A powder metallurgy material side bearing wear plate and preparation method thereof

By using high wear-resistant powder metallurgy materials, including copper powder, aluminum powder, tin powder, graphite and metal selenide, the side-bearing wear plate solves the problems of easy aging and poor wear resistance of nylon materials and achieves high wear resistance. Abrasiveness and stable friction coefficient extend service life and reduce replacement frequency.

CN117900485BActive Publication Date: 2024-10-01EAST CHINA JIAOTONG UNIVERSITY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410141818.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-01
Publication Date
2024-10-01
Estimated Expiration
2044-02-01

AI Technical Summary

Technical Problem

Nylon, the material of the side bearing wear plate of the current railway freight cars, cannot balance the friction coefficient and wear resistance, resulting in a short service life and easy aging. It is also greatly affected by ambient temperature and humidity, leading to deformation and damage.

Method used

High wear-resistant powder metallurgy materials are used, including copper powder, aluminum powder, tin powder, graphite, metal selenide and boron carbide, and are sintered through the powder metallurgy process to form a side bearing wear plate to improve the structural strength and wear resistance. Add graphite and Metal selenide improves wear resistance, and boron carbide increases friction and resists sticking.

Benefits of technology

It significantly improves the wear resistance and service life of the side bearing wear plate, reduces the wear rate, ensures stable performance under different environmental conditions, extends the replacement frequency, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117900485B_ABST
    Figure CN117900485B_ABST
Patent Text Reader

Abstract

The present invention discloses a side bearing wear plate made of a highly wear-resistant powder metallurgy material and a preparation method thereof, and belongs to the technical field of railway vehicle equipment. The side bearing wear plate made of a highly wear-resistant powder metallurgy material of the present invention comprises the following raw materials in parts by weight: 62 to 87 parts of copper powder, 3 to 8 parts of aluminum powder, 2 to 5 parts of tin powder, 5 to 15 parts of graphite, 2 to 6 parts of metal selenide, and 1 to 4 parts of boron carbide. The side bearing wear plate made of a highly wear-resistant powder metallurgy material of the present invention has the characteristics of good wear resistance, high temperature resistance, high strength, good mechanical properties, long service life, etc., and the performance of the side bearing wear plate of the present invention is less affected by the service conditions, and can ensure that the use performance of the side bearing wear plate is not affected when the external environment changes greatly.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of railway vehicle equipment, and in particular to a side bearing wear plate made of a high-wear-resistant powder metallurgy material and a preparation method thereof. Background Art

[0002] Railway freight car side bearing wear plates are used on the two springs of railway freight car bogies as the contact surface between the carriage and the bogie, increasing the rotational resistance torque between the bogie and the car body. Its use nature requires that it must have a sufficiently large friction coefficient to reduce the lateral acceleration of the bogie, ensure that the vehicle does not move in a serpentine manner, and ensure driving safety. The material of the current railway freight car side bearing wear plates is basically nylon, which is difficult to meet the requirements of friction coefficient and wear resistance at the same time. Although it has a high friction coefficient, its wear resistance is often poor, which greatly shortens the service life of the product.

[0003] According to existing regulations, the service life of the side bearing wear plates for railway freight cars is 5 years, and the wear limit is 3mm. However, since the side bearing wear plates are exposed to the air for a long time during use, and are affected by frictional heat during use, it is easy for the nylon material to age and become brittle, or even break, resulting in the side bearing wear plates being scrapped prematurely. In addition, the nylon material is greatly affected by the ambient temperature and humidity; when the temperature is high and the humidity is high, the nylon side bearing wear plates expand, the strength decreases, the friction coefficient increases, the wear increases, and they are prone to deformation; and when the temperature is low and the humidity is low, the nylon side bearing wear plates have reduced toughness, reduced friction coefficient, and are prone to breakage. Therefore, how to invent a side bearing wear plate with strong anti-aging performance, high strength, high temperature resistance, high humidity resistance, excellent friction coefficient, and good wear resistance, to increase the service life of the side bearing wear plates and reduce the replacement frequency, has become a technical problem that needs to be urgently solved by technical personnel in this field. Summary of the invention

[0004] The purpose of the present invention is to provide a side bearing wear plate made of a highly wear-resistant powder metallurgy material and a preparation method thereof, so as to solve the problems existing in the above-mentioned prior art. The side bearing wear plate made of a highly wear-resistant powder metallurgy material of the present invention has a suitable and stable friction coefficient and a low wear rate, and its performance is less affected by the service conditions, and can ensure that the performance of the side bearing wear plate is not affected when the external environment changes greatly.

