0.77, 1:0.80, 1:0.83, 1:0.85 or a range consisting of any two of them. The mass ratio of the secondary modifier and the thiol modifier affects the grafting rate of the heavy metal scavenger. When the mass ratio of the secondary modifier and the thiol modifier is less than 1:0.65, it will affect the reaction conversion rate. When the mass ratio of the secondary modifier and the thiol modifier is greater than 1:0.85, it will affect the hydrophobicity. The inventors found that when the mass ratio of the secondary modifier and the thiol modifier is (1:0.65)-(1:0.85), heavy metal scavengers with different grafting rates of thiol compounds can be obtained, thereby improving the effect of the heavy metal scavenger in removing heavy metals.

[0041] In the present disclosure, the mass ratio of the calcium sulfate hemihydrate whisker to γ-aminopropyltriethoxysilane (KH550) is 0.75:1-1.1:1, for example, it can be 0.75:1, 0.78:1, 0.80:1, 0.85:1, 0.90:1, 0.95:1, 1.00:1, 1.05:1, 1.1:1 or a range consisting of any two of them, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable; when the mass ratio of the calcium sulfate hemihydrate whisker to γ-aminopropyltriethoxysilane is less than 0.75:1, the coupling effect of the coupling agent will be affected; when the mass ratio of the calcium sulfate hemihydrate whisker to γ-aminopropyltriethoxysilane is greater than 1.1:1, the degree of modification will be affected.

[0042] In the present disclosure, the mass ratio of the maleimide to the primary modified product is 0.6:1-1.2:1, for example, it can be 0.6:1, 0.65:1, 0.7:1, 0.75:1, 0.8:1, 0.85:1, 0.9:1, 0.95:1, 1:1, 1.05:1, 1.1:1, 1.15:1, 1.2:1 or a range consisting of any two of them, but is not limited to the listed values, and other values ​​not listed in the numerical range are also applicable; the mass ratio of the maleimide to the primary modified product is 0.6:1-1.2:1, for example, it can be 0.6:1, 0.65:1, 0.7:1, 0.75:1, 0.8:1, 0.85:1, 0.9:1, 0.95:1, 1:1, 1.05:1, 1.1:1, 1.15:1, 1.2:1 or a range consisting of any two of them. The reaction of maleimide and the primary modifier must be carried out under neutral conditions. If maleimide and the primary modifier are under alkaline conditions, the maleimide will be hydrolyzed, resulting in the inability of the secondary modifier to react with the thiol compound. Under neutral conditions, the mass ratio of maleimide and the primary modifier is another factor affecting the secondary modification. If the mass ratio of maleimide and the primary modifier is greater than 1.2:1 or less than 0.6:1, the modification effect of maleimide will be reduced, and thus the removal rate of heavy metals by the heavy metal scavenger will decrease.

[0043] In the present disclosure, the mass ratio of the secondary modifier to the photoinitiator is 50:1-60:1, for example, it can be 50:1, 51:1, 52:1, 53:1, 54:1, 55:1, 56:1, 57:1, 58:1, 59:1, 60:1 or a range consisting of any two of them, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0044] In the process of preparing heavy metal scavengers, the dosage of secondary modifiers, photoinitiators, and thiol compounds is a factor affecting the grafting rate of thiol compounds. The present invention obtains heavy metal scavengers with different grafting rates by adjusting the dosage of secondary modifiers, photoinitiators, and thiol compounds.

[0045] In the present disclosure, the pH of the first solution and the second solution are each independently selected from 2.5-5, for example, it can be 2.5, 2.6, 2.7, 2.8, 2.9, 3.0, 3.1, 3.2, 3.3, 3.4, 3.5, 4.0, 4.5, 5.0 or a range consisting of any two of them, but is not limited to the listed values, and other unlisted values ​​within the numerical range are also applicable.

[0046] Calcium sulfate hemihydrate whiskers and γ-aminopropyltriethoxysilane can only react under acidic conditions. If the pH of the first solution and the second solution is alkaline, the calcium sulfate hemihydrate whiskers and γ-aminopropyltriethoxysilane cannot react. The inventors found that when the pH of the first solution and the second solution is the same and the pH is in the range of 2.5-3.5, the calcium sulfate hemihydrate whiskers and γ-aminopropyltriethoxysilane can fully react, providing a good foundation for subsequent secondary modification.

