Preparation and application method of a novel wheat straw pulping catalyst
Through catalyst treatment with anhydrous sodium sulfite and other components, the problems of inaccurate heating and sewage discharge in wheat straw pulping are solved, efficient utilization of wheat straw fibers and high-quality finished products are achieved, and the physical properties of corrugated base paper are improved.
Patent Information
- Application Number
- CN202311826134.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2023-12-28
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2043-12-28
AI Technical Summary
The existing wheat straw pulping catalyst needs to be heated during use, and the preparation is not accurate, resulting in high residual alkali content after wheat straw pulping, large water consumption, easy explosion during the production process, uneven pulp quality, and failure to fully utilize the original ecological fiber. resource.
Anhydrous sodium sulfite is used as the main agent, combined with methyl hydroxyethyl cellulose, sodium dodecyl sulfate, cellulase and lignin degradation agents, and the wheat straw raw material is processed through continuous balanced fermentation and natural temperature rise to prepare a product that does not require external The heated catalyst reduces sewage discharge and is mixed with domestic waste paper pulp to form ultra-high-strength corrugated base paper.
It achieves stable pre-soaking and balanced fermentation of wheat straw fiber, reduces production costs, saves water and electricity, improves fiber integrity and finished product quality, and significantly improves the tensile strength, folding resistance and ring pressure indicators of ultra-high-strength corrugated base paper. Reduced sizing degree.
Smart Images

Figure CN117887693B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of catalyst preparation and application, and specifically refers to a preparation and application method of a novel wheat straw pulping catalyst. Background Art
[0002] Wheat straw pulp is a liquid made from wheat straw, which has a wide range of uses and is a renewable resource. Wheat straw pulp contains a large amount of cellulose and can be used by pulp mills to produce high-quality paper that is environmentally friendly, sustainable and recyclable.
[0003] At present, the existing wheat straw pulping and papermaking technology mainly has the following problems: First, when processing pulp, the catalyst liquid used must be heated to above 80°C, and the heated liquid must be used to soak wheat straw and other raw materials. The prepared catalyst liquid is completely manually explored and added, which is not accurate and scientific, resulting in uneven raw and raw materials after soaking and poor quality; Second, the wheat straw pulp soaked with traditional catalyst liquid is prone to mold, black and smelly, and the squeezed sewage will be black and sticky. The residual alkali content after pulping is very high, which increases the pressure and water consumption of subsequent pulp washing; Third, the raw materials are soaked for a long time, and unnecessary harmful components are dissolved in large quantities, so that the residual alkali COD content in the residual liquid of the finished pulp is very high, generally 60,000 mg / L, and the high value can even reach more than 100,000 mg / L. A large amount of water is used and excess wastewater is treated, which increases investment and production costs; Fourth, the continuous addition of chlorine during the bleaching process is prone to explosion, and the final pulp quality is uneven. It can only be used as a filler mixed with waste paper, wasting the best original ecological fiber resources and failing to maximize the utilization value of raw materials. Summary of the invention
[0004] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a preparation and application method of a novel wheat straw pulping catalyst. In order to solve the problems that the original catalyst must be heated when used, the preparation is not accurate and scientific, the residual alkali content after wheat straw pulping is high, the water consumption is large, the addition of chlorine during production is prone to explosion, and the pulping quality is uneven, the present invention proposes to use anhydrous sodium sulfite as the main agent, and the prepared catalyst is used to continuously and evenly ferment the wheat straw raw material, so that no external heating and no sewage discharge are required. The prepared wheat straw fiber pulp is mixed with domestic waste to make ultra-high-strength corrugated base paper, realizing the maximum utilization value of the original ecological pulp of wheat straw fiber.
[0005] In order to achieve the above object, the technical solution adopted by the present invention is as follows: The present invention proposes a novel wheat straw pulping catalyst, comprising the following components in parts by weight:
[0006] 40-50 parts of anhydrous sodium sulfite, 18-22 parts of methyl hydroxyethyl cellulose, 6-10 parts of sodium dodecyl sulfate, 2-3 parts of cellulase, 1-12 parts of lignin degradation agent, 0.3-0.6 parts of preservative and fungicide, and 8-35 parts of ultrapure water.
[0007] Preferably, the cellulase is exoglucanase; the lignin degrading agent is lignin peroxidase; and the preservative fungicide is isothiazolinone fungicide.
[0008] The present invention also proposes a method for preparing a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0009] S1. Weigh appropriate weight portions of anhydrous sodium sulfite, methyl hydroxyethyl cellulose, sodium dodecyl sulfate, cellulase, lignin degradation agent, preservative and fungicide, and ultrapure water, put them into a catalyst preparation tank, stir and mix, and obtain an initial liquid catalyst;
[0010] S2. Using 5-10 mol / L sodium hydroxide solution and 5-10 mol / L hydrochloric acid solution, the final pH of the initial liquid catalyst obtained in S1 is adjusted to 6.5-8.0 to obtain a novel wheat straw pulping catalyst.
[0011] Preferably, in S1, the catalyst preparation tank has a stirring temperature of 20-30°C, a stirring speed of 1000-1200 r / min, and a stirring time of 1.25-2 h.
[0012] The present invention also proposes an application method of a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0013] Step 1: Pre-impregnation by grading, placing the novel wheat straw pulping catalyst and wheat straw into a double-screw stirrer for pre-impregnation, obtaining wheat straw impregnated with the catalyst and the remaining novel wheat straw pulping catalyst;
[0014] Step 2: Efficient compounding: after the pre-impregnation is completed, the content of anhydrous sodium sulfite in the remaining novel wheat straw pulping catalyst obtained in step 1 is measured, and the consumed part is replenished in time to obtain a compounded novel wheat straw pulping catalyst, which acts on the next round of graded pre-impregnation;
[0015] Step 3: catalytic heating: put the wheat straw soaked with the catalyst prepared in step 1 into the catalytic reaction tank, and naturally ferment and heat it to 70-85°C for 12-15 hours to obtain softened wheat straw fiber raw material;
[0016] Step 4: Put the softened wheat straw fiber raw material prepared in step 3 into an oblique kneading machine for rubbing and separating, and then use a high-concentration pulping machine to obtain golden wheat straw pulp;
[0017] Step 5: beating and screening. The golden straw pulp prepared in step 4 is further processed. The golden straw pulp is put into a decomposition tank for full swelling. Then, it is refined by two medium-concentration pulping machines and screened by an outflow corrugated screen. The qualified straw pulp is collected in a refined pulp bin. The qualified straw pulp has a beating degree of 35-40°SR and a wet weight of 2.6-3.0 g. The unqualified straw pulp is returned to the decomposition tank.