[0005] To achieve the above object, the present invention provides the following solutions:

[0006] One of the technical solutions of the present invention: a side bearing wear plate of a highly wear-resistant powder metallurgy material, comprising the following raw materials in parts by weight: 62 to 87 parts of copper powder, 3 to 8 parts of aluminum powder, 2 to 5 parts of tin powder, 5 to 15 parts of graphite, 2 to 6 parts of metal selenide and 1 to 4 parts of boron carbide.

[0007] Furthermore, the metal selenide includes molybdenum diselenide and / or niobium diselenide.

[0008] Furthermore, the particle size of the copper powder is ≤74 μm, the particle size of the aluminum powder is ≤74 μm, the particle size of the tin powder is ≤74 μm, the particle size of the graphite is 100-600 μm, the particle size of the metal selenide is ≤10 μm, and the particle size of the boron carbide is 60-150 μm.

[0009] The high wear-resistant powder metallurgy material side bearing wear plate uses copper powder as the base material, and can be sintered into a copper alloy with the added aluminum powder and tin powder, thereby improving the structural strength, mechanical properties and temperature resistance of the side bearing wear plate. It can solve the problems of easy aging and poor temperature resistance of the existing nylon material, and the wear resistance of the side bearing wear plate can be significantly improved, thereby increasing the service life of the side bearing wear plate.

[0010] The graphite and metal selenide in the side bearing wear plate made of high wear-resistant powder metallurgy material can be used as anti-wear agents. Graphite has excellent anti-seizure performance and is particularly suitable for high-load and compressive wear-resistant working conditions. Adding graphite can improve the wear resistance of the side bearing wear plate. On the premise of ensuring that the side bearing wear plate has a suitable friction coefficient, it can not only protect the pair from damage, but also make the side bearing wear plate itself have a stable friction coefficient; metal selenide has thermal stability and does not absorb moisture in the air, which can improve the high temperature resistance of the side bearing wear plate, increase the wear resistance of the side bearing wear plate, and thus extend the service life of the side bearing wear plate.

[0011] Boron carbide in the side bearing wear plate made of high wear-resistant powder metallurgy material acts as a friction agent, which plays the role of increasing friction, wear resistance and anti-seizure, and improves the friction coefficient of the side bearing wear plate. In addition, the hardness of boron carbide is appropriate, which can protect the dual material during the friction process, ensuring that the side bearing wear plate has a suitable and stable friction coefficient.

[0012] The second technical solution of the present invention is a method for preparing the above-mentioned high wear-resistant powder metallurgy material side bearing wear plate, comprising the following steps:

[0013] The raw materials are premixed by weight, and then aviation kerosene is added to mix evenly, followed by pressing (cold pressing) and sintering (sintering and solidification) to obtain the high wear-resistant powder metallurgy material side bearing wear plate.

[0014] Furthermore, the amount of the aviation kerosene used is 0.8-1.2% of the total weight of the raw materials.

[0015] Furthermore, the compression molding pressure is 300-500 MPa, and the holding time is 2-4 s.

[0016] Furthermore, the sintering temperature is 800-850° C., the pressure is 1.5-2.5 MPa, the holding time is 2-4 hours, and the protective atmosphere is hydrogen or decomposed ammonia (ammonia is decomposed into hydrogen and nitrogen in a molar ratio of 1:3).

[0017] Furthermore, the mixing time is 7 to 9 hours.

[0018] The third technical solution of the present invention: an application of the above-mentioned high wear-resistant powder metallurgy material side bearing wear plate in the preparation of railway freight cars.

