A phosphate polymer quasi-solid electrolyte, in-situ solidification preparation method and application

Through the in-situ solidification preparation method of phosphate polymer quasi-solid electrolyte, the battery safety problem is solved, and a quasi-solid electrolyte with high ionic conductivity and stability is achieved, which significantly improves the safety performance and cycle stability of the battery.

CN117895064BActive Publication Date: 2024-11-19SHENZHEN UNIV
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202311594392.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2023-11-27
Publication Date
2024-11-19
Estimated Expiration
2043-11-27

AI Technical Summary

Technical Problem

The safety problems of existing batteries have not been completely solved, especially the frequent battery safety accidents caused by the use of highly flammable organic electrolytes. The existing methods only reduce the risk of thermal runaway in the electrode materials to a certain extent, and fail to completely solve the battery. Security issues.

Method used

Using a in-situ solidification preparation method of phosphate polymer quasi-solid electrolyte, the reaction of cyclochlorophosphate monomer and hydroxyl-containing functional monomer under the action of acid binding agent, combined with cosolvents, initiators and Crosslinking agent, forming a crosslinked polymer quasi-solid electrolyte with high thermal stability and electrochemical stability.

Benefits of technology

Quasosolid electrolytes with high ionic conductivity, low interfacial impedance, stability and electrochemical stability have been achieved, which significantly improves the safety performance and cycle stability of the battery, reduces the crystallinity of the material, and has a wider range of applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117895064B_ABST
    Figure CN117895064B_ABST
Patent Text Reader

Abstract

The present invention provides a quasi-solid electrolyte of a phosphate polymer, an in-situ solidification preparation method and application, wherein a phosphate monomer is prepared by an esterification reaction between a cyclic chlorophosphate monomer and a monomer containing a hydroxyl functional unit; then the phosphate monomer, an initiator, a cross-linking agent and a lithium salt are added to a cosolvent and stirred until uniform, thereby obtaining a quasi-solid electrolyte precursor liquid; then the quasi-solid electrolyte precursor liquid is allowed to stand, so that the quasi-solid precursor liquid undergoes ring-opening polymerization to obtain a cross-linked polymer quasi-solid electrolyte. The present invention improves the thermal stability of the cross-linked polymer quasi-solid electrolyte, reduces the crystallinity of the polymer matrix, and finally obtains a quasi-solid polymer electrolyte with high ionic conductivity, low interfacial impedance, high stability and electrochemical stability, which can not only effectively improve the safety performance of the battery, but also has excellent positive and negative electrode combination capabilities, and can significantly improve the comprehensive performance of the secondary battery cycle and energy storage.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of new energy materials, and in particular to a phosphate polymer quasi-solid electrolyte, an in-situ solidification preparation method and an application in the preparation of secondary batteries. Background Art

[0002] In recent years, people have made considerable efforts to solve the battery safety problem, including using special diaphragm materials, adding various reagents such as overcharge protection agents, adding external safety control systems, etc. However, these methods cannot really solve the battery safety problem, but only reduce the thermal runaway risk of electrode materials to a certain extent. As long as highly flammable organic electrolytes are used, battery safety accidents will continue to occur. Summary of the invention

[0003] The first object of the present invention is to provide an in-situ preparation method of a quasi-solid polymer electrolyte with high thermal stability and electrochemical stability in view of the problems existing in the background technology.

[0004] To this end, the above-mentioned purpose of the present invention is achieved through the following technical solutions:

[0005] A method for preparing a quasi-solid electrolyte of a phosphate polymer by in-situ solidification, comprising the following steps:

[0006] S1, the compound of formula I (cyclic chlorophosphate monomer) and the monomer containing hydroxyl functional unit react in an organic solvent under the action of an acid binding agent to prepare a phosphate monomer;

[0007]

[0008] In the formula: R1 is H or an alkane group; R2 is H or an alkane group;

[0009] The synthesis temperature of the phosphate monomer is -50°C to 60°C, and the reaction time is 0.5h to 72h;

[0010] S2, mixing the phosphate monomer, cosolvent, initiator, crosslinking agent and lithium salt obtained in step S1 in a certain proportion, stirring evenly, to obtain a quasi-solid electrolyte precursor liquid;

[0011] S3, allowing the quasi-solid electrolyte precursor liquid obtained in step S2 to stand to obtain a cross-linked polymer quasi-solid electrolyte;

[0012] The standing temperature is 15°C to 60°C, and the standing time is 0.5h to 72h.

