Hydrophobic modified AGM separator and preparation method thereof

By pretreatment and spraying modified hydrophobic coatings on the AGM partition, a coating with low surface energy and micro-nano rough structure is formed, which solves the problem of reduced hydrophobic performance caused by epoxy resin curing and improves the hydrophobicity of the AGM partition. Performance and strength.

CN118943642AInactive Publication Date: 2024-11-12ANHUI BAOHONG NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411057985.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-02
Publication Date
2024-11-12
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The hydroxyl groups generated by the epoxy ring opening during the curing process of existing AGM partitions lead to an increase in surface energy, reducing hydrophobic properties, and limiting the application of epoxy resin in the hydrophobicity of AGM partitions.

Method used

By pretreating on glass fibers to increase surface roughness and spraying modified hydrophobic coatings on the surface of the AGM partitions, containing modified nanosilica colloids and modified epoxy resins, to form micro-nano rough structures and low surfaces Energized coating to improve hydrophobic properties.

Benefits of technology

It improves the hydrophobic properties and strength of the AGM partition, reduces the loss of electrolyte, and enhances the toughness and impact strength of the material.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004976980310000091
    Figure BDA0004976980310000091
Patent Text Reader

Abstract

The invention discloses a hydrophobic modified AGM separator and a preparation method thereof, and belongs to the technical field of storage batteries, and the preparation method comprises the following steps: S1, after pickling glass fibers, soaking the glass fibers in a pretreatment solution for 5-6 hours to obtain hydrophobic pretreated glass fibers; s2, the hydrophobic pretreated glass fibers, high-density polyethylene fibers and auxiliaries are subjected to pulping, pulp mixing and deslagging treatment and then input into a forming machine, and an AGM partition board blank is obtained; and S3, uniformly spraying the modified hydrophobic coating on the AGM partition plate blank to form a uniform coating with the thickness of 110-120 microns, and then drying and curing to obtain the hydrophobic modified AGM partition plate, according to the invention, the glass fiber is taken as a base material, the high-density polyethylene fiber is taken as a reinforcement body, and a coating with a micro-nano coarse structure and low surface energy is formed on the surface of the AGM separator through the modified hydrophobic coating, so that the hydrophobic performance and strength of the AGM separator are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of storage batteries, and in particular relates to a hydrophobically modified AGM separator and a preparation method thereof. Background Art

[0002] With the increasing demand for energy and the improvement of environmental awareness, batteries have been widely used in the fields of communications, electricity, electric vehicles and energy storage systems due to their practicality, economy and environmental protection. AGM separator plays a key role in batteries. It can not only isolate the electrolyte, but also effectively prevent the positive and negative electrodes from short-circuiting. Improving the hydrophobicity of AGM separator can reduce the loss of electrolyte.

[0003] In the prior art, coatings with super hydrophobic properties usually have low surface energy and the ability to form micro-nano-scale rough structures on the surface of the material. Epoxy resin has excellent coating film adhesion ability. Epoxy resin is usually used as the coating base material, and the coating is cured on the surface of the AGM separator under the action of a curing agent. However, during the curing process of the epoxy resin, the hydroxyl groups generated by the ring opening of the epoxy group increase the surface energy of the material and reduce the hydrophobic properties of the AGM separator. Therefore, the application of epoxy resin in the hydrophobicity of the AGM separator is limited. Summary of the invention

[0004] The object of the present invention is to provide a hydrophobically modified AGM separator and a preparation method thereof to solve the problems in the background technology.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A method for preparing a hydrophobically modified AGM separator comprises the following steps:

[0007] S1. placing the glass fiber in a hydrochloric acid solution with a concentration of 1wt%, pickling it at 70-80°C for 4-5h, washing it with deionized water, soaking it in a pretreatment solution for 5-6h, and then washing and drying it to obtain a hydrophobic pretreated glass fiber;

[0008] S2, after the hydrophobic pretreated glass fiber, high-density polyethylene fiber and additives are processed by beating, mixing and deslagging, they are input into a molding machine to obtain an AGM separator blank;

[0009] S3, spraying the modified hydrophobic coating evenly on the AGM separator blank to form a uniform coating with a thickness of 110-120 μm, and then drying and curing to obtain a hydrophobic modified AGM separator;

[0010] The weight ratio of the glass fiber, the hydrochloric acid solution and the pretreatment liquid is 100-110:400-500:500-600; the weight ratio of the hydrophobic pretreated glass fiber, the high-density polyethylene fiber and the additive is 90-100:15-18:2-3.