[0019] The present invention discloses the following technical effects:

[0020] (1) The side bearing wear plate made of highly wear-resistant powder metallurgy material of the present invention has the characteristics of good wear resistance, high temperature resistance, high strength, good mechanical properties, long service life, etc., and the performance of the side bearing wear plate of the present invention is less affected by the service conditions, and the performance of the side bearing wear plate can be ensured not to be affected when the external environment changes greatly.

[0021] (2) The side bearing wear plate of the present invention is made by powder metallurgy process. The aviation kerosene added during the batching process can not only effectively prevent dust generated during the mixing, but also effectively avoid component segregation generated during the mixing process, thereby ensuring uniform mixing of the raw materials and facilitating the consistency of material properties.

[0022] (3) The preparation method of the side bearing wear plate of the present invention includes the steps of weighing, mixing, cold pressing, sintering and curing, etc., which has the advantages of clear process links, tight connection and simple operation, thereby ensuring that the side bearing wear plate has the quality characteristics of high structural strength, good mechanical properties, stable friction coefficient, good wear resistance and long service life.

[0023] (4) The present invention adopts pressing molding under relatively high pressure and pressure sintering under protective atmosphere, which ensures that the side bearing wear plate has the advantages of high temperature resistance and strength, suitable and stable friction coefficient, excellent wear resistance, etc.

[0024] (5) The side bearing wear plate of the present invention is made of only six components, the material components are simple, the process is simple and easy to control, and the production cost is low.

[0025] (6) The friction coefficient of the side bearing wear plate prepared by the present invention is similar to that of the nylon side bearing wear plate currently used on railway freight cars, both of which are within the reasonable range of 0.3 to 0.4. However, the friction coefficient curve of nylon material fluctuates greatly, while the friction coefficient of the side bearing wear plate prepared by the present invention is extremely stable with small fluctuations. Moreover, under this friction coefficient condition, the side bearing wear plate prepared by the present invention has high wear resistance, and the wear rate is from 5.46×10 -8 cm 3 / N·m is reduced to 2.27×10-9 cm 3 / N·m, therefore, the side bearing wear plate can have a longer service life. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments will be briefly introduced below. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0027] Figure 1 A metallographic photograph of a side bearing wear plate made of a highly wear-resistant powder metallurgy material prepared in Example 4 of the present invention;

[0028] Figure 2 The friction curve of the commercially available nylon side bearing wear plate;

[0029] Figure 3 This is the friction curve of the side bearing wear plate made of highly wear-resistant powder metallurgy material prepared in Example 4 of the present invention. DETAILED DESCRIPTION

[0030] Various exemplary embodiments of the present invention will now be described in detail. This detailed description should not be considered as limiting the present invention, but should be understood as a more detailed description of certain aspects, features, and embodiments of the present invention.

[0031] It should be understood that the terms described in the present invention are only for describing special embodiments and are not intended to limit the present invention. In addition, for the numerical range in the present invention, it should be understood that each intermediate value between the upper and lower limits of the scope is also specifically disclosed. Each smaller range between the intermediate value in any stated value or stated range and any other stated value or intermediate value in the described range is also included in the present invention. The upper and lower limits of these smaller ranges can be independently included or excluded in the scope.

[0032] Unless otherwise indicated, all technical and scientific terms used herein have the same meanings as those generally understood by those skilled in the art. Although the present invention describes only preferred methods and materials, any methods and materials similar or equivalent to those described herein may also be used in the implementation or testing of the present invention. All documents mentioned in this specification are incorporated by reference to disclose and describe the methods and / or materials associated with the documents. In the event of a conflict with any incorporated document, the content of this specification shall prevail.

[0033] It will be apparent to those skilled in the art that various modifications and variations may be made to the specific embodiments of the present invention description without departing from the scope or spirit of the present invention. Other embodiments derived from the present invention description will be apparent to those skilled in the art. The present application description and examples are exemplary only.

[0034] The words “include,” “including,” “have,” “contain,” etc. used in this document are open-ended terms, meaning including but not limited to.

