A soft light water-based light-curing coating and preparation method thereof

Through the combination of hydrogenated rosin modified polyacrylate emulsion and functionalized nanosilica, the problem of insufficient adhesion and mechanical properties of water-based photocuring coatings is solved, and the physical properties and antioxidant effects of the coatings are improved. It is suitable for new materials and Industrial production of new processes.

CN117903683BActive Publication Date: 2024-11-08ZHONGSHAN XINFENG LIGHT CURING MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410073702.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-17
Publication Date
2024-11-08
Estimated Expiration
2044-01-17

AI Technical Summary

Technical Problem

Due to the viscosity limitation of the photocuring resin, existing water-based photocuring coatings have reduced the mechanical properties and adhesion of the coating, which limits its large-scale industrial production application of new materials and new processes.

Method used

Use hydrogenated rosin modified polyacrylate emulsion and surface functionalized nanosilica load-hindered phenolic antioxidants to improve the adhesion and mechanical properties of the coating, and prepare the modified polyacrylate emulsion through semi-continuous emulsion polymerization to form Cross-linked network structure to improve reactive activity and flexibility.

Benefits of technology

It significantly improves the adhesion, adhesion and physical properties of the photocured coating, enhances the pencil hardness, solvent resistance and impact resistance of the adhesive film, and improves the overall mechanical properties and oxidation resistance of the coating.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117903683B_ABST
    Figure CN117903683B_ABST
Patent Text Reader

Abstract

The invention relates to the field of coatings, and discloses a soft light water-based photocurable coating. The soft light water-based photocurable coating comprises the following raw materials in parts by weight: 70-90 parts of polyurethane acrylate, 30-50 parts of modified polyacrylate emulsion, 3-8 parts of photoinitiator, 25-40 parts of modified nano-silicon dioxide, 0.2-2 parts of leveling agent, 0.2-2 parts of defoamer, and 10-25 parts of purified water; the modified polyacrylate emulsion is a hydrogenated rosin-modified polyacrylate emulsion containing epoxy groups; the modified nano-silicon dioxide is a nano-silicon dioxide surface functionalized by a silane coupling agent, and then a hindered phenol antioxidant is grafted. The invention utilizes the hydrogenated rosin-modified polyacrylate emulsion to improve the adhesion and bonding performance of the photocurable coating, and also enables the hydrogenated rosin to be better integrated into the adhesive film, thereby obtaining better physical properties; in addition, the surface functionalized nano-silicon dioxide is used to load the hindered phenol antioxidant, thereby giving the coating good mechanical properties and antioxidant effects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a soft light water-based photocurable coating and a preparation method thereof. Background Art

[0002] Photocurable coatings, also known as photosensitive coatings, use UV to trigger chemically active liquid materials to quickly polymerize and crosslink, and instantly solidify into films. Water-based photocurable coatings inherit and develop the advantages of traditional oil-based photocurable coating technology and water-based coatings and ink technologies. They have quickly become a research hotspot due to their superior performance advantages such as environmental protection, wide application, safety, and relatively simple construction. They have the advantages of fast curing speed, energy saving, excellent coating performance, wide application range of substrates, and are conducive to the elimination of VOCs. They are widely used in wood, plastic, optical fiber, paper and other material fields.

[0003] In the prior art, water-based photocurable coatings are limited by the viscosity of the photocurable resin, and have a low molecular weight, so they shrink greatly after the polymerization reaction. Also, because faster reaction speed and better performance are required, some acrylate monomers are often added to the photocurable coating formula to balance the crosslinking density and reduce the reaction steric hindrance. Resins with higher functionality need to reduce the crosslinking degree through low-functionality monomers, while resins with lower functionality need to increase the reaction speed through trifunctional or higher-functionality monomers. However, higher functionality will cause a large shrinkage rate of the system, resulting in a decrease in the mechanical properties and adhesion of the coating, which limits the application of photocurable coatings in large-scale industrial production of new materials and new processes. Summary of the invention