[0011] Further, the pretreatment solution is prepared by dissolving 0.2-2 g of hexadecyltrimethylammonium bromide in 100 mL of deionized water;

[0012] Further, the modified hydrophobic coating is prepared by the following steps:

[0013] A1. Add anhydrous ethanol and 25wt% ammonia water to deionized water, stir and mix, add tetraethyl orthosilicate dropwise at 55-60°C, stir and react for 2-4h, then add hexamethyldisilazane, and ultrasonically react for 2-3h to obtain modified nano silica colloid; using ammonia water as a catalyst, the silanol groups generated by the hydrolysis of tetraethylorthosilicate are subjected to condensation polymerization to obtain silica colloid, which is then bonded with the trimethylsilyl group of hexamethyldisilazane to obtain modified silica colloid containing hydrophobic hexamethyldisilazane grafting;

[0014] A2. Add modified epoxy resin to tetrahydrofuran, stir and mix at 20-30° C., then add modified nano silica colloid and isophorone diamine, stir and mix, and then ultrasonically react for 30-50 minutes, and then stand and defoam for 10 minutes to obtain a modified hydrophobic coating; tetrahydrofuran is used as a solvent and isophorone diamine is used as a curing agent to obtain a modified hydrophobic coating containing a micro-nano structure and low surface energy.

[0015] Furthermore, the volume ratio of the deionized water, anhydrous ethanol, ammonia water, ethyl orthosilicate and hexamethyldisilazane is 20:5-6:1:4-5:2-3.

[0016] Furthermore, the volume ratio of tetrahydrofuran, modified epoxy resin, modified nano silica colloid and isophorone diamine is 35:9-10:1-2:0.5.

[0017] Furthermore, the modified epoxy resin is prepared by the following steps:

[0018] B1. Add hexafluorobutyl acrylate and hexafluorobutyl methacrylate to butanone, stir and mix, add mercaptoethanol and azobisisobutyronitrile, react at 80-90° C. for 16-24 hours, cool to 60-70° C., add isocyanoethyl methacrylate and dibutyltin dilaurate, continue to stir and react for 18-24 hours, purify with petroleum ether, and dry to obtain a prepolymer intermediate; use azobisisobutyronitrile and dibutyltin dilaurate as catalysts and mercaptoethanol as a chain transfer agent, adopt a free radical polymerization method to introduce a long fluorocarbon chain into the isocyanoethyl methacrylate molecular chain, and obtain a prepolymer intermediate containing a long fluorocarbon chain and a methacryloyloxy group, wherein the methacryloyloxy group serves as a polymerizable group;

[0019] B2. Add the prepolymer intermediate and glycidyl methacrylate to butanone, stir and mix, add azobisisobutyronitrile, react at 70-80°C for 8-10h, purify with petroleum ether, dry, dissolve in butanone, add bisphenol A epoxy resin, stir and react for 1-2h, and then evacuate at 50°C to obtain a modified epoxy resin; use azobisisobutyronitrile as a catalyst, perform free radical copolymerization with the prepolymer intermediate and glycidyl methacrylate to obtain a modified acrylate containing an epoxy group and a long fluorocarbon chain, and then perform a ring-opening reaction with the bisphenol A epoxy resin to embed the modified acrylate containing a long fluorocarbon chain into the bisphenol A epoxy resin matrix to obtain a modified epoxy resin containing a long fluorocarbon chain.

[0020] Furthermore, the usage ratio of butanone, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, mercaptoethanol, azobisisobutyronitrile, isocyanoethyl methacrylate and dibutyltin dilaurate is 40mL:10-12mL:8-11mL:1-2mL:0.5g:4-6mL:0.4mL.

[0021] Furthermore, the usage ratio of butanone, prepolymer intermediate, glycidyl methacrylate, azobisisobutyronitrile and bisphenol A epoxy resin is 100 mL: 10-12 mL: 9-14 mL: 1 g: 18-20 mL.

[0022] A hydrophobically modified AGM separator is prepared by the above preparation method.