[0035] The “parts” described in the following examples are all “parts by weight”.

[0036] The particle size of the copper powder used in the present invention is ≤74μm, the particle size of the aluminum powder is ≤74μm, the particle size of the tin powder is ≤74μm, the particle size of the graphite powder is 100-600μm, the particle size of the molybdenum diselenide powder is ≤10μm, the particle size of the niobium diselenide powder is <10μm, and the particle size of the boron carbide is 60-150μm.

[0037] Example 1

[0038] A method for preparing a side bearing wear plate made of highly wear-resistant powder metallurgy material:

[0039] The high wear-resistant powder metallurgy material side bearing wear plate is composed of the following raw materials in parts by weight: 62 parts of copper powder (particle size is 5-35μm), 8 parts of aluminum powder (particle size is 5-74μm), 5 parts of tin powder (particle size is 5-35μm), 15 parts of graphite (particle size is 100-300μm), 3 parts of molybdenum diselenide powder (particle size is 0.5-5μm), 3 parts of niobium diselenide powder (particle size is 0.5-5μm) and 4 parts of boron carbide (particle size is 60-150μm).

[0040] Preparation method:

[0041] (1) Copper powder, aluminum powder, tin powder, graphite, molybdenum diselenide powder, niobium diselenide powder, and boron carbide were premixed, and 1.2 parts of aviation kerosene were added to mix the powders. The mixed powders were put into a drum mixer and mixed for 9 hours. Then, the mixed mixture was filled into a mold, and the mixture was pressed on a powder hydraulic press (pressing pressure of 500 MPa, holding time of 4 seconds) to obtain a compact.

[0042] (2) The compact is placed in a sintering furnace and sintered under pressure in a hydrogen atmosphere (sintering temperature is 850°C, sintering pressure is 2.5 MPa, and holding time is 4 h) to obtain a side bearing wear plate of a highly wear-resistant powder metallurgy material.

[0043] Example 2

[0044] A method for preparing a side bearing wear plate made of highly wear-resistant powder metallurgy material:

[0045] The high wear-resistant powder metallurgy material side bearing wear plate is composed of the following raw materials in parts by weight: 73 parts of copper powder (particle size is 5-35μm), 7 parts of aluminum powder (particle size is 5-74μm), 3 parts of tin powder (particle size is 5-35μm), 8 parts of graphite (particle size is 300-600μm), 6 parts of molybdenum diselenide powder (particle size is 0.5-5μm) and 3 parts of boron carbide (particle size is 60-150μm).

[0046] Preparation method:

[0047] (1) Copper powder, aluminum powder, tin powder, graphite, molybdenum diselenide powder, and boron carbide were premixed, and 0.9 parts of aviation kerosene were added to mix the powders. The mixed powders were put into a drum mixer and mixed for 7 hours. Then, the mixed mixture was filled into a mold, and the mixture was pressed on a powder hydraulic press (pressing pressure of 400 MPa, holding time of 2 seconds) to obtain a compact.

[0048] (2) The compact is placed in a sintering furnace and sintered under pressure in a decomposed ammonia atmosphere (sintering temperature is 810°C, sintering pressure is 2.0 MPa, and holding time is 2 h) to obtain a side bearing wear plate of a highly wear-resistant powder metallurgy material.

[0049] Example 3

[0050] A method for preparing a side bearing wear plate made of highly wear-resistant powder metallurgy material:

[0051] The high wear-resistant powder metallurgy material side bearing wear plate is composed of the following raw materials in parts by weight: 73 parts of copper powder (particle size is 35-74μm), 4 parts of aluminum powder (particle size is 35-74μm), 4 parts of tin powder (particle size is 35-74μm), 13 parts of graphite (particle size is 100-300μm), 2 parts of molybdenum diselenide powder (particle size is 5-10μm) and 4 parts of boron carbide (particle size is 60-150μm).