[0004] In order to solve the deficiencies mentioned in the above-mentioned background technology, the purpose of the present invention is to provide a soft light water-based photocurable coating and a preparation method thereof, and the adhesion and bonding properties of the photocurable coating are improved by using hydrogenated rosin modified polyacrylate emulsion, and the hydrogenated rosin is better integrated into the adhesive film to obtain better physical properties. In addition, surface functionalized nano-silica is used to load hindered phenolic antioxidants to give the coating good mechanical properties and antioxidant effects.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] A soft light water-based light-curing coating comprises the following raw materials in parts by weight: 70-90 parts of polyurethane acrylate, 30-50 parts of modified polyacrylate emulsion, 3-8 parts of photoinitiator, 25-40 parts of modified nano-silicon dioxide, 0.2-2 parts of leveling agent, 0.2-2 parts of defoaming agent, and 10-25 parts of purified water;

[0007] The modified polyacrylate emulsion is a hydrogenated rosin modified polyacrylate emulsion containing epoxy groups;

[0008] The modified nano silicon dioxide is prepared by functionalizing the surface of the nano silicon dioxide using N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and then grafting 3,5-di-tert-butyl-4-hydroxybenzoic acid hindered phenol antioxidant.

[0009] Preferably, the photoinitiator is one or more combinations of 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, dialkoxyacetophenone, and α-hydroxyalkyl benzophenone; the leveling agent is one or a combination of BYK333 and BYK349; the defoamer is one or more combinations of tributyl phosphate, defoamer Deqian 3100, defoamer BYK088, and defoamer BYK028.

[0010] Preferably, the modified polyacrylate emulsion comprises the following raw materials in parts by weight: 10-25 parts of butyl acrylate, 10-25 parts of methyl methacrylate, 2-5 parts of hydroxyethyl acrylate, 3-10 parts of hydrogenated rosin, 1-3.5 parts of glycidyl methacrylate, 0.1-0.5 parts of ammonium persulfate aqueous solution, 1-5 parts of compound emulsifier, and 20-50 parts of purified water;

[0011] The preparation method of the modified polyacrylate emulsion comprises the following steps:

[0012] A. Mixing alkylphenol polyoxyethylene ether and sodium lauryl sulfate to obtain a composite emulsifier, and stirring and mixing the composite emulsifier with purified water to prepare a pre-emulsion;

[0013] B. Take butyl acrylate, methyl methacrylate, hydroxyethyl acrylate, glycidyl methacrylate, compound emulsifier, hydrogenated rosin and purified water, stir and mix, emulsify at 400-700r / min for 20-40min. After emulsification, adjust the stirring rate to 100-250r / min, heat to 70-80℃, add initiator ammonium persulfate aqueous solution dropwise, and heat to 80-90℃;

[0014] C. Slowly add the pre-emulsion prepared in step A with a dropping funnel, adding 1 mL of ammonium persulfate aqueous solution every 30 minutes. After the pre-emulsion is added, pour in the remaining ammonium persulfate aqueous solution, keep warm for 2 to 4 hours, cool to 30 to 50° C., and discharge to prepare modified polyacrylate.

[0015] Preferably, the mass ratio of alkylphenol polyoxyethylene ether to sodium dodecyl sulfate in the composite emulsifier is 1:1, and the mass fraction of the ammonium persulfate aqueous solution is 2.5%.

[0016] Preferably, the preparation method of the modified nano-silicon dioxide comprises the following steps:

[0017] S1. Disperse the dried nano-silica in toluene for ultrasonic dispersion. After the ultrasonic dispersion is completed, nitrogen is passed through the reaction. Under magnetic stirring, N-(2-ethylamino)-3-propylaminotrimethoxysilane and triethylamine are added, and the mixture is stirred at 70 to 90° C. and refluxed for 9 to 12 hours. After the reaction is completed, the mixture is cooled to room temperature, filtered, and repeatedly washed with toluene and ethanol, and then dried in an oven to prepare surface functionalized nano-silica.

[0018] S2. Weigh 3,5-di-tert-butyl-4-hydroxybenzoic acid into a three-necked flask, add chloroform, place in a 40-60° C. magnetic stirring water bath, open the condensed water, slowly add distilled thionyl chloride dropwise with a constant pressure dropping funnel, and continue to react for 4-6 hours. The obtained reaction solution is subjected to rotary evaporation to prepare 3,5-di-tert-butyl-4-hydroxybenzoyl chloride;

[0019] S3. Take the surface functionalized silica obtained in step S1, add toluene and ultrasonically disperse it, evacuate it, and pass nitrogen protection. Take the 3,5-di-tert-butyl-4-hydroxybenzoyl chloride obtained in step S2, dissolve it in toluene and then slowly add it dropwise, stir and mix, then add triethylamine dropwise, and react at a constant temperature for 18 to 24 hours under nitrogen protection. After the reaction is completed, filter it, rinse it with toluene and methanol several times, and place it at 70 to 90°C to vacuum dry to prepare modified nano-silica.