[0023] Beneficial effects of the present invention:

[0024] The pretreatment liquid of the present invention contains hexadecyl trimethyl ammonium bromide, which can be coated on the surface of the glass fiber by electrostatic adsorption with the glass fiber with negative surface charge after pickling during impregnation treatment, thereby increasing the roughness of the surface of the glass fiber and improving the mechanical interlocking effect of the subsequent coating. At the same time, the methyl and methylene groups on the coating layer improve the hydrophobicity of the glass fiber. In addition, the hexadecyl trimethyl ammonium bromide can also be used as a softener to reduce the damage to the glass fiber during the pulping process and improve the toughness of the AGM separator.

[0025] The modified hydrophobic coating of the present invention introduces modified nano silica colloid with hydrophobic properties. When the modified hydrophobic coating is sprayed on the surface of the AGM separator blank, the modified nano silica colloid and the hydrophobic phase of the AGM separator blank are mutually adsorbed, so that the modified nano silica colloid is evenly dispersed on the AGM separator blank, and a coating layer with a micro-nano rough structure is formed on the surface of the AGM separator, thereby improving the hydrophobic property of the AGM separator.

[0026] The modified epoxy resin of the present invention introduces a long fluorocarbon chain with low surface energy into the molecular chain. Compared with the short fluorocarbon chain, the long fluorocarbon chain not only has stronger hydrophobicity, but also has the property of being easier to migrate to the coating substrate, so that the surface energy of the modified epoxy resin is reduced and the hydrophobicity is improved. When the modified hydrophobic coating is sprayed on the surface of the AGM partition blank, the long fluorocarbon chain can be entangled with the hydrophobic phase of the AGM partition blank through intermolecular entanglement, and the modified epoxy resin is evenly and stably coated on the surface of the AGM partition, so that the surface energy of the AGM partition is reduced, and the hydrophobicity of the AGM partition is further improved; at the same time, under the action of the curing agent, the epoxy group of the modified epoxy resin is ring-opened, and the molecular chains are bonded to each other to form a three-dimensional cross-linked network, which improves the impact strength of the coating, and then improves the strength of the AGM partition;

[0027] The present invention uses glass fiber as a base material and high-density polyethylene fiber as a reinforcement. Through the synergistic effect of modified nano silica colloid and modified epoxy resin in the modified hydrophobic coating, a coating with a micro-nano rough structure and low surface energy is formed on the surface of the AGM separator, thereby improving the hydrophobic performance and strength of the AGM separator. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] Example 1

[0030] This embodiment provides a modified hydrophobic coating, which is prepared by the following steps:

[0031] A1. Add 10 mL of anhydrous ethanol and 2 mL of 25 wt% ammonia water to 40 mL of deionized water, stir and mix, add 8 mL of ethyl orthosilicate dropwise at 55°C, stir and react for 2 h, then add 4 mL of hexamethyldisilazane, and ultrasonically react for 2 h to obtain modified nano silica colloid;

[0032] A2. Add 18 mL of modified epoxy resin to 70 mL of tetrahydrofuran, stir and mix at 20°C, then add 2 mL of modified nano silica colloid and 1 mL of isophorone diamine, stir and mix, then ultrasonically react for 30 minutes, and then stand and defoam for 10 minutes to obtain a modified hydrophobic coating.

[0033] Example 2

[0034] This embodiment provides a modified hydrophobic coating, which is prepared by the following steps:

[0035] A1. Add 11 mL of anhydrous ethanol and 2 mL of 25 wt% ammonia water to 40 mL of deionized water, stir and mix, add 9 mL of tetraethyl orthosilicate dropwise at 58 °C, stir and react for 3 h, then add 5 mL of hexamethyldisilazane, and ultrasonically react for 2.5 h to obtain modified nano silica colloid;

[0036] A2. Add 19 mL of modified epoxy resin to 70 mL of tetrahydrofuran, stir and mix at 25 °C, then add 3 mL of modified nano silica colloid and 1 mL of isophorone diamine, stir and mix, then ultrasonically react for 40 min, and then stand and defoam for 10 min to obtain a modified hydrophobic coating.