[0018] Step 6: The qualified wheat straw pulp prepared in step 5 is mixed with pure domestic waste paper pulp in a mixing bin at a blending ratio of 10-30%, and pumped to a 4400 / 500 long-net multi-cylinder papermaking machine to obtain a quantitative 80-120 g / m 2 Ultra-high-strength corrugated paper.
[0019] Preferably, in step 1, the weight ratio of the novel wheat straw pulping catalyst to the wheat straw is 1:40-60; the pre-soaking temperature of the double-helix stirrer is 30-40° C., and the pre-soaking time is 24-28 h.
[0020] Preferably, in step 2, the determination of the content of anhydrous sodium sulfite specifically comprises the following steps:
[0021] L1. Quickly weigh 0.25 kg of the new wheat straw pulping catalyst remaining after pre-soaking, accurate to 0.0001 g;
[0022] L2, place the remaining novel wheat straw pulping catalyst obtained in L1 into a 250 mL iodine volumetric flask pre-added with 50 mL of 0.1 mol / L iodine standard solution and 30-50 mL of ultrapure water to obtain a catalyst liquid to be measured;
[0023] L3, add 2 mL of 50% hydrochloric acid solution to the catalyst liquid to be measured obtained in L2, mix and place at 25°C in the dark for 5 min to obtain a catalyst liquid sample to be titrated;
[0024] L4. Use 0.1 mol / L sodium thiosulfate standard solution to titrate the catalyst liquid sample obtained in L3 until it turns light yellow. Add 3 mL of starch indicator and continue titrating until the blue color disappears, which is the end point. At the same time, perform a blank experiment and calculate the content of anhydrous sodium sulfite: percentage of anhydrous sodium sulfite = difference between the volume of sodium thiosulfate standard solution consumed by the blank and the volume of sodium thiosulfate standard solution consumed by the sample × concentration of sodium thiosulfate standard solution × 0.06302 / mass of sample × 100%.
[0025] Preferably, in step four, the oblique silk kneading machine has a power of 6-10 kW, a main shaft speed of 1680-2800 r / min, a silk kneading length of 80-100 mm, and a range of 4000-8000 mm; the high-concentration pulping machine has a power of 30-50 kW, a pulping temperature of 28-34°C, and a pulping time of 1.5-2.6 h.
[0026] Preferably, in step five, the swelling temperature of the decomposition tank is 30-36°C, and the swelling time is 2-3 h; the power of the medium-concentration refiner is 20-30 kW, the refining temperature is 30-35°C, and the refining time is 1.5-3 h; the power of the outflow corrugated screen is 22-45 kW, the pulp inlet pressure is 0.1-0.25 MPa, and the screen hole specification is 1.2-2.4 mm.
[0027] Preferably, in step six, the mixing temperature of the mixing bin is 30-40°C, the mixing speed is 600-800 r / min, and the mixing time is 2-2.8 h; the power of the fourdrinier multi-cylinder papermaking machine is 150-180 kW, the working speed is 200-300 m / min, the dynamic balance speed is 400-500 m / min, and the working pressure is 0.6-0.8 MPa.
[0028] The beneficial effects achieved by the present invention are as follows:
[0029] The novel wheat straw pulping catalyst prepared by the present invention is environmentally friendly and efficient, and the anhydrous sodium sulfite, cellulase, and lignin degradation agent contained therein can be continuously and evenly fermented, heated, softened, and degraded with wheat straw, and the quality of the wheat straw soaked with the catalyst is stable; when the novel wheat straw pulping catalyst is pre-soaked with wheat straw, no external heating, no soaking, and no sewage discharge are required, and the remaining novel wheat straw pulping catalyst after pre-soaking is measured by a scientific method for the content of anhydrous sodium sulfite therein, and the consumed part is replenished in time, and the obtained composite novel wheat straw pulping catalyst can be used to pre-soak the next round of wheat straw, so that the novel wheat straw pulping catalyst is fully utilized without waste, and the production cost is greatly saved compared with the traditional process. , which has great promotion advantages; the softened wheat straw fiber raw material does not need to be excessively soaked and boiled, so the fiber dissolution is less, the pulp is high, water and electricity are saved, and an oblique silk kneading machine is used for sufficient rubbing and silk separation instead of cutting and grinding, which effectively protects the integrity of the plant fiber; the plant fiber belongs to the original ecological fiber, and the qualified wheat straw pulp of the present invention better maintains the strength and toughness of the plant fiber itself, thus showing excellent characteristics, especially for the papermaking of ultra-high strength corrugated paper, as long as the blending amount with pure domestic waste paper pulp is between 15-30%, the tensile index, folding index and ring crush index of the ultra-high strength corrugated paper can be significantly improved, and the sizing degree of the product can be reduced. The tensile index of the prepared ultra-high strength corrugated paper reaches 33 Nm / g, and the folding index is 2.52 kPa.m 2 / g, ring crush index is 8.71 Nm / g, sizing degree is 0.27 mm, and it has good quality; however, the wheat straw pulp processed by traditional technology can only be used as filler with a blending amount of between 3-5% due to its simple technology and rigid model. As for improving the physical indicators of the finished paper, it is even more difficult. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] In order to more clearly illustrate the present invention or the technical solutions in the prior art, the following will be described in a clear and understandable manner in conjunction with the accompanying drawings. Obviously, the drawings described below are only for the present invention, and for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.