[0013] While adopting the above technical solutions, the present invention may also adopt or combine the following technical solutions:

[0014] As a preferred technical solution of the present invention: the monomer containing hydroxyl functional unit includes: monohydric alcohol monomer and / or polyhydric alcohol monomer;

[0015] The monohydric alcohol monomer (carbon atom number ≤ 20) is methanol (CH3OH), ethanol (CH3CH2OH), propanol (CH3CH2CH2OH), isopropanol (CH3CH2(OH)CH3), glycidol (C3H6O2), triethylene glycol monomethyl ether (CH3OCH2CH2OCH2CH2OCH2CH2OH), 2,2,2-trifluoroethanol (CF3CH2OH), hexafluoroisopropanol ((CF3)2CHOH), 2,2,3,3,3-pentafluoro-1-propanol (HOCH2CF2CF3), 3-amino-2-fluoropropane-1-ol (NH2CH2CHFCH2OH), (3,3-difluorocyclopentane)methanol (HOCH2C5H7F2), citronellol ((CH3)2C=CHCH2CH2CH(CH3)CH2CH2OH), cinnamyl alcohol (C6H5CH=CHCH2OH), cyclohexanol (C6H 11 OH), diethylene glycol monoethyl ester (C2H5OCH2CH2OCH2CH2COOCH3), 2-hydroxyethyl acrylate (CH2=CHCOOCH2CH2OH), 2-hydroxyethyl acetate (CH3COOCH2CH2OH), phenol (C6H5OH), p-quinoline (CH3C6H4OH), 4-hydroxybenzonitrile (HOC6H4CN), trifluoromethylbenzyl alcohol (C6H5CH(OH)CF3), 1,1,1,3,3,3-hexafluoro-2-phenyl-2-propanol (C6H5CH(OH)(CF3)2), 1,1,1-trifluoro-2-phenyl-3-butene-2-ol (C6H5CH(OH)(CF3)2), 10 H9F3O), 4,4'-difluorobenzhamol (HOCH(C6H4F)2), 1-cyano-1-phenyl-2,2,2-trifluoroethanol (F3CC(CN)(C6H5)OH), 2-cyano-3-(4-hydroxyphenyl) ethyl acrylate (C 12 H 11 NO3), butoxycarbonyl-hydroxylated lysine (C 13 H 21 F3N2O5) at least one;

[0016] The polyol monomer (carbon number ≤ 20) is ethylene glycol (HOCH2CH2OH), 3,6-octanediol (CH3CH2CH(OH)CH2CH2CH(OH)CH2CH3), propylene glycol (HOCH2CH(OH)CH2OH), (2-hydroxyethyl)-β-cyclodextrin (C 56 H 98 O 42), 2-hydroxypropyl-β-cyclodextrin (C 63 H 112 O 42 ), (2-hydroxypropyl)-α-cyclodextrin (C 54 H 96 O 36 )、(2,6-di-O-)ethyl-β-cyclodextrin (C 70 H 126 O 35 )、2,2,3,3,4,4,5,5-octafluoro-1,6-hexanediol (HOCH2CF2CF2CF2CF2CH2OH), 1,3-bis(hexafluoro-α-hydroxyisopropyl)benzene (C 12 H6F 12 O2), pentaerythritol allyl ether (C(CH2OCH2CH=CH2) x (CH2OH) y )

[0017] The molar ratio of the compound of formula I to the hydroxyl functional group contained in the hydroxyl functional unit monomer is 10:1 to 1:10.

[0018] As a preferred technical solution of the present invention: the acid binding agent is triethylamine (TEA), diethylamine (C4H 11 At least one of ethylamine (C2H7N), pyridine (Py), N,N-diisopropylethylamine (DIPEA), 4-dimethylaminopyridine (DMAP), triethanolamine (TEA), tetrabutylammonium bromide (TBAB), ammonium carbonate ((NH4)2CO3), sodium carbonate (Na2CO3), and potassium carbonate (K2CO3);

[0019] The molar ratio of the compound of formula I to the acid binding agent is 1:1 to 1:10.

[0020] As a preferred technical solution of the present invention: the organic solvent is at least one of tetrahydrofuran (THF), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), dichloromethane (DCM), chloroform (CHCl3), toluene (C6H5CH3), petroleum ether, acetone (AC), methyl tert-butyl ether (MTBE), N-methylpyrrolidone (NMP) and ethyl acetate (EA);

[0021] The volume ratio of the volume of the organic solvent to the total volume of the compound of formula I and the monomer containing a hydroxyl functional unit is 100:1 to 1:1.

[0022] As a preferred technical solution of the present invention: the cosolvent is at least one of ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF), N-methylpyrrolidone (NMP), ethylene carbonate (EC), fluoroethylene carbonate (FEC), diethyl carbonate (DEC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC);

[0023] The volume ratio of the co-solvent to the phosphate ester monomer is 100:1 to 1:1.

[0024] As a preferred technical solution of the present invention: the initiator is at least one of lithium hexafluorophosphate (LiPF6), tin fluoride (SnF4), lithium difluorooxalatoborate (LiDFOB), magnesium trifluoromethanesulfonate (Mg(OTf)2), zinc trifluoromethanesulfonate (Zn(OTf)2), 1-hydroxycyclohexyl phenyl ketone, lithium tetrafluoroborate (LiBF4), tris(pentafluorophenyl) borane (TPFPB), lithium tetracyanoborate (LiTCB), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), Lewis acid and aluminum trifluoromethanesulfonate (Al(OTf)3);

[0025] The mass ratio of the compound of formula I to the initiator is 10:1 to 1:10.