[0047] In the present disclosure, the specific surface area of ​​the calcium sulfate hemihydrate whisker is 40-130m 2 / g, and the aspect ratio is 80-110; for example, the specific surface area of ​​hemihydrate calcium sulfate whiskers can be 40m 2 / g, 45m 2 / g, 50m 2 / g, 55m 2 / g, 60m 2 / g, 65m 2 / g, 70m 2 / g, 75m 2 / g, 80m 2 / g, 85m 2 / g, 90m 2 / g, 95m 2 / g、100m 2 / g、105m 2 / g, 110m 2 / g, 115m 2 / g, 120m 2 / g, 125m 2 / g, 130m 2 / g, but not limited to this; the aspect ratio of the calcium sulfate hemihydrate whisker can be 80, 82, 84, 85, 87, 89, 90, 91, 93, 95, 96, 98, 100, 102, 104, 106, 108, 110, but not limited to this.

[0048] The specific surface area and aspect ratio of calcium sulfate hemihydrate whiskers will affect the removal effect of heavy metals by heavy metal capture agents. The inventors found that the specific surface area of ​​calcium sulfate hemihydrate whiskers is 40-130m 2 / g, and the aspect ratio is 80-110, which can increase the effect of heavy metal capture agent in removing heavy metals.

[0049] In the present disclosure, in the preparation of the primary modified product, the reaction temperature is 20-40°C, and the reaction time is 0.5-3h; specifically, the reaction temperature can be 20°C, 23°C, 25°C, 28°C, 30°C, 32°C, 35°C, 37°C, 40°C, but not limited to this; the reaction time can be 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, but not limited to this.

[0050] In the present disclosure, in the preparation of the secondary modified product, the reaction time is 10-12 hours; within the above reaction time range, a secondary modified product with good secondary modification effect can be obtained.

[0051] In the present disclosure, the specific steps for preparing the heavy metal capture agent are as follows:

[0052] Add the photoinitiator and the mercapto compound to the third alcohol solvent, perform ultrasonic oscillation for 3-5 minutes, then add the secondary modifier, perform ultrasonic oscillation for 10-15 minutes; the obtained solution is subjected to photocuring reaction, and the reaction product is dried, washed and filtered to obtain a heavy metal scavenger.

[0053] Firstly subjecting the photoinitiator and the mercapto compound to ultrasonic oscillation and then adding the secondary modifier to ultrasonic oscillate can avoid the secondary modifier or the mercapto compound from agglomerating and affecting the photocuring reaction.

[0054] In the present disclosure, the solid-liquid ratio of phosphogypsum and hydrochloric acid is 0.1-0.2 g / mL; and / or, the treatment temperature is 110-130°C, and the treatment time is 10-30 min; and / or, the mass fraction of hydrochloric acid is 21%-98%; and / or, the aging time is 5-8 h; by adjusting the solid-liquid ratio of phosphogypsum and hydrochloric acid, the treatment temperature, time, the mass fraction of hydrochloric acid and the aging time, a specific surface area of ​​40-120 m 2 / g, hemihydrate calcium sulfate whiskers with an aspect ratio of 80-100.

[0055] In addition, in the present disclosure, before treating the phosphogypsum with hydrochloric acid, the phosphogypsum may be pretreated, and the pretreatment step includes water washing or flotation, and the pretreatment can remove soluble impurities and organic matter in the phosphogypsum.

[0056] In the present disclosure, the first alcohol solvent, the second alcohol solvent, and the third alcohol solvent are each independently selected from at least one of ethanol, methanol, propanol, and n-butanol. In the process of preparing the first solution, calcium sulfate hemihydrate whiskers are easily soluble in water, so the first alcohol solvent is selected as an anhydrous alcohol solvent, such as anhydrous ethanol and anhydrous methanol; in the process of preparing the second solution, the aqueous solution of the second alcohol solvent can promote the reaction of γ-aminopropyltriethoxysilane and calcium sulfate hemihydrate whiskers; wherein, the inventors found that when the volume ratio of the second alcohol solvent to water is 2-4, the reaction of silane γ-aminopropyltriethoxysilane and calcium sulfate hemihydrate whiskers can be effectively improved.

[0057] In the present disclosure, the polar solvent is at least one of dimethyl sulfoxide, N,N'-dimethylformamide, and N,N'-dimethylacetamide.

[0058] In the present disclosure, the photoinitiator is benzoin and its derivatives, such as benzoin, benzoin dimethyl ether, benzoin ethyl ether, benzoin isopropyl ether, and benzoin butyl ether. In the present disclosure, benzoin dimethyl ether (BDK) is selected as the photoinitiator.