[0031] Figure 1 This is a graph showing the tensile index measurement results of the ultra-high-strength corrugated base paper prepared in Examples 1-5 of the present invention;
[0032] Figure 2 This is a graph showing the folding index test results of the ultra-high-strength corrugated paper prepared in Examples 1-5 of the present invention;
[0033] Figure 3 This is a graph showing the ring crush index measurement results of the ultra-high strength corrugated paper prepared in Examples 1-5 of the present invention;
[0034] Figure 4 This is a graph showing the sizing degree measurement results of the ultra-high strength corrugated base paper prepared in Examples 1-5 of the present invention. DETAILED DESCRIPTION
[0035] The following will clearly and completely describe the technical solutions in the embodiments of the present invention based on the above design of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0036] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.
[0037] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials used in the following examples are purchased from commercial channels unless otherwise specified.
[0038] Example 1: This example provides a preparation and application method of a novel wheat straw pulping catalyst, wherein the novel wheat straw pulping catalyst comprises the following components in parts by weight:
[0039] 40 parts of anhydrous sodium sulfite, 18 parts of methyl hydroxyethyl cellulose, 6 parts of sodium dodecyl sulfate, 2 parts of glucan exo-onuclease, 1 part of lignin peroxidase, 0.3 parts of isothiazolinone fungicide, and 8 parts of ultrapure water.
[0040] This embodiment also provides a method for preparing a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0041] S1. Weigh appropriate weight portions of anhydrous sodium sulfite, methyl hydroxyethyl cellulose, sodium dodecyl sulfate, cellulase, lignin degradation agent, preservative and fungicide, and ultrapure water, put them into a catalyst preparation tank, and stir to mix at a stirring temperature of 20° C., a stirring speed of 1000 r / min, and a stirring time of 1.25 h to obtain an initial liquid catalyst;
[0042] S2. Using 5 mol / L sodium hydroxide solution and 5 mol / L hydrochloric acid solution, the final pH of the initial liquid catalyst obtained in S1 was adjusted to 6.5 to obtain a novel wheat straw pulping catalyst.
[0043] This embodiment also provides an application method of a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0044] Step 1: pre-impregnation by graded method: the new wheat straw pulping catalyst and wheat straw are put into a double-screw stirrer in a weight ratio of 1:40, and the pre-impregnation temperature is 30°C, and the pre-impregnation time is 24 hours to obtain wheat straw impregnated with the catalyst and the remaining new wheat straw pulping catalyst;
[0045] Step 2, efficient compounding, after the pre-immersion is completed, measure the content of anhydrous sodium sulfite in the remaining novel wheat straw pulping catalyst obtained in step 1, quickly weigh 0.25 kg of the remaining novel wheat straw pulping catalyst after the pre-immersion is completed, accurate to 0.0001 g, and place the remaining novel wheat straw pulping catalyst in a 250 mL iodine volumetric flask pre-added with 50 mL of 0.1 mol / L iodine standard solution and 30-50 mL of ultrapure water to obtain a catalyst liquid to be measured, add 2 mL of 50% hydrochloric acid solution to the catalyst liquid to be measured, mix and place at 25°C in the dark for 5 min to obtain a catalyst liquid sample to be titrated, use a 0.1 mol / L sodium thiosulfate standard solution to titrate the catalyst liquid sample to be titrated until it turns light yellow, then add 3 mL starch indicator is titrated continuously until the blue color disappears, which is the end point. At the same time, a blank experiment is performed to calculate the content of anhydrous sodium sulfite: the percentage of anhydrous sodium sulfite = the difference between the volume of sodium thiosulfate standard solution consumed by the blank and the volume of sodium thiosulfate standard solution consumed by the sample × the concentration of sodium thiosulfate standard solution × 0.06302 / the mass of the sample × 100%. The consumed part is replenished in time to obtain the composite new wheat straw pulping catalyst, which acts on the next round of graded pre-soaking;
[0046] Step 3: catalytic heating: put the wheat straw soaked with the catalyst prepared in step 1 into the catalytic reaction tank, and naturally ferment and heat to 70°C for 12 hours to obtain softened wheat straw fiber raw material;
[0047] Step 4: Put the softened wheat straw fiber raw material prepared in step 3 into an oblique kneading machine with a power of 6 kW, a main shaft speed of 1680 r / min, a kneading length of 80 mm, a range of 4000 mm, rub and separate the fibers, and then use a high-concentration pulping machine with a power of 30 kW, a pulping temperature of 28°C, and a pulping time of 1.5 h to obtain golden wheat straw pulp;
[0048] Step 5: brooming and screening. The golden straw pulp prepared in step 4 is further processed. The golden straw pulp is put into a decomposition tank for full swelling. The swelling temperature is 30°C and the swelling time is 2 h. Then, it is refined by two medium-concentration pulping machines with a power of 20 kW, a pulping temperature of 30°C and a pulping time of 1.5 h. It is screened by an outflow corrugated screen with a power of 22 kW, a pulping pressure of 0.1 MPa and a sieve hole specification of 1.2 mm. The qualified straw pulp is collected in a refined pulp bin. The qualified straw pulp has a beating degree of 35°SR and a wet weight of 2.6 g. The unqualified straw pulp is returned to the decomposition tank.
[0049] Step 6: The qualified wheat straw pulp prepared in step 5 is fully mixed with pure domestic waste paper pulp in a mixing bin at a blending ratio of 10%, the mixing temperature is 30°C, the mixing speed is 600 r / min, the mixing time is 2 h, and the pump is sent to a 4400 / 500 long-net multi-cylinder papermaking machine with a power of 150 kW, a working speed of 200 m / min, a dynamic balance speed of 400 m / min, and a working pressure of 0.6 MPa to obtain a quantitative of 80 g / m 2 Ultra-high-strength corrugated paper.
[0050] Example 2: This example provides a preparation and application method of a novel wheat straw pulping catalyst, wherein the novel wheat straw pulping catalyst comprises the following components in parts by weight:
[0051] 45 parts of anhydrous sodium sulfite, 20 parts of methyl hydroxyethyl cellulose, 8 parts of sodium dodecyl sulfate, 2.5 parts of glucan exo-onuclease, 6 parts of lignin peroxidase, 0.4 parts of isothiazolinone fungicide, and 25 parts of ultrapure water.