[0026] As a preferred technical solution of the present invention: the cross-linking agent is an epoxy cross-linking agent and / or a polyhydroxy inorganic hybrid cross-linking agent;

[0027] The epoxy crosslinking agent is pentaerythritol glycidyl ether (C 17 H 28 O8), polyethylene glycol diglycidyl ether (C3H5O2-(C2H4O) n -C3H5O), glycerol diglycidyl ether (C9H 16 O5), propylene glycol triglycidyl ether (C 12 H 20 O6), dicyclopentadiene epoxy compound (C 10 H 12 O2), bisphenol A diglycidyl ether (C 21 H 24 O4), resorcinol diglycidyl ether (C 12 H 14 O4), 1,4-butanediol diglycidyl ether (C 10 H 18 O4), trimethylolpropane triglycidyl ether (C 15 H 26 O6), γ-glycidyl ether oxygen silyl propyl sesquioxane, 2,4,6,8-tetramethyl-2,4,6,8-tetra(propyl glycidyl ether) cyclotetrasiloxane (C28 H 56 O 12 Si4) at least one;

[0028] The polyhydroxy inorganic hybrid crosslinking agent is at least one of hydroxylated silica;

[0029] The mass ratio of the compound of formula I to the cross-linking agent is 10:1 to 1:10, and the content can be 0%.

[0030] As a preferred technical solution of the present invention: the lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium iodide (LiI), lithium bis(oxalatoborate) (LiBOB) and lithium hexafluoroarsenate (LiAsF6);

[0031] The mass ratio of the compound of formula I to the lithium salt is 20:1 to 1:10.

[0032] The second object of the present invention is to provide a phosphate ester cross-linked polymer quasi-solid electrolyte prepared by the in-situ solid-state preparation method of the phosphate ester polymer quasi-solid electrolyte described above.

[0033] Another object of the present invention is to provide an application of the aforementioned phosphate cross-linked polymer quasi-solid electrolyte in the preparation of lithium metal batteries.

[0034] The present invention provides a quasi-solid electrolyte of a phosphate polymer, an in-situ solidification preparation method and an application in the preparation of a secondary battery. A phosphate monomer is prepared by an esterification reaction between a cyclic chlorophosphate monomer and a monomer containing a hydroxyl functional unit; the phosphate monomer, an initiator, a crosslinking agent and a lithium salt are added to a cosolvent and stirred until uniform, thereby obtaining a quasi-solid electrolyte precursor liquid; and the quasi-solid electrolyte precursor liquid is allowed to stand, so that the quasi-solid precursor liquid undergoes ring-opening polymerization, thereby obtaining a cross-linked polymer quasi-solid electrolyte. The role of the phosphate in the phosphate polymer quasi-solid electrolyte obtained by the present invention is to be flame retardant and to improve ion transmission; the role of the monomer containing hydroxyl functional units is that the introduction of strong polar groups such as ether bonds can greatly improve the ion transmission rate, and the other is that the long chain helps to reduce the glass transition temperature of the material and improve the material application atmosphere; the addition of the initiator causes the new phosphate monomer to undergo in-situ ring-opening polymerization to form a linear polymer, and the added cross-linking agent is connected to the new phosphate monomer through the ring opening, further allowing the linear polymer to be cross-linked to form a complex three-dimensional inorganic cross-linking network, thereby improving the structural stability of the material; and the thermal stability of the cross-linked polymer quasi-solid electrolyte is improved through hybridization, the crystallinity of the polymer matrix is ​​reduced, and the ionic conductivity of the cross-linked polymer quasi-solid electrolyte is further improved, and finally a quasi-solid polymer electrolyte with high ionic conductivity, low interface impedance, high stability and electrochemical stability is obtained, which can not only effectively improve the safety performance of the battery, but also has excellent positive and negative electrode combination ability, and can significantly improve the comprehensive performance of the cycle and energy storage of the secondary battery. At the same time, the preparation method provided by the present invention has simple process, safe operation, high product purity, and low environmental pollution. It can utilize the existing liquid electrolyte production process without increasing equipment investment and has broad industrialization prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] Figure 1 This is a test diagram of the cycle performance of the battery prepared in Example 1.

[0036] Figure 2 This is a test diagram of the cycle performance of the battery prepared in Example 2.

[0037] Figure 3 This is a test diagram of the cycle performance of the battery prepared in Example 3.

[0038] Figure 4 This is a test diagram of the cycle performance of the battery prepared in the comparative example. DETAILED DESCRIPTION

[0039] A method for preparing a quasi-solid electrolyte of a phosphate polymer by in-situ solidification, comprising the following steps:

[0040] S1, the compound of formula I (cyclic chlorophosphate monomer) and the monomer containing hydroxyl functional unit react in an organic solvent under the action of an acid binding agent to prepare a phosphate monomer;

[0041]

[0042]

[0043] In the formula: R1 is H or an alkane group; R2 is H or an alkane group;

[0044] The synthesis temperature of the phosphate monomer is -50°C to 60°C, and the reaction time is 0.5h to 72h;

[0045] Hereinafter, taking R1 as H and R2 as H as an example, the reaction in step S1 is as follows:

[0046]

[0047] S2, mixing the phosphate monomer, cosolvent, initiator, crosslinking agent and lithium salt obtained in step S1 in a certain proportion, stirring evenly, to obtain a quasi-solid electrolyte precursor liquid;