[0059] In a second aspect, a heavy metal capture agent is provided, wherein the heavy metal capture agent is prepared by the above-mentioned preparation method of the heavy metal capture agent.

[0060] In the present disclosure, the grafting rate of the thiol compound in the heavy metal capture agent is 19%-55%. For example, the grafting rate of the thiol compound in the heavy metal capture agent can be but is not limited to 19%, 20%, 21%, 22%, 23%, 24%, 25%, 26%, 27%, 28%, 29%, 30%, 31%, 32%, 33%, 34%, 35%, 36%, 37%, 38%, 39%, 40%, 41%, 42%, 43%, 44%, 45%, 46%, 47%, 48%, 49%, 50%, 51%, 52%, 53%, 54%, 55%. The inventors found that when the grafting rate of the thiol compound in the heavy metal capture agent is less than 19% or greater than 55%, the effect of the heavy metal capture agent in removing heavy metals will decrease. When the grafting rate of the thiol compound in the heavy metal capture agent is 25-40%, the removal rate of the heavy metal capture agent for heavy metals can be improved.

[0061] In a third aspect, the invention provides application of the heavy metal scavenger in water treatment.

[0062] The heavy metal capture agent disclosed in the present invention can remove heavy metals such as nickel, cobalt, and manganese in wastewater, thereby expanding the application scope of phosphogypsum in water treatment.

[0063] Example 1

[0064] This embodiment provides a method for preparing a heavy metal capture agent, comprising the following steps:

[0065] Preparation of calcium sulfate hemihydrate whiskers:

[0066] 500 g of phosphogypsum was pulped, the black oil film was scraped off by a laboratory simulated oil scraper, and then put into a laboratory simulated three-stage countercurrent washing device for impurity removal. After impurity removal, the sample was filtered and dried to obtain phosphogypsum that met the "Building Gypsum" standard, which was the pretreated phosphogypsum;

[0067] 21% hydrochloric acid and 98% hydrochloric acid were placed in a water bath at a volume ratio of 20:1 and stirred evenly. After heating to 120°C, 10g of pretreated phosphogypsum was added and reacted for 15 minutes. The obtained product was filtered while hot. After the filtrate was aged for 6 hours, the obtained product was washed, filtered and dried to obtain hemihydrate calcium sulfate whiskers. The specific surface area of ​​the hemihydrate calcium sulfate whiskers was 60m 2 / g, aspect ratio is 90.

[0068] Preparation of primary modification:

[0069] 2 g of calcium sulfate hemihydrate whiskers were added to 200 mL of anhydrous ethanol, and then stirred at 200 rpm for 50 min to dissolve, and dilute sulfuric acid was added to make the pH of the solution = 3 to obtain a first solution;

[0070] 2.5 g KH550 was added to 50 mL ethanol aqueous solution, stirred at 200 rpm for 20 min to dissolve, and then dilute sulfuric acid was added to adjust the pH of the solution to 3 to obtain a second solution, wherein the volume ratio of ethanol to water in the ethanol aqueous solution was 2:1;

[0071] Under the conditions of a rotation speed of 200 rpm and a temperature of 30° C., the second solution was added dropwise to the first solution and reacted for 1 hour. After the obtained product was dried, a primary modified product was obtained.

[0072] Preparation of secondary modified product: Add 2g of maleimide to N,N'-dimethylformamide, stir to dissolve, add 2% sodium hydroxide solution to make the pH of the solution 7.2 to obtain a third solution; add 2g of primary modified product to the third solution, react at room temperature for 11h, and dry the obtained product to obtain a secondary modified product.

[0073] Preparation of heavy metal capture agent: 0.04g BDK was added to 50mL methanol solution, stirred evenly, then 1.5g trimethylolpropane-3-mercaptopropionate was added, ultrasonic oscillation was performed for 5min, and then 2g secondary modified product was added, ultrasonic oscillation was performed for 15min, the obtained solution was smeared on a surface dish, irradiated with ultraviolet light for 5min and then dried, the obtained product was washed with ethanol solution and filtered, and the obtained filter material was the heavy metal capture agent; the grafting rate of the thiol compound in the heavy metal capture agent was 53%.