[0052] Preparation method:

[0053] (1) Copper powder, aluminum powder, tin powder, graphite, molybdenum diselenide powder, and boron carbide were premixed, and 1.2 parts of aviation kerosene were added to mix the powders. The mixed powders were put into a drum mixer and mixed for 8 hours. Then, the mixed mixture was filled into a mold, and the mixture was pressed on a powder hydraulic press (pressing pressure of 500 MPa, holding time of 4 seconds) to obtain a compact.

[0054] (2) The compact is placed in a sintering furnace and sintered under pressure in a decomposed ammonia atmosphere (sintering temperature is 840°C, sintering pressure is 2.5 MPa, and holding time is 4 h) to obtain a side bearing wear plate of a highly wear-resistant powder metallurgy material.

[0055] Example 4

[0056] A method for preparing a side bearing wear plate made of highly wear-resistant powder metallurgy material:

[0057] The high wear-resistant powder metallurgy material side bearing wear plate is composed of the following raw materials in parts by weight: 74 parts of copper powder (particle size is 35-74μm), 5 parts of aluminum powder (particle size is 35-74μm), 3 parts of tin powder (particle size is 35-74μm), 10 parts of graphite (particle size is 200-400μm), 3 parts of molybdenum diselenide powder (particle size is 5-10μm), 3 parts of niobium diselenide powder (particle size is 5-10μm) and 2 parts of boron carbide (particle size is 60-150μm).

[0058] Preparation method:

[0059] (1) Copper powder, aluminum powder, tin powder, graphite, molybdenum diselenide powder, niobium diselenide powder, and boron carbide were premixed, and 1.0 part of aviation kerosene was added to mix the powders evenly. The mixed powders were put into a drum mixer and mixed for 8 hours. Then, the mixed mixture was filled into a mold, and the mixture was pressed on a powder hydraulic press (pressing pressure of 400 MPa, holding time of 3 seconds) to obtain a compact.

[0060] (2) The compact was placed in a sintering furnace and sintered under pressure in a hydrogen atmosphere (sintering temperature: 825°C, sintering pressure: 2.0 MPa, holding time: 3 h) to obtain a side bearing wear plate made of highly wear-resistant powder metallurgy material. See the metallographic photograph for details. Figure 1 .

[0061] from Figure 1 It can be seen that the various components are evenly embedded in the light yellow copper matrix. The added aluminum powder and tin powder can be sintered into copper alloy, which can improve the structural strength, mechanical properties and temperature resistance of the side bearing wear plate; graphite and metal selenide are used as anti-wear agents to improve the wear resistance of the side bearing wear plate. On the premise of ensuring that the side bearing wear plate has a suitable friction coefficient, it can not only protect the dual material from damage, but also make the side bearing wear plate itself have a stable friction coefficient, thereby extending the service life of the side bearing wear plate; boron carbide, as a friction agent, plays the role of increasing friction, wear resistance and anti-seizure. In addition, the hardness of boron carbide is appropriate, which can protect the dual material during the friction process and ensure that the side bearing wear plate has a suitable and stable friction coefficient.

[0062] Example 5

[0063] A method for preparing a side bearing wear plate made of highly wear-resistant powder metallurgy material:

[0064] The high wear-resistant powder metallurgy material side bearing wear plate is composed of the following raw materials in parts by weight: 75 parts of copper powder (particle size is 35-74μm), 6 parts of aluminum powder (particle size is 35-74μm), 3 parts of tin powder (particle size is 35-74μm), 12 parts of graphite (particle size is 300-600μm), 2 parts of niobium diselenide powder (particle size is 0.5-10μm) and 2 parts of boron carbide (particle size is 60-150μm).

[0065] Preparation method:

[0066] (1) Copper powder, aluminum powder, tin powder, graphite, niobium diselenide powder, and boron carbide were premixed, and 1.0 part of aviation kerosene was added to mix the powders evenly. The mixed powders were put into a drum mixer and mixed for 9 hours. Then, the evenly mixed mixture was filled into a mold, and the mixture was pressed on a powder hydraulic press (pressing pressure of 500 MPa, holding time of 4 seconds) to obtain a compact.