[0048] S3, allowing the quasi-solid electrolyte precursor liquid obtained in step S2 to stand to obtain a cross-linked polymer quasi-solid electrolyte;

[0049] The standing temperature is 15℃~60℃, and the standing time is 0.5h~72h;

[0050] The reaction looks like this:

[0051]

[0052] The monomers containing hydroxyl functional groups include: monohydric alcohol monomers and / or polyhydric alcohol monomers;

[0053] Monohydric alcohol monomers (carbon atom number ≤ 20) are methanol (CH3OH), ethanol (CH3CH2OH), propanol (CH3CH2CH2OH), isopropanol (CH3CH2(OH)CH3), glycidol (C3H6O2), triethylene glycol monomethyl ether (CH3OCH2CH2OCH2CH2OCH2CH2OH), 2,2,2-trifluoroethanol (CF3CH2OH), hexafluoroisopropanol ((CF3)2CHOH), 2,2,3,3,3-pentafluoro-1-propanol (HOCH2CF2CF3), 3-amino-2-fluoropropane-1-ol (NH2CH2CHFCH2OH), (3,3-difluorocyclopentane)methanol (HOCH2C5H7F2), citronellol ((CH3)2C=CHCH2CH2CH(CH3)CH2CH2OH), cinnamyl alcohol (C6H5CH=CHCH2OH), cyclohexanol (C6H 11 OH), diethylene glycol monoethyl ester (C2H5OCH2CH2OCH2CH2COOCH3), 2-hydroxyethyl acrylate (CH2=CHCOOCH2CH2OH), 2-hydroxyethyl acetate (CH3COOCH2CH2OH), phenol (C6H5OH), p-quinoline (CH3C6H4OH), 4-hydroxybenzonitrile (HOC6H4CN), trifluoromethylbenzyl alcohol (C6H5CH(OH)CF3), 1,1,1,3,3,3-hexafluoro-2-phenyl-2-propanol (C6H5CH(OH)(CF3)2), 1,1,1-trifluoro-2-phenyl-3-butene-2-ol (C6H5CH(OH)(CF3)2), 10 H9F3O), 4,4'-difluorobenzhamol (HOCH(C6H4F)2), 1-cyano-1-phenyl-2,2,2-trifluoroethanol (F3CC(CN)(C6H5)OH), 2-cyano-3-(4-hydroxyphenyl) ethyl acrylate (C 12 H 11 NO3), butoxycarbonyl-hydroxylated lysine (C 13 H 21 F3N2O5) at least one;

[0054] Polyol monomers (carbon number ≤ 20) are ethylene glycol (HOCH2CH2OH), 3,6-octanediol (CH3CH2CH(OH)CH2CH2CH(OH)CH2CH3), propylene glycol (HOCH2CH(OH)CH2OH), (2-hydroxyethyl)-β-cyclodextrin (C 56 H 98 O 42 ), 2-hydroxypropyl-β-cyclodextrin (C 63 H 112 O 42 ), (2-hydroxypropyl)-α-cyclodextrin (C54 H 96 O 36 )、(2,6-di-O-)ethyl-β-cyclodextrin (C 70 H 126 O 35 )、2,2,3,3,4,4,5,5-octafluoro-1,6-hexanediol (HOCH2CF2CF2CF2CF2CH2OH), 1,3-bis(hexafluoro-α-hydroxyisopropyl)benzene (C 12 H6F 12 O2), pentaerythritol allyl ether (C(CH2OCH2CH=CH2) x (CH2OH) y )

[0055] The molar ratio of the compound of formula I to the hydroxyl functional group contained in the monomer containing a hydroxyl functional unit is 10:1 to 1:10.

[0056] The acid binding agent is triethylamine (TEA), diethylamine (C4H 11 At least one of ethylamine (C2H7N), pyridine (Py), N,N-diisopropylethylamine (DIPEA), 4-dimethylaminopyridine (DMAP), triethanolamine (TEA), tetrabutylammonium bromide (TBAB), ammonium carbonate ((NH4)2CO3), sodium carbonate (Na2CO3), and potassium carbonate (K2CO3);

[0057] The molar ratio of the compound of formula I to the acid binding agent is 1:1 to 1:10.

[0058] The organic solvent is at least one of tetrahydrofuran (THF), N,N-dimethylformamide (DMF), N,N-dimethylacetamide (DMAC), dichloromethane (DCM), chloroform (CHCl3), toluene (C6H5CH3), petroleum ether, acetone (AC), methyl tert-butyl ether (MTBE), N-methylpyrrolidone (NMP) and ethyl acetate (EA);

[0059] The volume ratio of the volume of the organic solvent to the total volume of the compound of formula I and the monomer containing a hydroxyl functional unit is 100:1 to 1:1.

[0060] The cosolvent is at least one of ethylene glycol dimethyl ether (DME), tetrahydrofuran (THF), N-methylpyrrolidone (NMP), ethylene carbonate (EC), fluoroethylene carbonate (FEC), diethyl carbonate (DEC), dimethyl carbonate (DMC) and ethyl methyl carbonate (EMC);

[0061] The volume ratio of the co-solvent to the phosphate ester monomer is 100:1 to 1:1.