[0074] Example 2

[0075] This embodiment provides a method for preparing a heavy metal capture agent, comprising the following steps:

[0076] Preparation of calcium sulfate hemihydrate whiskers:

[0077] 500 g of phosphogypsum was pulped, the black oil film was scraped off by a laboratory simulated oil scraper, and then put into a laboratory simulated three-stage countercurrent washing device for impurity removal. After impurity removal, the sample was filtered and dried to obtain phosphogypsum that met the "Building Gypsum" standard, which was the pretreated phosphogypsum;

[0078] 21% hydrochloric acid and 98% hydrochloric acid were placed in a water bath at a volume ratio of 20:1 and stirred evenly. After heating to 120°C, 10g of pretreated phosphogypsum was added and reacted for 15 minutes. The obtained product was filtered while hot. After the filtrate was aged for 6 hours, the obtained product was washed, filtered and dried to obtain hemihydrate calcium sulfate whiskers. The specific surface area of ​​the hemihydrate calcium sulfate whiskers was 60m 2 / g, aspect ratio is 90.

[0079] Preparation of primary modification:

[0080] 2 g of calcium sulfate hemihydrate whiskers were added to 200 mL of anhydrous ethanol, and then stirred at 200 rpm for 50 min to dissolve, and dilute sulfuric acid was added to make the pH of the solution = 3 to obtain a first solution;

[0081] 1.8 g KH550 was added to 50 mL ethanol aqueous solution, stirred at 200 rpm for 20 min to dissolve, and then dilute sulfuric acid was added to adjust the pH of the solution to 3 to obtain a second solution, wherein the volume ratio of ethanol to water in the ethanol aqueous solution was 2:1;

[0082] Under the conditions of a rotation speed of 200 rpm and a temperature of 30° C., the second solution was added dropwise to the first solution and reacted for 1 hour. After the obtained product was dried, a primary modified product was obtained.

[0083] Preparation of secondary modified product: Add 1.6g of maleimide to N,N'-dimethylformamide, stir to dissolve, add 2% sodium hydroxide solution to make the pH of the solution 7.5, and obtain a third solution; add 2g of primary modified product to the third solution, react at room temperature for 11h, and dry the obtained product to obtain a secondary modified product.

[0084] Preparation of heavy metal capture agent: add 0.04g BDK to 50mL methanol solution, stir evenly, add 1.7g ethyl 3-mercaptopropionate, ultrasonically oscillate for 5min, then add 2g secondary modifier, ultrasonically oscillate for 15min, apply the obtained solution on a surface dish, irradiate with ultraviolet light for 5min and then dry, wash the obtained product with ethanol solution and filter, the obtained filter material is the heavy metal capture agent; the grafting rate of thiol compounds in the heavy metal capture agent is 31%.

[0085] Example 3

[0086] This embodiment provides a method for preparing a heavy metal capture agent, comprising the following steps:

[0087] Preparation of calcium sulfate hemihydrate whiskers:

[0088] 500 g of phosphogypsum was pulped, the black oil film was scraped off by a laboratory simulated oil scraper, and then put into a laboratory simulated three-stage countercurrent washing device for impurity removal. After impurity removal, the sample was filtered and dried to obtain phosphogypsum that met the "Building Gypsum" standard, which was the pretreated phosphogypsum;

[0089] 21% hydrochloric acid and 98% hydrochloric acid were placed in a water bath at a volume ratio of 20:1 and stirred evenly. After heating to 120°C, 10g of pretreated phosphogypsum was added and reacted for 15 minutes. The obtained product was filtered while hot. After the filtrate was aged for 6 hours, the obtained product was washed, filtered and dried to obtain hemihydrate calcium sulfate whiskers. The specific surface area of ​​the hemihydrate calcium sulfate whiskers was 60m 2 / g, aspect ratio is 90.

[0090] Preparation of primary modification:

[0091] 2 g of calcium sulfate hemihydrate whiskers were added to 200 mL of anhydrous ethanol, and then stirred at 200 rpm for 50 min to dissolve, and dilute sulfuric acid was added to make the pH of the solution = 3 to obtain a first solution;

[0092] 2.6 g KH550 was added to 50 mL ethanol aqueous solution, stirred at 200 rpm for 20 min to dissolve, and then dilute sulfuric acid was added to adjust the pH of the solution to 3 to obtain a second solution, wherein the volume ratio of ethanol to water in the ethanol aqueous solution was 2:1;

[0093] Under the conditions of a rotation speed of 200 rpm and a temperature of 30° C., the second solution was added dropwise to the first solution and reacted for 1 hour. After the obtained product was dried, a primary modified product was obtained.