[0052] This embodiment also provides a method for preparing a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0053] S1. Weigh appropriate weight portions of anhydrous sodium sulfite, methyl hydroxyethyl cellulose, sodium dodecyl sulfate, cellulase, lignin degradation agent, preservative and fungicide, and ultrapure water, put them into a catalyst preparation tank, and stir to mix at a stirring temperature of 25° C., a stirring speed of 1080 r / min, and a stirring time of 1.7 h to obtain an initial liquid catalyst;
[0054] S2. Using 8 mol / L sodium hydroxide solution and 8 mol / L hydrochloric acid solution, the final pH of the initial liquid catalyst obtained in S1 was adjusted to 7.5 to obtain a novel wheat straw pulping catalyst.
[0055] This embodiment also provides an application method of a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0056] Step 1: pre-impregnation by graded method: the new wheat straw pulping catalyst and wheat straw are put into a double-screw stirrer in a weight ratio of 1:50, and the pre-impregnation temperature is 35° C. The pre-impregnation time is 26 h to obtain wheat straw impregnated with the catalyst and the remaining new wheat straw pulping catalyst;
[0057] Step 2, efficient compounding, after the pre-immersion is completed, measure the content of anhydrous sodium sulfite in the remaining novel wheat straw pulping catalyst obtained in step 1, quickly weigh 0.25 kg of the remaining novel wheat straw pulping catalyst after the pre-immersion is completed, accurate to 0.0001 g, and place the remaining novel wheat straw pulping catalyst in a 250 mL iodine volumetric flask pre-added with 50 mL of 0.1 mol / L iodine standard solution and 30-50 mL of ultrapure water to obtain a catalyst liquid to be measured, add 2 mL of 50% hydrochloric acid solution to the catalyst liquid to be measured, mix and place at 25°C in the dark for 5 min to obtain a catalyst liquid sample to be titrated, use a 0.1 mol / L sodium thiosulfate standard solution to titrate the catalyst liquid sample to be titrated until it turns light yellow, then add 3 mL starch indicator is titrated continuously until the blue color disappears, which is the end point. At the same time, a blank experiment is performed to calculate the content of anhydrous sodium sulfite: the percentage of anhydrous sodium sulfite = the difference between the volume of sodium thiosulfate standard solution consumed by the blank and the volume of sodium thiosulfate standard solution consumed by the sample × the concentration of sodium thiosulfate standard solution × 0.06302 / the mass of the sample × 100%. The consumed part is replenished in time to obtain the composite new wheat straw pulping catalyst, which acts on the next round of graded pre-soaking;
[0058] Step 3: catalytic heating: put the wheat straw soaked with the catalyst prepared in step 1 into the catalytic reaction tank, and naturally ferment and heat it to 80°C for 14 hours to obtain softened wheat straw fiber raw material;
[0059] Step 4: Put the softened wheat straw fiber raw material prepared in step 3 into an oblique silk kneading machine with a power of 8 kW, a main shaft speed of 2000 r / min, a silk kneading length of 90 mm, a range of 6000 mm, rub and separate the silk, and then use a high-concentration pulping machine with a power of 40 kW, a pulping temperature of 30°C, and a pulping time of 1.8 h to obtain golden wheat straw pulp;
[0060] Step 5: brooming and screening. The golden straw pulp prepared in step 4 is further processed. The golden straw pulp is put into a decomposition tank for full swelling. The swelling temperature is 33°C and the swelling time is 2.5 h. Then, it is refined by two medium-concentration pulping machines with a power of 25 kW, a pulping temperature of 33°C and a pulping time of 2.5 h. It is screened by an outflow corrugated screen with a power of 30 kW, a pulping pressure of 0.2 MPa and a sieve hole specification of 2.0 mm. The qualified straw pulp is collected in a refined pulp bin. The qualified straw pulp has a beating degree of 38°SR and a wet weight of 2.8 g. The unqualified straw pulp is returned to the decomposition tank.
[0061] Step 6: The qualified wheat straw pulp prepared in step 5 is fully mixed with pure domestic waste paper pulp in a mixing bin at a blending ratio of 20%. The mixing temperature is 35°C, the mixing speed is 700 r / min, the mixing time is 2.4 h, and the pump is sent to a 4400 / 500 long-net multi-cylinder papermaking machine with a power of 170 kW, a working speed of 250 m / min, a dynamic balance speed of 450 m / min, and a working pressure of 0.7 MPa to obtain a quantitative of 100 g / m 2 Ultra-high-strength corrugated paper.
[0062] Example 3: This example provides a preparation and application method of a novel wheat straw pulping catalyst, wherein the novel wheat straw pulping catalyst comprises the following components in parts by weight:
[0063] 50 parts of anhydrous sodium sulfite, 22 parts of methyl hydroxyethyl cellulose, 10 parts of sodium dodecyl sulfate, 3 parts of glucan exo-onuclease, 12 parts of lignin peroxidase, 0.6 parts of isothiazolinone fungicide, and 35 parts of ultrapure water.
[0064] This embodiment also provides a method for preparing a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0065] S1. Weigh appropriate weight portions of anhydrous sodium sulfite, methyl hydroxyethyl cellulose, sodium dodecyl sulfate, cellulase, lignin degradation agent, preservative and fungicide, and ultrapure water, put them into a catalyst preparation tank, and stir to mix them at a stirring temperature of 30° C. and a stirring speed of 1200 r / min for 2 h to obtain an initial liquid catalyst;
[0066] S2. Using 10 mol / L sodium hydroxide solution and 10 mol / L hydrochloric acid solution, the final pH of the initial liquid catalyst obtained in S1 was adjusted to 8.0 to obtain a novel wheat straw pulping catalyst.