[0062] The initiator is at least one of lithium hexafluorophosphate (LiPF6), tin fluoride (SnF4), lithium difluorooxalatoborate (LiDFOB), magnesium trifluoromethanesulfonate (Mg(OTf)2), zinc trifluoromethanesulfonate (Zn(OTf)2), 1-hydroxycyclohexylphenyl ketone, lithium tetrafluoroborate (LiBF4), tris(pentafluorophenyl)borane (TPFPB), lithium tetracyanoborate (LiTCB), 1,8-diazabicyclo[5.4.0]undec-7-ene (DBU), Lewis acid and aluminum trifluoromethanesulfonate (Al(OTf)3);

[0063] The mass ratio of the compound of formula I to the initiator is 10:1 to 1:10.

[0064] The crosslinking agent is an epoxy crosslinking agent and / or a polyhydroxy inorganic hybrid crosslinking agent;

[0065] The epoxy crosslinking agent is pentaerythritol glycidyl ether (C 17 H 28 O8), polyethylene glycol diglycidyl ether (C3H5O2-(C2H4O) n -C3H5O), glycerol diglycidyl ether (C9H 16 O5), propylene glycol triglycidyl ether (C 12 H 20 O6), dicyclopentadiene epoxy compound (C 10 H 12 O2), bisphenol A diglycidyl ether (C 21 H 24 O4), resorcinol diglycidyl ether (C 12 H 14 O4), 1,4-butanediol diglycidyl ether (C 10 H 18 O4), trimethylolpropane triglycidyl ether (C 15 H 26 O6), γ-glycidyl ether oxygen silyl propyl sesquioxane, 2,4,6,8-tetramethyl-2,4,6,8-tetra(propyl glycidyl ether) cyclotetrasiloxane (C 28 H 56 O 12 Si4) at least one;

[0066] The polyhydroxy inorganic hybrid crosslinking agent is at least one of hydroxylated silica;

[0067] The mass ratio of the compound of formula I to the cross-linking agent is 10:1 to 1:10.

[0068] The lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), lithium bis(fluorosulfonyl)imide (LiFSI), lithium iodide (LiI), lithium bis(oxalatoborate) (LiBOB) and lithium hexafluoroarsenate (LiAsF6);

[0069] The mass ratio of the compound of formula I to the lithium salt is 20:1 to 1:10.

[0070] The present invention also provides a phosphate ester cross-linked polymer quasi-solid electrolyte prepared by the in-situ solid-state preparation method of the phosphate ester polymer quasi-solid electrolyte described above.

[0071] The present invention also provides the use of the above-mentioned phosphate cross-linked polymer quasi-solid electrolyte in the preparation of lithium metal batteries.

[0072] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0073] In addition, the meaning of "and / or" appearing in the full text includes three parallel solutions. Taking "A and / or B" as an example, it includes solution A, solution B, or a solution that satisfies both A and B. In addition, the technical solutions between the various embodiments can be combined with each other, but it must be based on the ability of ordinary technicians in this field to implement. When the combination of technical solutions is contradictory or cannot be implemented, it should be deemed that such a combination of technical solutions does not exist and is not within the scope of protection required by the present invention. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0074] In order to enable the details and operations of the above-mentioned embodiments of the present invention to be clearly understood by those skilled in the art, as well as to significantly demonstrate the improved performance of the cross-linked polymer quasi-solid electrolyte and its preparation method and application in the embodiments of the present invention, the above-mentioned technical scheme is illustrated by multiple embodiments below.

[0075] Example 1

[0076] 1 mol of cyclic chloroethylene phosphate was slowly dripped into a mixed solution of 1 mol of diethylene glycol monoethyl ester, 0.8 mol of pyridine and 200 mL of ethyl acetate. The whole reaction was kept at -20°C and stirred for 12 hours.

[0077] 0.01 mol of the prepared novel phosphate monomer, 0.02 mol of lithium hexafluorophosphate (LiPF6) and 0.02 mol of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were added in batches into 10 mL of ethylene glycol dimethyl ether (DME), and the mixture was stirred evenly to obtain a quasi-solid electrolyte precursor solution;

[0078] Example 2

[0079] 1 mol of cyclic chloroethylene phosphate was slowly dripped into a mixed solution of 1 mol of diethylene glycol monoethyl ester, 0.8 mol of pyridine and 200 mL of ethyl acetate. The whole reaction was kept at -20°C and stirred for 12 hours.

[0080] 0.01 mol of the prepared novel phosphate monomer, 0.02 mol of lithium hexafluorophosphate (LiPF6), 0.02 mol of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI), and 4.1 wt.% of hydroxylated silicon dioxide were added in batches to 10 mL of ethylene glycol dimethyl ether (DME), and the mixture was mixed and stirred to obtain a quasi-solid electrolyte precursor solution;

[0081] Example 3

[0082] 1 mol of cyclic chloroethylene phosphate was slowly dripped into a mixed solution of 1 mol of diethylene glycol monoethyl ester, 0.8 mol of pyridine and 200 mL of ethyl acetate, and the entire reaction was kept at -20°C and stirred for 12 hours to obtain a new phosphate monomer;