[0037] Example 3

[0038] This embodiment provides a modified hydrophobic coating, which is prepared by the following steps:

[0039] A1. Add 12 mL of anhydrous ethanol and 2 mL of 25 wt% ammonia water to 40 mL of deionized water, stir and mix, add 10 mL of ethyl orthosilicate dropwise at 60°C, stir and react for 4 h, then add 6 mL of hexamethyldisilazane, and ultrasonically react for 3 h to obtain modified nano silica colloid;

[0040] A2. Add 20 mL of modified epoxy resin to 70 mL of tetrahydrofuran, stir and mix at 30° C., then add 4 mL of modified nano silica colloid and 1 mL of isophorone diamine, stir and mix, then ultrasonically react for 50 min, and then stand and defoam for 10 min to obtain a modified hydrophobic coating.

[0041] Example 4

[0042] This embodiment provides a modified epoxy resin, which is prepared by the following steps:

[0043] B1. Add 10 mL of hexafluorobutyl acrylate and 8 mL of hexafluorobutyl methacrylate to 40 mL of butanone, stir and mix, add 1 mL of mercaptoethanol and 0.5 g of azobisisobutyronitrile, react at 80° C. for 16 h, then cool to 60° C., add 4 mL of isocyanoethyl methacrylate and 0.4 mL of dibutyltin dilaurate, continue stirring and reacting for 18 h, and then purify with petroleum ether and dry to obtain a prepolymer intermediate;

[0044] B2. Add 10 mL of the prepolymer intermediate and 9 mL of glycidyl methacrylate to 40 mL of butanone, stir to mix, add 1 g of azobisisobutyronitrile, react at 70 °C for 8 h, purify with petroleum ether and dry, dissolve in 60 mL of butanone, add 18 mL of bisphenol A epoxy resin, stir to react for 1 h, and then evacuate at 50 °C to obtain a modified epoxy resin.

[0045] Example 5

[0046] This embodiment provides a modified epoxy resin, which is prepared by the following steps:

[0047] B1. Add 11 mL of hexafluorobutyl acrylate and 10 mL of hexafluorobutyl methacrylate to 40 mL of butanone, stir and mix, add 1.5 mL of mercaptoethanol and 0.5 g of azobisisobutyronitrile, react at 85° C. for 20 h, then cool to 65° C., add 5 mL of isocyanoethyl methacrylate and 0.4 mL of dibutyltin dilaurate, continue stirring and reacting for 20 h, and then purify with petroleum ether and dry to obtain a prepolymer intermediate;

[0048] B2. Add 11 mL of the prepolymer intermediate and 12 mL of glycidyl methacrylate to 40 mL of butanone, stir to mix, add 1 g of azobisisobutyronitrile, react at 75 °C for 9 h, purify with petroleum ether and dry, dissolve in 60 mL of butanone, add 19 mL of bisphenol A epoxy resin, stir to react for 1.5 h, and then evacuate at 50 °C to obtain a modified epoxy resin.

[0049] Example 6

[0050] This embodiment provides a modified epoxy resin, which is prepared by the following steps:

[0051] B1. Add 12 mL of hexafluorobutyl acrylate and 11 mL of hexafluorobutyl methacrylate to 40 mL of butanone, stir and mix, add 2 mL of mercaptoethanol and 0.5 g of azobisisobutyronitrile, react at 90° C. for 24 h, then cool to 70° C., add 6 mL of isocyanoethyl methacrylate and 0.4 mL of dibutyltin dilaurate, continue stirring and reacting for 24 h, and then purify with petroleum ether and dry to obtain a prepolymer intermediate;

[0052] B2. Add 12 mL of prepolymer intermediate and 14 mL of glycidyl methacrylate to 40 mL of butanone, stir to mix, add 1 g of azobisisobutyronitrile, react at 80 °C for 10 h, purify with petroleum ether and dry, dissolve in 60 mL of butanone, add 20 mL of bisphenol A epoxy resin, stir to react for 2 h, and then evacuate at 50 °C to obtain a modified epoxy resin.

[0053] Example 7

[0054] This embodiment provides a hydrophobically modified AGM separator, comprising the following steps:

[0055] S1. Add 0.2 g of hexadecyltrimethylammonium bromide to 100 mL of deionized water, stir to dissolve, and obtain a pretreatment solution.