[0067] This embodiment also provides an application method of a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0068] Step 1: pre-impregnation by graded method: the new wheat straw pulping catalyst and wheat straw are put into a double-screw stirrer in a weight ratio of 1:60, and the pre-impregnation temperature is 40°C, and the pre-impregnation time is 28 hours to obtain wheat straw impregnated with the catalyst and the remaining new wheat straw pulping catalyst;
[0069] Step 2, efficient compounding, after the pre-immersion is completed, measure the content of anhydrous sodium sulfite in the remaining novel wheat straw pulping catalyst obtained in step 1, quickly weigh 0.25 kg of the remaining novel wheat straw pulping catalyst after the pre-immersion is completed, accurate to 0.0001 g, and place the remaining novel wheat straw pulping catalyst in a 250 mL iodine volumetric flask pre-added with 50 mL of 0.1 mol / L iodine standard solution and 30-50 mL of ultrapure water to obtain a catalyst liquid to be measured, add 2 mL of 50% hydrochloric acid solution to the catalyst liquid to be measured, mix and place at 25°C in the dark for 5 min to obtain a catalyst liquid sample to be titrated, use a 0.1 mol / L sodium thiosulfate standard solution to titrate the catalyst liquid sample to be titrated until it turns light yellow, then add 3 mL starch indicator is titrated continuously until the blue color disappears, which is the end point. At the same time, a blank experiment is performed to calculate the content of anhydrous sodium sulfite: the percentage of anhydrous sodium sulfite = the difference between the volume of sodium thiosulfate standard solution consumed by the blank and the volume of sodium thiosulfate standard solution consumed by the sample × the concentration of sodium thiosulfate standard solution × 0.06302 / the mass of the sample × 100%. The consumed part is replenished in time to obtain the composite new wheat straw pulping catalyst, which acts on the next round of graded pre-soaking;
[0070] Step 3: catalytic heating: put the wheat straw soaked with the catalyst prepared in step 1 into the catalytic reaction tank, and naturally ferment and heat it to 85°C for 15 hours to obtain softened wheat straw fiber raw material;
[0071] Step 4: Put the softened wheat straw fiber raw material prepared in step 3 into an oblique kneading machine with a power of 10 kW, a main shaft speed of 2800 r / min, a kneading length of 100 mm, a range of 8000 mm, rub and separate the fibers, and then use a high-concentration pulping machine with a power of 50 kW, a pulping temperature of 34°C, and a pulping time of 2.6 h to obtain golden wheat straw pulp;
[0072] Step 5: brooming and screening. The golden straw pulp prepared in step 4 is further processed. The golden straw pulp is put into the decomposition tank for full swelling. The swelling temperature is 36°C and the swelling time is 3 h. Then it is refined by two medium-concentration pulping machines with a power of 30 kW, a pulping temperature of 35°C and a pulping time of 3 h. It is screened by an outflow corrugated screen with a power of 45 kW, a pulping pressure of 0.25 MPa and a sieve hole specification of 2.4 mm. The qualified straw pulp is collected in the refined pulp bin. The qualified straw pulp has a beating degree of 40°SR and a wet weight of 3.0 g. The unqualified straw pulp is returned to the decomposition tank.
[0073] Step 6: The qualified wheat straw pulp prepared in step 5 is fully mixed with pure domestic waste paper pulp in a mixing bin at a blending ratio of 30%. The mixing temperature is 40°C, the mixing speed is 800 r / min, the mixing time is 2.8 h, and the pump is sent to a 4400 / 500 long-net multi-cylinder papermaking machine with a power of 180 kW, a working speed of 300 m / min, a dynamic balance speed of 500 m / min, and a working pressure of 0.8 MPa to obtain a quantitative of 120 g / m 2 Ultra-high-strength corrugated paper.
[0074] Example 4: This example provides a preparation and application method of a novel wheat straw pulping catalyst, wherein the novel wheat straw pulping catalyst comprises the following components in parts by weight:
[0075] 43 parts of anhydrous sodium sulfite, 19 parts of methyl hydroxyethyl cellulose, 7 parts of sodium dodecyl sulfate, 2.2 parts of glucan exo-onuclease, 4 parts of lignin peroxidase, 0.35 parts of isothiazolinone fungicide, and 20 parts of ultrapure water.
[0076] This embodiment also provides a method for preparing a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0077] S1. Weigh appropriate weight portions of anhydrous sodium sulfite, methyl hydroxyethyl cellulose, sodium dodecyl sulfate, cellulase, lignin degradation agent, preservative and fungicide, and ultrapure water, put them into a catalyst preparation tank, and stir to mix at a stirring temperature of 23° C., a stirring speed of 1050 r / min, and a stirring time of 1.5 h to obtain an initial liquid catalyst;
[0078] S2. Using 7 mol / L sodium hydroxide solution and 7 mol / L hydrochloric acid solution, the final pH of the initial liquid catalyst obtained in S1 was adjusted to 7 to obtain a novel wheat straw pulping catalyst.
[0079] This embodiment also provides an application method of a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0080] Step 1: pre-impregnation by graded method: the new wheat straw pulping catalyst and wheat straw are put into a double-screw stirrer in a weight ratio of 1:45, the pre-impregnation temperature is 33°C, the pre-impregnation time is 25 hours, and the catalyst-impregnated wheat straw and the remaining new wheat straw pulping catalyst are obtained;
[0081] Step 2, efficient compounding, after the pre-immersion is completed, measure the content of anhydrous sodium sulfite in the remaining novel wheat straw pulping catalyst obtained in step 1, quickly weigh 0.25 kg of the remaining novel wheat straw pulping catalyst after the pre-immersion is completed, accurate to 0.0001 g, and place the remaining novel wheat straw pulping catalyst in a 250 mL iodine volumetric flask pre-added with 50 mL of 0.1 mol / L iodine standard solution and 30-50 mL of ultrapure water to obtain a catalyst liquid to be measured, add 2 mL of 50% hydrochloric acid solution to the catalyst liquid to be measured, mix and place at 25°C in the dark for 5 min to obtain a catalyst liquid sample to be titrated, use a 0.1 mol / L sodium thiosulfate standard solution to titrate the catalyst liquid sample to be titrated until it turns light yellow, then add 3 mL starch indicator is titrated continuously until the blue color disappears, which is the end point. At the same time, a blank experiment is performed to calculate the content of anhydrous sodium sulfite: the percentage of anhydrous sodium sulfite = the difference between the volume of sodium thiosulfate standard solution consumed by the blank and the volume of sodium thiosulfate standard solution consumed by the sample × the concentration of sodium thiosulfate standard solution × 0.06302 / the mass of the sample × 100%. The consumed part is replenished in time to obtain the composite new wheat straw pulping catalyst, which acts on the next round of graded pre-soaking;
[0082] Step 3: catalytic heating: put the wheat straw soaked with the catalyst prepared in step 1 into the catalytic reaction tank, and naturally ferment and heat it to 75°C for 13 hours to obtain softened wheat straw fiber raw material;
[0083] Step 4: Put the softened wheat straw fiber raw material prepared in step 3 into an oblique silk kneading machine with a power of 7 kW, a main shaft speed of 1800 r / min, a silk kneading length of 85 mm, a range of 5000 mm, rub and separate the silk, and then use a high-concentration pulping machine with a power of 35 kW, a pulping temperature of 29°C, and a pulping time of 1.7 h to obtain golden wheat straw pulp;
[0084] Step 5: brooming and screening. The golden straw pulp prepared in step 4 is further processed. The golden straw pulp is put into the decomposition tank for full swelling. The swelling temperature is 32°C and the swelling time is 2.3 h. Then it is refined by two medium-concentration pulping machines with a power of 22 kW, a pulping temperature of 32°C and a pulping time of 1.8 h. It is screened by an outflow corrugated screen with a power of 28 kW, a pulping pressure of 0.18 MPa and a sieve hole specification of 1.8 mm. The qualified straw pulp is collected in the refined pulp bin. The qualified straw pulp has a beating degree of 37°SR and a wet weight of 2.7 g. The unqualified straw pulp is returned to the decomposition tank.