[0083] 1 mol of cyclic chloroethylene phosphate was slowly dripped into a mixed solution of 1 mol of trifluoroethanol, 0.8 mol of pyridine and 200 mL of ethyl acetate, and the entire reaction was kept at -20°C and stirred for 12 hours to obtain a new fluorine-containing phosphate monomer;

[0084] 0.009 mol of the prepared novel phosphate monomer, 0.001 mol of the novel fluorine-containing phosphate monomer, 0.02 mol of lithium hexafluorophosphate (LiPF6) and 0.02 mol of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were added in batches into 10 mL of ethylene glycol dimethyl ether (DME), and the mixture was stirred evenly to obtain a quasi-solid electrolyte precursor solution;

[0085] Comparative Example

[0086] 1 mol of cyclic chloroethylene phosphate was slowly dripped into a mixed solution of 1 mol of diethylene glycol monoethyl ester, 0.8 mol of pyridine and 200 mL of ethyl acetate. The whole reaction was kept at -20°C and stirred for 12 hours.

[0087] 0.01 mol of the prepared novel phosphate monomer and 0.02 mol of lithium bis(trifluoromethanesulfonyl)imide (LiTFSI) were added into 10 mL of ethylene carbonate (EC), and the mixture was stirred to obtain an electrolyte precursor solution;

[0088] Furthermore, in order to verify the progress of the embodiments of the present invention, the following cycle performance tests were performed on each embodiment and comparative example:

[0089] 1) Cathode preparation

[0090] 0.4g lithium iron phosphate, 0.05g conductive carbon black, and 0.05g polyvinylidene fluoride were added to 1.4mL N-methylpyrrolidone (NMP), mixed and stirred at room temperature for 12h, and then coated on a 20mm thick aluminum foil, and vacuum dried at 80℃ for 12h. The electrode was cut into discs with a diameter of 14mm. The loading of active material lithium iron phosphate was 1.0mg cm –2 .

[0091] 2) Battery assembly

[0092] The electrolyte precursor liquid prepared in Examples 1-3 and the comparative example was assembled into batteries in the order of negative electrode shell, spring sheet, gasket, lithium metal, diaphragm, precursor liquid, positive electrode, and positive electrode shell. After assembly, the batteries were pressed and sealed. The batteries were left standing at room temperature for 24 hours to ensure that the precursor liquid was solidified in situ. After standing, a 0.2C rate performance test was performed. The test results are as follows: Figure 1-4 shown.

[0093] At 0.2C rate, refer to Figure 1-3 The polymer quasi-solid electrolyte batteries prepared in Examples 1-3 have excellent cycle performance. After 100 cycles, the capacities are 137.5 mAh / g, 119.2 mAh / g and 137.2 mAh / g, respectively. The capacity of the comparative example is 128.1 mAh / g after 100 cycles. Therefore, the cross-linked polymer quasi-solid electrolyte battery prepared in the present invention has excellent cycle stability and high capacity.

[0094] Example 1 A novel phosphate monomer was synthesized by esterification reaction using diethylene glycol monoethyl ester as a hydroxyl functional monomer. An equimolar amount of cyclochloroethylene phosphate was added to an ethyl acetate solution of diethylene glycol monoethyl ester, and the esterification reaction generated HCl. The acid-binding agent pyridine reacted with hydrochloric acid to form pyridine hydrochloride, and finally a novel phosphate monomer was synthesized. A linear polymer was synthesized by in situ ring-opening polymerization using LiPF6 as an initiator. LiPF6 was added to the novel phosphate monomer, and LiPF6 was partially decomposed into lithium fluoride and phosphorus pentafluoride. As a strong Lewis acid and a key initiator for polymerization, the above decomposition products enable it to proceed smoothly at room temperature; then phosphorus pentafluoride first combines with a small amount of water to form a complex, and then converts into an ion pair H + (PF5OH)-, becomes the initial active species of cationic polymerization, and triggers the ring opening of new phosphate monomers to become monomer active species; then the new phosphate monomer molecules continue to insert ion pairs to make the polymer chain grow; the introduction of co-solvents and lithium salts can make quasi-solid polymer electrolytes. Esterification reaction and in-situ ring-opening polymerization bring a large number of ether bonds. The presence of ether bonds greatly reduces the glass transition temperature and is conducive to the movement of polymer chains, which makes the polymer quasi-solid electrolyte behave as an amorphous electrolyte material with high ionic conductivity.