[0056] S1. 100 parts by weight of glass fiber are placed in 400 parts by weight of a 1 wt% hydrochloric acid solution, pickled at 70° C. for 4 h, washed with deionized water, and then immersed in 500 parts by weight of a pretreatment solution for 5 h, and then washed and dried to obtain a hydrophobic pretreated glass fiber;

[0057] S3, after pulping, slurry preparation and slag removal, 90 parts by weight of hydrophobic pretreated glass fiber, 15 parts by weight of high-density polyethylene fiber and 2 parts by weight of additives are input into a molding machine to obtain an AGM separator blank;

[0058] S4. The modified hydrophobic coating is evenly sprayed on the AGM separator blank to form a uniform coating with a thickness of 110 μm, and then dried and cured to obtain a hydrophobic modified AGM separator.

[0059] Example 8

[0060] This embodiment provides a hydrophobically modified AGM separator, comprising the following steps:

[0061] S1. Add 1 g of hexadecyltrimethylammonium bromide to 100 mL of deionized water, stir to dissolve, and obtain a pretreatment solution.

[0062] S1. 105 parts by weight of glass fiber are placed in 450 parts by weight of a 1 wt% hydrochloric acid solution, pickled at 75°C for 4.5 hours, washed with deionized water, and then immersed in 550 parts by weight of a pretreatment solution for 5.5 hours, and then washed and dried to obtain a hydrophobic pretreated glass fiber;

[0063] S3, 95 parts by weight of hydrophobic pretreated glass fiber, 17 parts by weight of high-density polyethylene fiber and 2.5 parts by weight of additives are subjected to pulping, slurry mixing and slag removal treatment, and then input into a molding machine to obtain an AGM separator blank;

[0064] S4. The modified hydrophobic coating is evenly sprayed on the AGM separator blank to form a uniform coating with a thickness of 115 μm, and then dried and cured to obtain a hydrophobic modified AGM separator.

[0065] Example 9

[0066] This embodiment provides a hydrophobically modified AGM separator, comprising the following steps:

[0067] S1. Add 2 g of hexadecyltrimethylammonium bromide to 100 mL of deionized water, stir and dissolve to obtain a pretreatment solution.

[0068] S1. 110 parts by weight of glass fiber are placed in 500 parts by weight of a 1 wt% hydrochloric acid solution, pickled at 80° C. for 5 h, washed with deionized water, and then immersed in 600 parts by weight of a pretreatment solution for 6 h. After washing and drying, a hydrophobic pretreated glass fiber is obtained;

[0069] S3, 100 parts by weight of hydrophobic pretreated glass fiber, 18 parts by weight of high-density polyethylene fiber and 3 parts by weight of additives are subjected to pulping, slurry mixing and slag removal treatment, and then input into a molding machine to obtain an AGM separator blank;

[0070] S4. The modified hydrophobic coating is evenly sprayed on the AGM separator blank to form a uniform coating with a thickness of 120 μm, and then dried and cured to obtain a hydrophobic modified AGM separator.

[0071] Comparative Example 1: Compared with Example 7, the glass fiber is not immersed in the pre-treatment liquid, and the rest is the same.

[0072] Comparative Example 2: Compared with Example 7, the modified hydrophobic coating was replaced with an equal amount of nano-silica sol, and the rest was the same.

[0073] Comparative Example 3: Compared with Example 7, the modified hydrophobic coating was replaced with an equal amount of epoxy resin coating, and the rest was the same.

[0074] Performance tests were performed on Examples 7 to 9 and Comparative Examples 1 to 3. Contact angle test: refer to GB / T24368-2009. The larger the contact angle, the smaller the rolling angle, and the better the hydrophobic performance. Impact strength: refer to GB / T 1043-2008. The results are shown in Table 1.

[0075] Table 1

[0076]

[0077] As can be seen from Table 1, the AGM separators made of modified nano silica colloid and epoxy resin in Examples 7-9 have significantly higher contact angles than those in Comparative Examples 1-3, and have good hydrophobic properties and impact strength, up to 77.3 kJ / m 2 , having higher strength; compared with Comparative Examples 2-3, Example 7 has a higher contact angle, indicating that under the synergistic effect of modified nano silica colloid and modified epoxy resin, the AGM separator has higher hydrophobicity and strength.

[0078] It should be noted that, in this article, relational terms such as first and second, etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. Moreover, the terms "include", "comprise" or any other variants thereof are intended to cover non-exclusive inclusion, so that a process, method, article or device including a series of elements includes not only those elements, but also other elements not explicitly listed, or also includes elements inherent to such process, method, article or device.