[0094] Preparation of secondary modified product: Add 1.2g maleimide to N,N'-dimethylformamide, stir to dissolve, add 2% sodium hydroxide solution to make the pH of the solution 7, and obtain a third solution; add 2g primary modified product to the third solution, react at room temperature for 11h, and obtain a secondary modified product after drying the obtained product.

[0095] Preparation of heavy metal capture agent: add 0.04g BDK to 50mL methanol solution, stir evenly, add 1.3g 3-mercapto-1-propanol, ultrasonically oscillate for 5min, then add 2g secondary modified product, ultrasonically oscillate for 15min, apply the obtained solution on a surface dish, irradiate with ultraviolet light for 5min and then dry, wash the obtained product with ethanol solution and filter, the obtained filter material is the heavy metal capture agent; the grafting rate of thiol compounds in the heavy metal capture agent is 19%.

[0096] Example 4

[0097] The present embodiment provides a method for preparing a heavy metal capture agent, which differs from the embodiment 1 only in that the steps for preparing the heavy metal catalyst are different. The steps for preparing the heavy metal catalyst in the present embodiment are as follows: 0.04 g of BDK is added to 50 mL of methanol solution, stirred evenly, 1.6 g of trimethylolpropane-3-mercaptopropionate is added, ultrasonically vibrated for 5 min, and then 2 g of a secondary modified substance is added, ultrasonically vibrated for 15 min, the resulting solution is smeared on a surface dish, irradiated with ultraviolet light for 5 min and then dried, the resulting product is washed with an ethanol solution and filtered, and the resulting filter material is the heavy metal capture agent; the grafting rate of the thiol compound in the heavy metal capture agent is 40%

[0098] Example 5

[0099] The present embodiment provides a method for preparing a heavy metal capture agent, which differs from the embodiment 1 only in that the steps for preparing the heavy metal catalyst are different. The steps for preparing the heavy metal catalyst in the present embodiment are as follows: adding 0.04 g BDK to 50 mL methanol solution, stirring evenly, adding 1.7 g trimethylolpropane-3-mercaptopropionate, ultrasonically oscillating for 5 min, then adding 2 g of a secondary modified substance, ultrasonically oscillating for 15 min, applying the obtained solution on a surface dish, irradiating with ultraviolet light for 5 min and then drying, washing the obtained product with an ethanol solution and filtering, and the obtained filter material is the heavy metal capture agent; the grafting rate of the thiol compound in the heavy metal capture agent is 31%.

[0100] Example 6

[0101] The present embodiment provides a method for preparing a heavy metal capture agent, which differs from the embodiment 1 only in that the steps for preparing the heavy metal catalyst are different. The steps for preparing the heavy metal catalyst in the present embodiment are as follows: adding 0.04 g of BDK to 50 mL of methanol solution, stirring evenly, adding 1.4 g of trimethylolpropane-3-mercaptopropionate, ultrasonically oscillating for 5 minutes, then adding 2 g of a secondary modified substance, ultrasonically oscillating for 15 minutes, applying the resulting solution on a surface dish, irradiating with ultraviolet light for 5 minutes and then drying, washing the resulting product with an ethanol solution and filtering, and the resulting filter material is the heavy metal capture agent; the grafting rate of the thiol compound in the heavy metal capture agent is 19%.

[0102] Example 7

[0103] The present embodiment provides a method for preparing a heavy metal capture agent, which differs from the embodiment 1 only in that the steps for preparing the heavy metal catalyst are different. The steps for preparing the heavy metal catalyst in the present embodiment are as follows: 0.04 g of BDK is added to 50 mL of methanol solution, stirred evenly, 1.35 g of trimethylolpropane-3-mercaptopropionate is added, ultrasonically oscillated for 5 min, and then 2 g of a secondary modified substance is added, ultrasonically oscillated for 15 min, the resulting solution is smeared on a surface dish, irradiated with ultraviolet light for 5 min and then dried, the resulting product is washed with an ethanol solution and filtered, and the resulting filter material is the heavy metal capture agent; the grafting rate of the thiol compound in the heavy metal capture agent is 15%.

[0104] Example 8

[0105] This embodiment provides a method for preparing a heavy metal capture agent, which is different from Embodiment 1 only in that the pH of the first solution and the second solution are different. In this embodiment, the pH of the first solution is 3.5, and the pH of the second solution is 3.5.

[0106] Example 9

[0107] This embodiment provides a method for preparing a heavy metal capture agent, which differs from Embodiment 1 only in that the pH values ​​of the first solution and the second solution are different. In this embodiment, the pH value of the first solution is 2.5, and the pH value of the second solution is 2.5.