[0020] Preferably, in step S1, the mass ratio of nano-silicon dioxide, N-(2-ethylamino)-3-propylaminotrimethoxysilane and triethylamine is 3-8:6-10:1.

[0021] Preferably, in step S3, the mass ratio of the surface functionalized silica to 3,5-di-tert-butyl-4-hydroxybenzoyl chloride is 2 to 5:1.

[0022] A method for preparing a soft light water-based photocurable coating comprises the following steps: mixing parts by weight of polyurethane acrylate, modified polyacrylate emulsion, photoinitiator, modified nano-silicon dioxide, defoamer, leveling agent and purified water, stirring and dispersing for 15 to 30 minutes, filtering with a 200 to 300 mesh filter screen, and preparing the soft light water-based photocurable coating.

[0023] Beneficial effects of the present invention:

[0024] The present invention uses butyl acrylate, methyl methacrylate, and hydroxyethyl acrylate as main monomers, hydrogenated rosin and glycidyl methacrylate as functional monomers, and adopts semi-continuous emulsion polymerization to prepare modified polyacrylate emulsion. The carboxyl group contained in hydrogenated rosin and the epoxy group in glycidyl methacrylate undergo a ring-opening reaction to form a cross-linked network structure, so that hydrogenated rosin can exert the unique performance of its triphenanthrene ring skeleton, improve the adhesion and bonding performance of the photocurable coating on the substrate, and also make hydrogenated rosin better integrated into the film, obtain better physical properties, and enhance the pencil hardness, solvent resistance and impact resistance of the film. In addition, high-functional polyurethane acrylate is used in combination with modified polyacrylate emulsion to increase the reactivity and flexibility of water-based photocurable coating.

[0025] The present invention utilizes ethoxyl groups at one end of a silane coupling agent to be hydrolyzed to generate silanol groups, which react with hydroxyl groups of nano-silicon dioxide to functionalize the surface of the nano-silicon dioxide. The carboxyl group at one end of 3,5-di-tert-butyl-4-hydroxybenzoic acid is activated to form an acyl chloride structure, which reacts with the amino group at the other end of the aminosilane coupling agent to load the nano-silicon dioxide with a hindered phenol antioxidant. This can reduce the agglomeration of inorganic particles and facilitate the dispersion of the nano-silicon dioxide. At the same time, it can also overcome the physical loss of the antioxidant due to migration and volatilization to a certain extent, and can give the coating good mechanical properties and antioxidant effects. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0027] Figure 1 It is the infrared spectrum of nano silicon dioxide before and after modification in Example 4 of the present invention. DETAILED DESCRIPTION

[0028] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0029] The polyurethane acrylate in the embodiment of the present invention is purchased from Changxing, model number Etercure6145-100, and the product name is hexafunctional polyurethane acrylate.

[0030] Embodiment 1 The preparation method of modified polyacrylate emulsion comprises the following steps:

[0031] A. Mix alkylphenol polyoxyethylene ether and sodium lauryl sulfate to obtain a composite emulsifier, and stir and mix 0.5 parts of the composite emulsifier with 8 parts of purified water to prepare a pre-emulsion;

[0032] B. Take 10 parts of butyl acrylate, 12 parts of methyl methacrylate, 2 parts of hydroxyethyl acrylate, 1 part of glycidyl methacrylate, 1 part of compound emulsifier, 3 parts of hydrogenated rosin and 20 parts of purified water, stir and mix, emulsify at 420r / min for 20min, after emulsification, adjust the stirring rate to 110r / min, heat to 70°C, add initiator ammonium persulfate aqueous solution dropwise, and heat to 85°C;

[0033] C. Use a dropping funnel to slowly drop the pre-emulsion prepared in step A, adding 1 mL of ammonium persulfate aqueous solution every 30 minutes. After the pre-emulsion is added, pour in the remaining ammonium persulfate aqueous solution, keep warm for 2 hours, cool to 30°C and discharge to prepare modified polyacrylate.