[0079] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

Claims

1. A method for preparing a hydrophobically modified AGM separator, characterized in that: The following steps are involved: S1. placing the glass fiber in a hydrochloric acid solution with a concentration of 1wt%, pickling it at 70-80°C for 4-5h, washing it with deionized water, soaking it in a pretreatment solution for 5-6h, and then washing and drying it to obtain a hydrophobic pretreated glass fiber; S2, after the hydrophobic pretreated glass fiber, high-density polyethylene fiber and additives are processed by beating, mixing and deslagging, they are input into a molding machine to obtain an AGM separator blank; S3, spraying the modified hydrophobic coating evenly on the AGM separator blank, and then drying and curing to obtain a hydrophobic modified AGM separator; The weight ratio of the glass fiber, the hydrochloric acid solution and the pretreatment solution is 100-110:400-500:500-600; The weight ratio of the hydrophobic pretreated glass fiber, the high-density polyethylene fiber and the auxiliary agent is 90-100:15-18:2-3.

2. The method for preparing a hydrophobically modified AGM separator according to claim 1, characterized in that: The pretreatment solution is prepared by dissolving 0.2-2 g of hexadecyltrimethylammonium bromide in 100 mL of deionized water.

3. The method for preparing a hydrophobically modified AGM separator according to claim 1, characterized in that: The modified hydrophobic coating is prepared by the following steps: A1. Add anhydrous ethanol and 25 wt% ammonia water to deionized water, stir and mix, add tetraethyl orthosilicate dropwise at 55-60° C., stir and react for 2-4 hours, then add hexamethyldisilazane, and ultrasonically react for 2-3 hours to obtain modified nano silica colloid; A2. Add modified epoxy resin to tetrahydrofuran, stir and mix at 20-30° C., then add modified nano silica colloid and isophorone diamine, stir and mix, then ultrasonically react for 30-50 minutes, and then stand and defoam for 10 minutes to obtain a modified hydrophobic coating.

4. The method for preparing a hydrophobically modified AGM separator according to claim 3, characterized in that: The volume ratio of the deionized water, anhydrous ethanol, ammonia water, ethyl orthosilicate and hexamethyldisilazane is 20:5-6:1:4-5:2-3.

5. The method for preparing a hydrophobically modified AGM separator according to claim 3, characterized in that: The volume ratio of tetrahydrofuran, modified epoxy resin, modified nano-silica and isophorone diamine is 35:9-10:1-2:0.

5.

6. The method for preparing a hydrophobically modified AGM separator according to claim 3, characterized in that: The modified epoxy resin is prepared by the following steps: B1. Add hexafluorobutyl acrylate and hexafluorobutyl methacrylate to butanone, stir and mix, add mercaptoethanol and azobisisobutyronitrile, react at 80-90° C. for 16-24 hours, cool to 60-70° C., add isocyanoethyl methacrylate and dibutyltin dilaurate, continue stirring and reacting for 18-24 hours, purify with petroleum ether, and dry to obtain a prepolymer intermediate; B2. Add the prepolymer intermediate and glycidyl methacrylate to butanone, stir and mix, add azobisisobutyronitrile, react at 70-80°C for 8-10h, purify with petroleum ether, dry, dissolve in butanone, add bisphenol A epoxy resin, stir and react for 1-2h, and then evacuate at 50°C to obtain a modified epoxy resin.

7. The method for preparing a hydrophobically modified AGM separator according to claim 6, characterized in that: The dosage ratio of butanone, hexafluorobutyl acrylate, hexafluorobutyl methacrylate, mercaptoethanol, azobisisobutyronitrile, isocyanoethyl methacrylate and dibutyltin dilaurate is 40mL: 10-12mL: 8-11mL: 1-2mL: 0.5g: 4-6mL: 0.4mL.

8. The method for preparing a hydrophobically modified AGM separator according to claim 6, characterized in that: The usage ratio of butanone, prepolymer intermediate, glycidyl methacrylate, azobisisobutyronitrile and bisphenol A epoxy resin is 100mL: 10-12mL: 9-14mL: 1g: 18-20mL.

9. A hydrophobically modified AGM separator, characterized in that: Prepared according to the preparation method according to any one of claims 1 to 8.