[0108] Example 10

[0109] This embodiment provides a method for preparing a heavy metal capture agent, which differs from Embodiment 1 only in that the pH values ​​of the first solution and the second solution are different. In this embodiment, the pH value of the first solution is 5, and the pH value of the second solution is 5.

[0110] Embodiment 11

[0111] This embodiment provides a method for preparing a heavy metal capture agent, which differs from Embodiment 1 only in that the pH values ​​of the first solution and the second solution are different. In this embodiment, the pH value of the first solution is 2, and the pH value of the second solution is 2.

[0112] Example 12

[0113] This embodiment provides a method for preparing a heavy metal scavenger. The difference between this embodiment and embodiment 1 is that the aging time in the preparation of calcium sulfate hemihydrate whiskers is different. The aging time in this embodiment is 5 hours, and the specific surface area of ​​the calcium sulfate hemihydrate whiskers is 40m 2 / g, aspect ratio is 80.

[0114] Embodiment 13

[0115] This embodiment provides a method for preparing a heavy metal scavenger. The difference between this embodiment and embodiment 1 is that the aging time in the preparation of calcium sulfate hemihydrate whiskers is different. The aging time in this embodiment is 5 hours, and the specific surface area of ​​the calcium sulfate hemihydrate whiskers is 120 m 2 / g, and the aspect ratio is 100.

[0116] Embodiment 14

[0117] This embodiment provides a method for preparing a heavy metal scavenger. The difference between this embodiment and embodiment 1 is that the aging time in the preparation of calcium sulfate hemihydrate whiskers is different. The aging time in this embodiment is 5 hours, and the specific surface area of ​​the calcium sulfate hemihydrate whiskers is 130 m 2 / g, and the aspect ratio is 110.

[0118] Comparative Example 1

[0119] This comparative example provides a method for preparing a heavy metal scavenger, which differs from Example 1 only in that 3-mercaptopropionic acid is used to replace trimethylolpropane-3-mercaptopropionate, and the grafting rate of the mercapto compound in the obtained heavy metal scavenger is 31%.

[0120] Comparative Example 2

[0121] This comparative example provides a method for preparing a heavy metal scavenger, which differs from Example 1 only in that N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane is used to replace KH550.

[0122] Comparative Example 3

[0123] This comparative example provides a method for preparing a heavy metal scavenger, which is different from Example 1 only in that the pH of the third solution is 10.

[0124] Comparative Example 4

[0125] This comparative example provides a method for preparing a heavy metal scavenger, which differs from Example 1 only in that the pH values ​​of the first solution and the second solution are different. In this comparative example, the pH value of the first solution is 6, and the pH value of the second solution is 6.

[0126] Effect Example 1

[0127] This effect example tests the removal effects of the primary modified product, the secondary modified product and the heavy metal capture agent obtained in Example 1 on heavy metals under different pH conditions.

[0128] The test method is as follows:

[0129] (1) Take 500 mL of ternary lithium battery precursor mother liquor wastewater, adjust the pH of the wastewater to 5, wherein nickel is 120 mg / L, cobalt is 30 mg / L, and manganese is 5 mg / L, add 1 g of the primary modifier, secondary modifier and heavy metal scavenger obtained in Example 1 respectively, react for 2 h, add 2 ml of flocculant, react for 30 min, test the nickel, cobalt and manganese contents in the wastewater, and calculate the removal rates of nickel, cobalt and manganese.

[0130] (2) Take 500 mL of ternary lithium battery precursor mother liquor wastewater, adjust the pH of the wastewater to 7, wherein nickel is 120 mg / L, cobalt is 30 mg / L, and manganese is 5 mg / L. Add 1 g of the primary modifier, secondary modifier and heavy metal scavenger obtained in Example 1 respectively, react for 2 h, add 2 ml of flocculant, react for 30 min, test the nickel, cobalt and manganese contents in the wastewater, and calculate the removal rates of nickel, cobalt and manganese.

[0131] (3) Take 500 mL of ternary lithium battery precursor mother liquor wastewater, adjust the pH of the wastewater to 9, wherein nickel is 120 mg / L, cobalt is 30 mg / L, and manganese is 5 mg / L. Add 1 g of the primary modifier, secondary modifier and heavy metal scavenger obtained in Example 1 respectively, react for 2 h, add 2 ml of flocculant, react for 30 min, test the nickel, cobalt and manganese contents in the wastewater, and calculate the removal rates of nickel, cobalt and manganese.