[0095] Example 2 A novel phosphate monomer was synthesized by esterification reaction using diethylene glycol monoethyl ester as a hydroxyl functional monomer. An equimolar amount of cyclochloroethylene phosphate was added to an ethyl acetate solution of diethylene glycol monoethyl ester, and the esterification reaction generated HCl. The acid-binding agent pyridine reacted with hydrochloric acid to form pyridine hydrochloride, and finally a novel phosphate monomer was synthesized. A cross-linked polymer network was synthesized by in situ ring-opening polymerization using LiPF6 as an initiator and hydroxylated silica as a cross-linking agent and cross-linking center. LiPF6 was added to the novel phosphate monomer, and LiPF6 was partially decomposed into lithium fluoride and phosphorus pentafluoride. As a strong Lewis acid and a key initiator for polymerization, the above decomposition products enable it to proceed smoothly at room temperature; then phosphorus pentafluoride first combines with a small amount of water to form a complex, and then converts into an ion pair H + (PF5OH) -, becoming the initial active species of cationic polymerization, and initiating the ring opening of new phosphate monomers to become monomer active species; then the new phosphate monomer molecules continue to insert ion pairs to make the polymer chain grow; then the hydroxylated silica (crosslinker) forms a unit structure by ring opening, so that multiple new phosphate monomers are connected to the hydroxylated silica to form a unit structure, and then countless units are connected to form a huge three-dimensional hybrid cross-linked network, which provides rigidity and high cycle stability for the prepared cross-linked polymer quasi-solid electrolyte; the introduction of cosolvents and lithium salts can make quasi-solid polymer electrolytes. Esterification reaction, in-situ ring-opening polymerization and cross-linking bring a large number of ether bonds. The presence of ether bonds greatly reduces the glass transition temperature, which is conducive to the movement of polymer chains, and thus makes the polymer quasi-solid electrolyte behave as an amorphous electrolyte material with high ionic conductivity.

[0096] Example 3 A novel phosphate monomer was synthesized by esterification reaction using diethylene glycol monoethyl ester as a hydroxyl functional monomer. An equimolar amount of cyclic chlorophosphate vinyl ester was added to an ethyl acetate solution of diethylene glycol monoethyl ester, and the esterification reaction generated HCl. The acid-binding agent pyridine reacted with hydrochloric acid to form pyridine hydrochloride, and finally a novel phosphate monomer was synthesized. And trifluoroethanol was used as a hydroxyl functional monomer, and a novel fluorine-containing phosphate monomer was synthesized by esterification reaction. An equimolar amount of cyclic chlorophosphate vinyl ester was added to an ethyl acetate solution of trifluoroethanol, and the esterification reaction generated HCl. The acid-binding agent pyridine reacted with hydrochloric acid to form pyridine hydrochloride, and finally a novel fluorine-containing phosphate monomer was synthesized. A linear polymer was synthesized by in situ ring-opening polymerization using LiPF6 as an initiator. LiPF6 was added to the novel phosphate monomer, and LiPF6 was partially decomposed into lithium fluoride and phosphorus pentafluoride. As a strong Lewis acid and a key initiator for polymerization, the above-mentioned decomposition products enable it to proceed smoothly at room temperature; then phosphorus pentafluoride first combines with a small amount of water to form a complex, and then converts into an ion pair H + (PF5OH) - , becoming the initial active species of cationic polymerization, and initiating the ring-opening of new phosphate monomers to become monomer active species; then the new phosphate monomer molecules continue to insert ion pairs to make the polymer chain grow; introducing cosolvents and lithium salts can make quasi-solid polymer electrolytes. Esterification reaction, in-situ ring-opening polymerization and cross-linking bring a large number of ether bonds. The presence of ether bonds greatly reduces the glass transition temperature and is conducive to the movement of polymer chains, thereby making the polymer quasi-solid electrolyte behave as an amorphous electrolyte material with high ionic conductivity.

[0097] In the comparative example, new phosphate monomers were added as additives to commercially available liquid electrolytes to explore the performance of batteries containing new un-ring-opened phosphate monomers. The experimental results show that some performance of batteries constructed with linear and cross-linked phosphates are better than those of monomer batteries with only additives, which reflects the advantages of in-situ ring-opening and cross-linking batteries.

[0098] The above are only preferred embodiments of the present invention, and do not limit the protection scope of the present invention. For those skilled in the art, the present invention may have various modifications and changes. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the patent protection scope of the present invention.

Claims

1. An in-situ solid-state preparation method for a phosphate polymer quasi-solid electrolyte, characterized in that: The in-situ solid-state preparation method comprises the following steps: S1, the compound of formula I and the monomer containing hydroxyl functional unit react in an organic solvent under the action of an acid binding agent to prepare a phosphate monomer; In the formula: R1 is H or an alkane group; R2 is H or an alkane group; The synthesis temperature of the phosphate monomer is -50°C to 60°C, and the reaction time is 0.5h to 72h; The monomers containing hydroxyl functional units include: monohydric alcohol monomers and / or polyhydric alcohol monomers; The molar ratio of the compound of formula I to the hydroxyl functional group contained in the hydroxyl functional unit monomer is 10:1 to 1:10; The acid binding agent is at least one of triethylamine, diethylamine, ethylamine, pyridine, N,N-diisopropylethylamine, 4-dimethylaminopyridine, triethanolamine, tetrabutylammonium bromide, ammonium carbonate, sodium carbonate, and potassium carbonate; The molar ratio of the compound of formula I to the acid binding agent is 1:1 to 1:10; The volume ratio of the volume of the organic solvent to the total volume of the compound of formula I and the monomer containing a hydroxyl functional unit is 100:1 to 1:1; S2, mixing the phosphate monomer, cosolvent, initiator, crosslinking agent and lithium salt obtained in step S1 in a certain proportion, stirring evenly, to obtain a quasi-solid electrolyte precursor liquid; The volume ratio of the cosolvent to the phosphate monomer is 100:1 to 1:1; The mass ratio of the compound of formula I to the initiator is 10:1 to 1:10; The mass ratio of the compound of formula I to the cross-linking agent is 10:1 to 1:10; The mass ratio of the compound of formula I to the lithium salt is 20:1 to 1:10; S3, allowing the quasi-solid electrolyte precursor liquid obtained in step S2 to stand to obtain a cross-linked polymer quasi-solid electrolyte; The standing temperature is 15°C to 60°C, and the standing time is 0.5h to 72h.