[0085] Step 6: The qualified wheat straw pulp prepared in step 5 is fully mixed with pure domestic waste paper pulp in a mixing bin at a blending ratio of 15%. The mixing temperature is 34°C, the mixing speed is 650 r / min, the mixing time is 2.2 h, and the pump is a 4400 / 500 long-net multi-cylinder papermaking machine with a power of 160 kW, a working speed of 230 m / min, a dynamic balance speed of 440 m / min, and a working pressure of 0.65 MPa. The quantitative value is 90 g / m 2 Ultra-high-strength corrugated paper.
[0086] Example 5: This example provides a preparation and application method of a novel wheat straw pulping catalyst, wherein the novel wheat straw pulping catalyst comprises the following components in parts by weight:
[0087] 48 parts of anhydrous sodium sulfite, 21 parts of methyl hydroxyethyl cellulose, 9 parts of sodium dodecyl sulfate, 2.8 parts of glucan exo-onuclease, 10 parts of lignin peroxidase, 0.5 parts of isothiazolinone fungicide, and 30 parts of ultrapure water.
[0088] This embodiment also provides a method for preparing a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0089] S1. Weigh appropriate weight portions of anhydrous sodium sulfite, methyl hydroxyethyl cellulose, sodium dodecyl sulfate, cellulase, lignin degradation agent, preservative and fungicide, and ultrapure water, put them into a catalyst preparation tank, and stir to mix them at a stirring temperature of 28° C., a stirring speed of 1160 r / min, and a stirring time of 1.9 h to obtain an initial liquid catalyst;
[0090] S2. Using 9 mol / L sodium hydroxide solution and 9 mol / L hydrochloric acid solution, the final pH of the initial liquid catalyst obtained in S1 was adjusted to 7.8 to obtain a novel wheat straw pulping catalyst.
[0091] This embodiment also provides an application method of a novel wheat straw pulping catalyst, which specifically comprises the following steps:
[0092] Step 1: pre-impregnation by graded method: the new wheat straw pulping catalyst and wheat straw are put into a double-screw stirrer in a weight ratio of 1:55, the pre-impregnation temperature is 38°C, the pre-impregnation time is 27 hours, and the catalyst-impregnated wheat straw and the remaining new wheat straw pulping catalyst are obtained;
[0093] Step 2, efficient compounding, after the pre-immersion is completed, measure the content of anhydrous sodium sulfite in the remaining novel wheat straw pulping catalyst obtained in step 1, quickly weigh 0.25 kg of the remaining novel wheat straw pulping catalyst after the pre-immersion is completed, accurate to 0.0001 g, and place the remaining novel wheat straw pulping catalyst in a 250 mL iodine volumetric flask pre-added with 50 mL of 0.1 mol / L iodine standard solution and 30-50 mL of ultrapure water to obtain a catalyst liquid to be measured, add 2 mL of 50% hydrochloric acid solution to the catalyst liquid to be measured, mix and place at 25°C in the dark for 5 min to obtain a catalyst liquid sample to be titrated, use a 0.1 mol / L sodium thiosulfate standard solution to titrate the catalyst liquid sample to be titrated until it turns light yellow, then add 3 mL starch indicator is titrated continuously until the blue color disappears, which is the end point. At the same time, a blank experiment is performed to calculate the content of anhydrous sodium sulfite: the percentage of anhydrous sodium sulfite = the difference between the volume of sodium thiosulfate standard solution consumed by the blank and the volume of sodium thiosulfate standard solution consumed by the sample × the concentration of sodium thiosulfate standard solution × 0.06302 / the mass of the sample × 100%. The consumed part is replenished in time to obtain the composite new wheat straw pulping catalyst, which acts on the next round of graded pre-soaking;
[0094] Step 3: catalytic heating: put the wheat straw soaked with the catalyst prepared in step 1 into the catalytic reaction tank, and naturally ferment and heat it to 83°C for 14.5 hours to obtain softened wheat straw fiber raw material;
[0095] Step 4: Put the softened wheat straw fiber raw material prepared in step 3 into an oblique kneading machine with a power of 9 kW, a main shaft speed of 2500 r / min, a kneading length of 95 mm, a range of 7000 mm, rub and separate the fibers, and then use a high-concentration pulping machine with a power of 45 kW, a pulping temperature of 32°C, and a pulping time of 2.4 h to obtain golden wheat straw pulp;
[0096] Step 5: brooming and screening. The golden straw pulp prepared in step 4 is further processed. The golden straw pulp is put into the decomposition tank for full swelling. The swelling temperature is 34°C and the swelling time is 2.8 h. Then it is refined by two medium-concentration pulping machines with a power of 28 kW, a pulping temperature of 34°C and a pulping time of 2.8 h. It is screened by an outflow corrugated screen with a power of 38 kW, a pulping pressure of 0.23 MPa and a sieve hole specification of 2.2 mm. The qualified straw pulp is collected in the refined pulp bin. The qualified straw pulp has a beating degree of 39°SR and a wet weight of 2.9 g. The unqualified straw pulp is returned to the decomposition tank.