[0132] The test results are shown in Table 1-3.

[0133] Table 1 Removal rates of nickel, cobalt and manganese by different modified substances at pH = 5

[0134] sample Nickel (mg / l) Cobalt (mg / l) Manganese (mg / l) As is 120 30 5 One-time modified 118 29 4.8 Secondary modified product 107 26 4.3 Heavy metal capture agent 95 21 3.6

[0135] Table 2 Removal rates of nickel, cobalt and manganese by different modified substances at pH = 7

[0136] sample Nickel (mg / l) Cobalt (mg / l) Manganese (mg / l) As is 120 30 5 One-time modified 102 25 4.6 Secondary modified product 93 23 3.9 Heavy metal capture agent 15 13 0.7

[0137] Table 3 Removal rates of nickel, cobalt and manganese by different modified substances at pH = 9

[0138] sample Nickel (mg / l) Cobalt (mg / l) Manganese (mg / l) As is 120 30 5 One-time modified 102 25 4.6 Secondary modified product 93 23 3.9 Heavy metal capture agent 7.2 8.6 0.1

[0139] It can be seen from Tables 1-3 that under acidic conditions, the heavy metal capture agent treats wastewater, wherein the nickel removal rate is 20.83%, the cobalt removal rate is 30%, and the manganese removal rate is 28%; under neutral conditions, the heavy metal capture agent treats wastewater, wherein the nickel removal rate is 87.5%, the cobalt removal rate is 56.67%, and the manganese removal rate is 86%; under alkaline conditions, the heavy metal capture agent treats wastewater, wherein the nickel removal rate is 94%, the cobalt removal rate is 71.33%, and the manganese removal rate is 98%; it can be seen that the heavy metal capture agent disclosed in the present invention has a good removal effect on nickel, cobalt, and manganese under neutral and alkaline conditions (pH = 7-9).

[0140] Effect Example 2

[0141] This effect example tests the removal effect of heavy metals by the heavy metal capture agents obtained in Examples 1-14 and Comparative Examples 1-4.

[0142] The test method is as follows: take 500mL of ternary lithium battery precursor mother liquor wastewater, adjust the pH of the wastewater to 9, wherein nickel is 120mg / L, cobalt is 30mg / L, and manganese is 5mg / L, add 1g of the primary modifier, secondary modifier and heavy metal scavenger obtained in Example 1 respectively, react for 2h, add 2ml of flocculation material, react for 30min, test the nickel, cobalt and manganese content in the wastewater, and calculate the removal rate of nickel, cobalt and manganese. The test results are shown in Table 4.

[0143] Table 4

[0144] sample nickel(%) cobalt(%) manganese(%) Example 1 94 71 98 Example 2 89 64 86 Example 3 69 61 78 Example 4 91 63 95 Example 5 74 57 89 Example 6 69 51 81 Example 7 62 48 76 Example 8 87 69 92 Example 9 84 67 88 Example 10 93 71 97 Embodiment 11 79 62 84 Example 12 91 65 87 Embodiment 13 93 71 93 Embodiment 14 97 76 98 Comparative Example 1 59 23 41 Comparative Example 2 36 17 26 Comparative Example 3 21 8 14 Comparative Example 4 32 26 13

[0145] It can be seen from Table 4 that the heavy metal capture agent disclosed in the present invention has a good removal effect on nickel, cobalt and manganese.

[0146] By comparing Example 1 with Examples 4-7, it can be seen that when the grafting rate of the thiol compound in the heavy metal capture agent is 19-55%, the removal rate of the heavy metal capture agent for nickel is 62%-94%, the removal rate for cobalt is 48%-71%, and the removal rate for manganese is 76%-98%.

[0147] By comparing Example 1 with Examples 8-11, it can be seen that when the pH of the first solution and the second solution are independently 2.5-5, the heavy metal capture agent has a nickel removal rate of 84%-94%, a cobalt removal rate of 67%-71%, and a manganese removal rate of 88%-98%.

[0148] Comparison of Example 1 and Examples 12-14 shows that when the specific surface area of ​​calcium sulfate hemihydrate whiskers is 60-130 m 2 / g, and when the aspect ratio is 80-110, the removal rate of the heavy metal capture agent for nickel is 91%-97%, the removal rate for cobalt is 65%-76%, and the removal rate for manganese is 87%-98%.

[0149] By comparing Example 1 with Comparative Examples 1-4, it can be seen that only the heavy metal capture agent prepared by selecting the raw materials and parameters disclosed in the present invention has a good removal effect on nickel, cobalt and manganese.