2. The in-situ solid-state preparation method of the phosphate polymer quasi-solid electrolyte according to claim 1, characterized in that: The monohydric alcohol monomer is methanol, ethanol, propanol, isopropanol, glycidol, triethylene glycol monomethyl ether, 2,2,2-trifluoroethanol, hexafluoroisopropanol, 2,2,3,3,3-pentafluoro-1-propanol, 3-amino-2-fluoropropane-1-ol, (3,3-difluorocyclopentane)methanol, citronellol, cinnamyl alcohol, cyclohexanol, diethylene glycol monoethyl ester, 2-hydroxyethyl acrylate, 2-hydroxyethyl acetate, phenol , at least one of p-quinone, 4-hydroxybenzonitrile, trifluoromethylbenzyl alcohol, 1,1,1,3,3,3-hexafluoro-2-phenyl-2-propanol, 1,1,1-trifluoro-2-phenyl-3-butene-2-ol, 4,4'-difluorobenzhydrol, 1-cyano-1-phenyl-2,2,2-trifluoroethanol, 2-cyano-3-(4-hydroxyphenyl)ethyl acrylate, and butoxycarbonyl-hydroxylated lysine; The polyol monomer is at least one of ethylene glycol, 3,6-octanediol, propylene glycol, (2-hydroxyethyl)-β-cyclodextrin, 2-hydroxypropyl-β-cyclodextrin, (2-hydroxypropyl)-α-cyclodextrin, (2,6-di-O-)ethyl-β-cyclodextrin, 2,2,3,3,4,4,5,5-octafluoro-1,6-hexanediol, 1,3-bis(hexafluoro-α-hydroxyisopropyl)benzene, and pentaerythritol allyl ether.

3. The in-situ solid-state preparation method of the phosphate polymer quasi-solid electrolyte according to claim 1, characterized in that: The organic solvent is at least one of tetrahydrofuran, N,N-dimethylformamide, N,N-dimethylacetamide, dichloromethane, chloroform, toluene, petroleum ether, acetone, methyl tert-butyl ether, N-methylpyrrolidone and ethyl acetate.

4. The in-situ solid-state preparation method of the phosphate polymer quasi-solid electrolyte according to claim 1, characterized in that: The cosolvent is at least one of ethylene glycol dimethyl ether, tetrahydrofuran, N-methyl pyrrolidone, ethylene carbonate, fluoroethylene carbonate, diethyl carbonate, dimethyl carbonate and ethyl methyl carbonate.

5. The in-situ solid-state preparation method of the phosphate polymer quasi-solid electrolyte according to claim 1, characterized in that: The initiator is at least one of lithium hexafluorophosphate, tin fluoride, lithium difluorooxalatoborate, magnesium trifluoromethanesulfonate, zinc trifluoromethanesulfonate, 1-hydroxycyclohexylphenyl ketone, lithium tetrafluoroborate, tris(pentafluorophenyl)borane, lithium tetracyanoborate, 1,8-diazabicyclo[5.4.0]undec-7-ene, Lewis acid and aluminum trifluoromethanesulfonate.

6. The in-situ solid-state preparation method of a phosphate polymer quasi-solid electrolyte according to claim 1, characterized in that: The crosslinking agent is an epoxy crosslinking agent and / or a polyhydroxy inorganic hybrid crosslinking agent; The epoxy crosslinking agent is at least one of pentaerythritol glycidyl ether, polyethylene glycol diglycidyl ether, glycerol diglycidyl ether, glycerol triglycidyl ether, dicyclopentadiene epoxy compound, bisphenol A diglycidyl ether, resorcinol diglycidyl ether, 1,4-butanediol diglycidyl ether, trimethylolpropane triglycidyl ether, γ-glycidyl ether oxygen silyl propyl sesquioxane, and 2,4,6,8-tetramethyl-2,4,6,8-tetra(propyl glycidyl ether) cyclotetrasiloxane; The polyhydroxy inorganic hybrid crosslinking agent is at least one of hydroxylated silicas.

7. The in-situ solid-state preparation method of a phosphate polymer quasi-solid electrolyte according to claim 1, characterized in that: The lithium salt is at least one of lithium bis(trifluoromethanesulfonyl)imide, lithium bis(fluorosulfonyl)imide, lithium iodide, lithium bis(oxalatoborate) and lithium hexafluoroarsenate.

8. A phosphate ester cross-linked polymer quasi-solid electrolyte prepared by the in-situ solid-state preparation method of a phosphate ester polymer quasi-solid electrolyte according to any one of claims 1 to 7.

9. Use of the phosphate cross-linked polymer quasi-solid electrolyte according to claim 8 in the preparation of lithium metal batteries.