[0067] (2) The pressed green sheet is placed in a sintering furnace and sintered under pressure in a hydrogen atmosphere (sintering temperature is 840°C, sintering pressure is 2.5 MPa, and holding time is 4 h) to obtain a side bearing wear plate of a highly wear-resistant powder metallurgy material.

[0068] Example 6

[0069] A method for preparing a side bearing wear plate made of highly wear-resistant powder metallurgy material:

[0070] The high wear-resistant powder metallurgy material side bearing wear plate is composed of the following raw materials in parts by weight: 75 parts of copper powder (particle size is 5-74μm), 3 parts of aluminum powder (particle size is 5-35μm), 5 parts of tin powder (particle size is 5-74μm), 7 parts of graphite (particle size is 300-600μm), 6 parts of niobium diselenide powder (particle size is 0.5-10μm) and 4 parts of boron carbide (particle size is 60-150μm).

[0071] Preparation method:

[0072] (1) Copper powder, aluminum powder, tin powder, graphite, niobium diselenide powder, and boron carbide were premixed, and 0.8 parts of aviation kerosene was added to mix the powders evenly. The mixed powders were put into a drum mixer and mixed for 7 hours. Then, the evenly mixed mixture was filled into a mold, and the mixture was pressed on a powder hydraulic press (pressing pressure of 300 MPa, holding time of 2 seconds) to obtain a compact.

[0073] (2) The compact is placed in a sintering furnace and sintered under pressure in a hydrogen atmosphere (sintering temperature is 820°C, sintering pressure is 1.5 MPa, and holding time is 3 h) to obtain a side bearing wear plate of a highly wear-resistant powder metallurgy material.

[0074] Example 7

[0075] A method for preparing a side bearing wear plate made of highly wear-resistant powder metallurgy material:

[0076] The high wear-resistant powder metallurgy material side bearing wear plate is composed of the following raw materials in parts by weight: 87 parts of copper powder (particle size is 5-74μm), 3 parts of aluminum powder (particle size is 5-35μm), 2 parts of tin powder (particle size is 5-74μm), 5 parts of graphite (particle size is 300-600μm), 1 part of molybdenum diselenide powder (particle size is 0.5-10μm), 1 part of niobium diselenide powder (particle size is 0.5-10μm) and 1 part of boron carbide (particle size is 60-150μm).

[0077] Preparation method:

[0078] (1) Copper powder, aluminum powder, tin powder, graphite, molybdenum diselenide powder, niobium diselenide powder, and boron carbide were premixed, and 0.8 parts of aviation kerosene were added to mix the powders. The mixed powders were put into a drum mixer and mixed for 7 hours. Then, the mixed mixture was filled into a mold, and the mixture was pressed on a powder hydraulic press (pressing pressure of 300 MPa, holding time of 2 seconds) to obtain a compact.

[0079] (2) The compact is placed in a sintering furnace and sintered under pressure in a decomposed ammonia atmosphere (sintering temperature is 800°C, sintering pressure is 1.5 MPa, and holding time is 2 h) to obtain a side bearing wear plate of a highly wear-resistant powder metallurgy material.

[0080] Comparative Example 1

[0081] A method for preparing a powder metallurgy material:

[0082] The powder metallurgy material is composed of the following raw materials in parts by weight: 82 parts of copper powder (particle size is 35-74 μm), 5 parts of aluminum powder (particle size is 35-74 μm), 3 parts of tin powder (particle size is 35-74 μm), and 10 parts of graphite (particle size is 200-400 μm).

[0083] Preparation method:

[0084] (1) After premixing copper powder, aluminum powder, tin powder, and graphite, 1 part of aviation kerosene is added to mix the powders evenly. The mixed powders are put into a drum mixer and mixed for 8 hours. Then, the evenly mixed mixture is filled into a mold and pressed on a powder hydraulic press (pressing pressure is 400 MPa, holding time is 3 s) to obtain a compact.

[0085] (2) The compact is placed in a sintering furnace and sintered under pressure in a decomposed ammonia atmosphere (sintering temperature is 825°C, sintering pressure is 2 MPa, and holding time is 3 h) to obtain a powder metallurgy material.