[0150] Finally, it should be noted that the above embodiments are used to illustrate the technical solution of the present disclosure rather than to limit the protection scope of the present disclosure. Although the present disclosure has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present disclosure can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present disclosure.

Claims

1. A method for preparing a heavy metal scavenger, characterized in that: The following steps are involved: Preparation of calcium sulfate hemihydrate whiskers: treating phosphogypsum with hydrochloric acid and then aging to obtain calcium sulfate hemihydrate whiskers; Preparing a primary modified product: mixing the calcium sulfate hemihydrate whiskers and the first alcohol solvent evenly, and adjusting the pH of the solution to 2-5 to obtain a first solution; After γ-aminopropyltriethoxysilane and the second alcohol solvent are uniformly mixed, the pH of the solution is adjusted to 2-5 to obtain a second solution; the first solution is added dropwise to the second solution to react to obtain a primary modified product; preparing a secondary modified product; After the maleimide and the polar solvent are uniformly mixed, the pH of the solution is adjusted to 8-9 to obtain a third solution; the primary modified product is added to the third solution for reaction to obtain a secondary modified product; Preparation of heavy metal scavenger: after uniformly dispersing a mixture of a secondary modified substance, a photoinitiator, a thiol compound, and a third alcohol solvent, performing a photocuring reaction to obtain a heavy metal scavenger; Wherein, the thiol compound is at least one of trimethylolpropane-3-mercaptopropionate, 3-mercaptopropionic acid ethyl ester, and 3-mercapto-1-propanol; the mass ratio of the secondary modified product to the thiol modified product is (1:0.65)-(1:0.85).

2. The preparation method according to claim 1, characterized in that The mass ratio of the secondary modified product to the mercapto modified product is (1:0.7)-(1:0.85).

3. The preparation method according to claim 1, characterized in that: The mass ratio of the calcium sulfate hemihydrate whiskers to γ-aminopropyltriethoxysilane is (0.75:1)-(1.1:1).

4. The preparation method according to claim 1, characterized in that: The mass ratio of the maleimide to the primary modified product is (0.6:1)-(1.2:1).

5. The preparation method according to claim 1, characterized in that: The mass ratio of the secondary modified product to the photoinitiator is (50:1)-(60:1).

6. The preparation method according to claim 1, characterized in that: The pH of the first solution and the second solution are each independently selected from 2.5-5.

7. The preparation method according to claim 1, characterized in that: The specific surface area of ​​the calcium sulfate hemihydrate whisker is 40-130 m 2 / g, aspect ratio is 80-110.

8. The preparation method according to claim 1, characterized in that: In the preparation of the primary modified product, the reaction temperature is 20-40° C. and the reaction time is 0.5-3 h.

9. The preparation method according to claim 1, characterized in that: In the preparation of the secondary modified product, the reaction time is 10-12 hours.

10. The preparation method according to claim 1, characterized in that: In the preparation of the heavy metal capture agent, ultrasonic oscillation is used for dispersion, and the time of ultrasonic oscillation is 10-20 minutes.

11. The preparation method according to claim 1, characterized in that: The solid-to-liquid ratio of the phosphogypsum and hydrochloric acid is 0.1-0.2 g / mL; and / or the treatment temperature is 110-130° C. and the treatment time is 10-30 min; and / or the mass fraction of the hydrochloric acid is 21%-98%; and / or the aging time is 5-8 h.

12. The preparation method according to claim 1, characterized in that: The first alcohol solvent, the second alcohol solvent and the third alcohol solvent are each independently selected from at least one of ethanol, methanol, propanol and n-butanol.

13. The preparation method according to claim 1, characterized in that: The polar solvent is at least one of dimethyl sulfoxide, N,N'-dimethylformamide and N,N'-dimethylacetamide.

14. The preparation method according to claim 1, characterized in that: The photoinitiator is benzoin and its derivatives.

15. A heavy metal scavenger, characterized in that: The heavy metal scavenger is prepared by the preparation method of the heavy metal scavenger according to any one of claims 1 to 14.

16. The heavy metal scavenger according to claim 15, characterized in that The grafting rate of the mercapto compound in the heavy metal capture agent is 19-55%.

17. The heavy metal scavenger according to claim 16, characterized in that The grafting rate of the mercapto compound in the heavy metal capture agent is 25-40%.

18. Use of the heavy metal scavenger according to claims 15 to 17 in water treatment.