[0097] Step 6: The qualified wheat straw pulp prepared in step 5 is fully mixed with pure domestic waste paper pulp in a mixing bin at a blending ratio of 22%. The mixing temperature is 38°C, the mixing speed is 750 r / min, the mixing time is 2.6 h, and the pump is a 4400 / 500 long-net multi-cylinder papermaking machine with a power of 175 kW, a working speed of 280 m / min, a dynamic balance speed of 480 m / min, and a working pressure of 0.75 MPa. The quantitative value is 110 g / m 2 Ultra-high-strength corrugated paper.
[0098] Comparative Example 1: This comparative example provides a method for preparing corrugated base paper, which specifically comprises the following steps:
[0099] 100 parts by weight of pure domestic waste pulp was pumped to a 4400 / 500 fourdrinier multi-cylinder papermaking machine with a power of 150 kW, a working speed of 200 m / min, a dynamic balance speed of 400 m / min, and a working pressure of 0.6 MPa to prepare a paper with a basis weight of 103 g / m 2 Corrugated paper.
[0100] Experimental Example 1: Tests for measuring the paper tensile index, folding index, ring crush index and sizing degree.
[0101] The ultra-high-strength corrugated base paper prepared in Example 1, Example 2, Example 3, Example 4, and Example 5 and the corrugated base paper prepared in Comparative Example 1 were tested, specifically comprising the following steps:
[0102] (1) Select the ultra-high-strength corrugated paper prepared in Examples 1-5 and the corrugated paper prepared in Comparative Example 1, and use paper strip samples with a length and width of 15 mm. Each paper strip sample needs 3 repetitions;
[0103] (2) Clamp the paper strip samples of Examples 1-5 and Comparative Example 1 between two clamps;
[0104] (3) Use a pendulum to apply a load on the paper strip, causing it to break. The load on the paper strip when it breaks is the tensile force, which is calculated according to the formula: tensile index (Nm / g) = tensile force × 100 ÷ (sample weight × sample width);
[0105] (4) Using a folding endurance meter, the folding endurance of the ultra-high-strength corrugated paper prepared in Examples 1-5 and the corrugated paper prepared in Comparative Example 1, with the length and width of the paper strip samples being 15 mm, was measured and the data was recorded;
[0106] (5) The ultra-high-strength corrugated base paper prepared in Examples 1-5 and the corrugated base paper prepared in Comparative Example 1, with a length and width of 15 mm, were inserted into the sample holder to form a ring shape, and then placed on the pressing plate of the compression instrument for electric uniform compression. The value displayed when the paper strip sample is crushed is the ring compression strength. The ring compression index is calculated according to the formula: Ring compression index (Nm / g) = 1000 × ring compression strength / quantitative weight of paper strip sample;
[0107] (6) Place the ultra-high-strength corrugated paper prepared in Examples 1-5 and the corrugated paper prepared in Comparative Example 1 on a glass plate, and place a scriber at a 45° angle to the glass plate to quickly and lightly draw a straight line;
[0108] (7) After the ink begins to spread and penetrate, continue to adjust (increase) the width of the pen until the ink stops spreading and penetrating.
[0109] (8) After the paper strips are naturally air-dried, they are compared with transparent standard width sheets. The maximum width of the lines without diffusion and penetration is the sizing degree of the finished paper.
[0110] Result analysis:
[0111] Figure 1 The tensile index measurement results of the ultra-high strength corrugated base paper prepared in Examples 1-5 of the present invention and the corrugated base paper prepared in Comparative Example 1 are shown in the figure. As shown in the figure, the tensile indexes of the ultra-high strength corrugated base paper prepared in Examples 1-5 are 23.3 Nm / g, 25 Nm / g, 33 Nm / g, 23 Nm / g, and 31 Nm / g, while the tensile index of the corrugated base paper prepared in Comparative Example 1 is 19 Nm / g, indicating that the addition of the qualified wheat straw pulp of the present invention greatly improves the tensile strength of the prepared ultra-high strength corrugated base paper.
[0112] Figure 2 The ultra-high-strength corrugated base paper prepared in Examples 1-5 of the present invention and the folding index test result of the corrugated base paper prepared in Comparative Example 1 are shown in the figure. The folding index of the ultra-high-strength corrugated base paper prepared in Examples 1-5 is 1.62 kPa.m 2 / g, 2.21 kPa.m 2 / g, 2.52 kPa.m 2 / g, 1.86 kPa.m 2 / g, 2.43 kPa.m 2 / g, while the folding index of the corrugated base paper prepared in Comparative Example 1 is 1.54 kPa.m 2 / g, indicating that the addition of the qualified wheat straw pulp of the present invention improves the folding resistance of the ultra-high-strength corrugated base paper.
[0113] Figure 3 The ring crush index measurement results of the ultra-high strength corrugated base paper prepared in Examples 1-5 of the present invention and the corrugated base paper prepared in Comparative Example 1 are shown in the figure. As shown in the figure, the ring crush index of the ultra-high strength corrugated base paper prepared in Examples 1-5 is 6.1 Nm / g, 7.5 Nm / g, 8.71 Nm / g, 6.92 Nm / g, and 8.36 Nm / g, while the ring crush index of the corrugated base paper prepared in Comparative Example 1 is 5.51 Nm / g, indicating that the addition of the qualified wheat straw pulp of the present invention greatly improves the ring crush index of the prepared ultra-high strength corrugated base paper.
[0114] Figure 4 The ultra-high-strength corrugated base paper prepared in Examples 1-5 of the present invention and the corrugated base paper prepared in Comparative Example 1 are shown in the sizing degree measurement results. As shown in the figure, the sizing degrees of the ultra-high-strength corrugated base paper prepared in Examples 1-5 are 0.62 mm, 0.56 mm, 0.27 mm, 0.66 mm, and 0.46 mm, while the sizing degree of the corrugated base paper prepared in Comparative Example 1 is 0.8 mm. When the sizing degree is too high, the paper fiber will become brittle and the prepared product will be easily damaged. Therefore, the quality of the ultra-high-strength corrugated base paper prepared in Examples 1-5 is significantly better than that of the corrugated base paper prepared in Comparative Example 1, indicating that the obtained qualified wheat straw pulp fiber has high strength and good toughness, and has significant advantages in the papermaking of ultra-high-strength corrugated base paper.