[0086] Comparative Example 2

[0087] A method for preparing a powder metallurgy material:

[0088] The powder metallurgy material is composed of the following raw materials in parts by weight: 76 parts of copper powder (particle size is 35-74 μm), 5 parts of aluminum powder (particle size is 35-74 μm), 3 parts of tin powder (particle size is 35-74 μm), 10 parts of graphite (particle size is 200-400 μm), 3 parts of molybdenum diselenide powder (particle size is 5-10 μm), and 3 parts of niobium diselenide powder (particle size is 5-10 μm).

[0089] Preparation method:

[0090] (1) Copper powder, aluminum powder, tin powder, graphite, molybdenum diselenide powder, and niobium diselenide powder were premixed, and 1 part of aviation kerosene was added to mix the powders evenly. The mixed powders were put into a drum mixer and mixed for 8 hours. Then, the evenly mixed mixture was filled into a mold, and the mixture was pressed on a powder hydraulic press (pressing pressure was 400 MPa, and holding time was 3 seconds) to obtain a compact.

[0091] (2) The compact is placed in a sintering furnace and sintered under pressure in a decomposed ammonia atmosphere (sintering temperature is 825°C, sintering pressure is 2 MPa, and holding time is 3 h) to obtain a powder metallurgy material.

[0092] Comparative Example 3

[0093] A method for preparing a powder metallurgy material:

[0094] The powder metallurgy material is composed of the following raw materials in parts by weight: 80 parts of copper powder (particle size is 35-74 μm), 5 parts of aluminum powder (particle size is 35-74 μm), 3 parts of tin powder (particle size is 35-74 μm), 10 parts of graphite (particle size is 200-400 μm), and 2 parts of boron carbide (particle size is 60-150 μm).

[0095] Preparation method:

[0096] (1) After premixing copper powder, aluminum powder, tin powder, graphite, and boron carbide, 1 part of aviation kerosene is added to mix the powders evenly. The mixed powders are put into a drum mixer and mixed for 8 hours. Then, the evenly mixed mixture is filled into a mold and pressed on a powder hydraulic press (pressing pressure is 400 MPa, holding time is 3 seconds) to obtain a compact.

[0097] (2) The compact is placed in a sintering furnace and sintered under pressure in a decomposed ammonia atmosphere (sintering temperature is 825°C, sintering pressure is 2 MPa, and holding time is 3 h) to obtain a powder metallurgy material.

[0098] Effect Example 1

[0099] According to the requirements and test specifications of standards such as TJ / CL477-2016 "Technical Requirements for Long-Stroke Elastic Side Bearings of Railway Freight Cars" and TB / T3269 "Elastic Side Bearings of Railway Freight Cars", the friction and wear properties of the high-wear-resistant powder metallurgy side bearing wear plate prepared in the embodiment of the present invention and the powder metallurgy material prepared in the comparative example were tested using a pin-disc friction tester, and the commercially available nylon side bearing wear plate was used as a control (the friction curve of the commercially available nylon side bearing wear plate is shown in Figure 2 ), such as friction curve, friction coefficient and wear rate. The disc is made of 45# steel, with heat treatment hardness of 47HRC~52HRC and size of Ф(60mm±0.5mm)×(10mm±0.2mm); the pin is made of side bearing wear plate material with size of Ф10mm×20mm.

[0100] Friction coefficient test: Loading pressure is 1.0MPa, running speed is 0.04m / s, the test is carried out continuously until the friction area reaches 70%, the friction force change should be within the range of ±10N, and the test data within the middle 20min is taken. The friction coefficient (μ) is calculated by the formula It is concluded that is the average friction force (torque) (N), and P is the working pressure (N).

[0101] Wear rate test of side bearing wear plate material: loading pressure is 2.0MPa, running speed is 0.2m / s, and the test is at least 48h. The wear rate (V) is calculated by the formula It is obtained that m1 is the weight of the sample before the test (g), m2 is the weight of the sample after the test (g), and ρ is the density of the sample (g / cm 3 ), t is the test running time (s), F is the loading load (N), and v is the test running speed (m / s).

[0102] The friction curve of the commercially available nylon side bearing wear plate is shown in Figure 2 The friction curve of the high wear-resistant powder metallurgy material side bearing wear plate prepared in Example 4 is shown in Figure 3 .

[0103] from Figure 2 and Figure 3 It can be seen that the friction coefficient curve of the commercially available nylon side bearing wear plate fluctuates greatly, and there is great instability during the friction process, while the friction coefficient curve of the high wear-resistant powder metallurgy side bearing wear plate prepared in Example 4 fluctuates less and is smoother, and the state is more stable during the friction process. The friction coefficient value is within the range of 0.30 to 0.40 specified for the side bearing wear plate material, which is a better side bearing wear plate material.

[0104] Table 1 Friction and wear properties of side bearing wear plates for railway freight cars

[0105]

[0106]

[0107] The requirements for side bearing wear plates for railway freight cars are: the material friction coefficient is between 0.3 and 0.4, and the material wear rate is less than or equal to 8.0×10 -8 cm 3 / N·m.

[0108] It can be seen from Table 1 that, compared with the nylon side bearing wear plate material of the current railway freight cars (the commercially available nylon side bearing wear plate), the friction coefficient of the side bearing wear plate material prepared by the present invention is more stable, and the friction coefficient fully meets the standard required by the composite side bearing wear plate, which can ensure the safety of railway freight car operation.

[0109] The material composition used in preparing the side bearing wear plate of the present invention is relatively simple, the economic cost is low, and the preparation process is relatively easy. It can be clearly seen from the wear rate data of the side bearing wear plates prepared in Examples 1 to 7 that, compared with the current nylon material (commercially available nylon side bearing wear plates), the wear rate of the side bearing wear plates prepared by the present invention is significantly reduced, the wear resistance of the side bearing wear plates is improved, the replacement frequency of the side bearing wear plates is reduced, the service life of the side bearing wear plates is increased, and manpower and material resources are saved.

[0110] The side bearing wear plate prepared by the invention has the advantages of high temperature resistance, high strength, and not easily affected by the environment, and can ensure the safety of railway freight car operation.

[0111] The embodiments described above are only descriptions of the preferred modes of the present invention, and are not intended to limit the scope of the present invention. Without departing from the design spirit of the present invention, various modifications and improvements made to the technical solutions of the present invention by ordinary technicians in this field should all fall within the protection scope determined by the claims of the present invention.

Claims

1. A powder metallurgy material side bearing wear plate, characterized in that: The invention comprises the following raw materials in parts by weight: 62 to 87 parts of copper powder, 3 to 8 parts of aluminum powder, 2 to 5 parts of tin powder, 5 to 15 parts of graphite, 2 to 6 parts of metal selenide and 1 to 4 parts of boron carbide; The metal selenide includes molybdenum diselenide and / or niobium diselenide; The particle size of the copper powder is 5-74 μm, the particle size of the aluminum powder is 5-74 μm, the particle size of the tin powder is 5-74 μm, the particle size of the graphite is 100-600 μm, the particle size of the metal selenide is 0.5-10 μm, and the particle size of the boron carbide is 60-150 μm.

2. A method for preparing the powder metallurgy material side bearing wear plate according to claim 1, characterized in that: The following steps are involved: The raw materials are premixed according to weight, and then aviation kerosene is added to mix them evenly, followed by pressing and molding, and sintering to obtain the powder metallurgy material side bearing wear plate.

3. The preparation method according to claim 2, characterized in that: The amount of the aviation kerosene used is 0.8-1.2% of the total weight of the raw materials.

4. The preparation method according to claim 2, characterized in that: The pressure of the pressing molding is 300-500 MPa, and the holding time is 2-4 s.

5. The preparation method according to claim 2, characterized in that: The sintering temperature is 800-850° C., the pressure is 1.5-2.5 MPa, the insulation time is 2-4 hours, and the protective atmosphere is hydrogen or decomposed ammonia.

6. Use of the powder metallurgy side bearing wear plate according to claim 1 in the preparation of railway freight cars.