[0115] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
[0116] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.
Claims
1. A method for applying a novel wheat straw pulping catalyst, characterized in that: The raw materials for preparing the novel wheat straw pulping catalyst are the following components in parts by weight: 40-50 parts of anhydrous sodium sulfite, 18-22 parts of methyl hydroxyethyl cellulose, 6-10 parts of sodium dodecyl sulfate, 2-3 parts of cellulase, 1-12 parts of lignin degradation agent, 0.3-0.6 parts of preservative and fungicide, 8-35 parts of ultrapure water; The cellulase is exoglucanase; the lignin degradation agent is lignin peroxidase; the preservative fungicide is isothiazolinone fungicide; The preparation method of the novel wheat straw pulping catalyst specifically comprises the following steps: S1. Weigh appropriate weight portions of anhydrous sodium sulfite, methyl hydroxyethyl cellulose, sodium dodecyl sulfate, cellulase, lignin degradation agent, preservative and fungicide, and ultrapure water, put them into a catalyst preparation tank, and stir to mix at a stirring temperature of 20-30° C., a stirring speed of 1000-1200 r / min, and a stirring time of 1.25-2 h to obtain an initial liquid catalyst; S2, using a 5-10 mol / L sodium hydroxide solution and a 5-10 mol / L hydrochloric acid solution to adjust the final pH of the initial liquid catalyst obtained in S1 to 6.5-8.0, to obtain a novel wheat straw pulping catalyst; The application method of the novel wheat straw pulping catalyst specifically comprises the following steps: Step 1: Pre-impregnation by grading, placing the novel wheat straw pulping catalyst and wheat straw into a double-screw stirrer for pre-impregnation, obtaining wheat straw impregnated with the catalyst and the remaining novel wheat straw pulping catalyst; Step 2: Efficient compounding: after the pre-impregnation is completed, the content of anhydrous sodium sulfite in the remaining novel wheat straw pulping catalyst obtained in step 1 is measured, and the consumed part is replenished in time to obtain a compounded novel wheat straw pulping catalyst, which acts on the next round of graded pre-impregnation; Step 3: catalytic heating: put the wheat straw soaked with the catalyst prepared in step 1 into the catalytic reaction tank, and naturally ferment and heat it to 70-85°C for 12-15 hours to obtain softened wheat straw fiber raw material; Step 4: Put the softened wheat straw fiber raw material prepared in step 3 into an oblique kneading machine for rubbing and separating, and then use a high-concentration pulping machine to obtain golden wheat straw pulp; Step 5: beating and screening. The golden straw pulp prepared in step 4 is further processed. The golden straw pulp is put into a decomposition tank for full swelling. Then, it is refined by two medium-concentration pulping machines and screened by an outflow corrugated screen. The qualified straw pulp is collected in a refined pulp bin. The qualified straw pulp has a beating degree of 35-40°SR and a wet weight of 2.6-3.0 g. The unqualified straw pulp is returned to the decomposition tank. Step 6: The qualified wheat straw pulp prepared in step 5 is mixed with pure domestic waste paper pulp in a mixing bin at a blending ratio of 10-30%, and pumped to a 4400 / 500 long-net multi-cylinder papermaking machine to obtain a quantitative 80-120 g / m 2 Ultra-high-strength corrugated paper; In step 1, the novel wheat straw pulping catalyst and wheat straw are put into the mixture in a weight ratio of 1:40-60; the pre-soaking temperature of the double-screw stirrer is 30-40° C., and the pre-soaking time is 24-28 h; In step 2, the determination of the content of anhydrous sodium sulfite specifically includes the following steps: L1. Quickly weigh 0.25 kg of the new wheat straw pulping catalyst remaining after pre-soaking, accurate to 0.0001 g; L2, place the remaining novel wheat straw pulping catalyst obtained in L1 into a 250 mL iodine volumetric flask pre-added with 50 mL of 0.1 mol / L iodine standard solution and 30-50 mL of ultrapure water to obtain a catalyst liquid to be measured; L3, add 2 mL of 50% hydrochloric acid solution to the catalyst liquid to be measured obtained in L2, mix and place at 25°C in the dark for 5 min to obtain a catalyst liquid sample to be titrated; L4. Use 0.1 mol / L sodium thiosulfate standard solution to titrate the catalyst liquid sample obtained in L3 until it turns light yellow. Add 3 mL of starch indicator and continue titrating until the blue color disappears, which is the end point. At the same time, perform a blank experiment and calculate the content of anhydrous sodium sulfite: the percentage of anhydrous sodium sulfite = the difference between the volume of sodium thiosulfate standard solution consumed by the blank and the volume of sodium thiosulfate standard solution consumed by the sample × the concentration of sodium thiosulfate standard solution × 0.06302 / the mass of the sample × 100%; In step 4, the power of the oblique silk kneading machine is 6-10 kW, the main shaft speed is 1680-2800 r / min, the silk kneading length is 80-100 mm, and the range is 4000-8000 mm; the power of the high-concentration pulping machine is 30-50 kW, the pulping temperature is 28-34°C, and the pulping time is 1.5-2.6 h; In step 5, the swelling temperature of the decomposition tank is 30-36°C, and the swelling time is 2-3 h; the power of the medium-concentration refiner is 20-30 kW, the refining temperature is 30-35°C, and the refining time is 1.5-3 h; the power of the outflow corrugated screen is 22-45 kW, the pulp inlet pressure is 0.1-0.25 MPa, and the screen hole specification is 1.2-2.4 mm; In step six, the mixing temperature of the mixing bin is 30-40°C, the mixing speed is 600-800 r / min, and the mixing time is 2-2.8 h; the power of the fourdrinier multi-cylinder papermaking machine is 150-180 kW, the working speed is 200-300 m / min, the dynamic balance speed is 400-500 m / min, and the working pressure is 0.6-0.8 MPa.