[0034] Embodiment 2 The preparation method of modified polyacrylate emulsion comprises the following steps:

[0035] A. Mix alkylphenol polyoxyethylene ether and sodium lauryl sulfate to obtain a composite emulsifier, and stir and mix 1 part of the composite emulsifier with 15 parts of purified water to prepare a pre-emulsion;

[0036] B. Take 15 parts of butyl acrylate, 15 parts of methyl methacrylate, 3 parts of hydroxyethyl acrylate, 2 parts of glycidyl methacrylate, 2 parts of compound emulsifier, 5 parts of hydrogenated rosin and 30 parts of purified water, stir and mix, emulsify at 500r / min for 25min, after emulsification, adjust the stirring rate to 200r / min, heat to 80℃, add initiator ammonium persulfate aqueous solution dropwise, and heat to 90℃;

[0037] C. Use a dropping funnel to slowly drop the pre-emulsion prepared in step A, adding 1 mL of ammonium persulfate aqueous solution every 30 minutes. After the pre-emulsion is added, pour in the remaining ammonium persulfate aqueous solution, keep warm for 2 hours, cool to 30°C and discharge to prepare modified polyacrylate.

[0038] The preparation method of the modified polyacrylate emulsion of embodiment 3 comprises the following steps:

[0039] A. Mix alkylphenol polyoxyethylene ether and sodium lauryl sulfate to obtain a composite emulsifier, and stir and mix 1 part of the composite emulsifier with 15 parts of purified water to prepare a pre-emulsion;

[0040] B. Take 20 parts of butyl acrylate, 20 parts of methyl methacrylate, 5 parts of hydroxyethyl acrylate, 3 parts of glycidyl methacrylate, 3 parts of compound emulsifier, 7 parts of hydrogenated rosin and 32 parts of purified water, stir and mix, emulsify at 620r / min for 35min, after emulsification, adjust the stirring rate to 250r / min, heat to 80℃, add initiator ammonium persulfate aqueous solution dropwise, and heat to 90℃;

[0041] C. Use a dropping funnel to slowly drop the pre-emulsion prepared in step A, and add 1 mL of ammonium persulfate aqueous solution every 30 minutes. After the pre-emulsion is added, pour in the remaining ammonium persulfate aqueous solution, keep warm for 3 hours, cool to 45°C and discharge to prepare modified polyacrylate.

[0042] Embodiment 4 The preparation method of modified nano-silicon dioxide comprises the following steps:

[0043] S1. Take 15.0g of dried nano-silica and disperse it in toluene for ultrasonic dispersion. After the ultrasonic dispersion is completed, nitrogen is passed through the reaction. Under magnetic stirring, 27.3g of N-(2-ethylamino)-3-propylaminotrimethoxysilane and 3.6g of triethylamine are added. The mixture is stirred at 70°C and refluxed for 9h. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed repeatedly with toluene and ethanol, and then dried in an oven to prepare surface functionalized nano-silica.

[0044] S2. Weigh 16.8 g of 3,5-di-tert-butyl-4-hydroxybenzoic acid into a three-necked flask, add chloroform, place in a 42° C. magnetic stirring water bath, open the condensed water, slowly add distilled thionyl chloride dropwise with a constant pressure dropping funnel, and continue to react for 4 hours. The obtained reaction solution is subjected to rotary evaporation to prepare 3,5-di-tert-butyl-4-hydroxybenzoyl chloride;

[0045] S3. Take 10.8 g of the surface functionalized silica obtained in step S1, add toluene and ultrasonically disperse it, evacuate it, and pass nitrogen for protection. Take 3.0 g of the 3,5-di-tert-butyl-4-hydroxybenzoyl chloride obtained in step S2, dissolve it in toluene and then slowly add it dropwise, stir and mix, then add triethylamine dropwise, and react at a constant temperature for 18 hours under nitrogen protection. After the reaction is completed, filter it, rinse it with toluene and methanol several times, and dry it in vacuum at 70°C to prepare modified nano-silica.

[0046] The infrared spectroscopy analysis of nano-silicon dioxide and modified nano-silicon dioxide was carried out, and the results are as follows Figure 1 As shown in the figure, it can be seen that before and after the nano-silica grafted antioxidant, the –1 There are broad absorption peaks at all locations. After the nano-silica surface is grafted with silane coupling agent, curve b is at 2930cm –1There is an absorption peak at 2963 cm, which corresponds to the stretching vibration peak of -CH2 on the silane coupling agent. –1 The -CH3 stretching vibration peak at 1637 cm is the methyl group of 3,5-di-tert-butyl. –1 and 1558cm –1 The characteristic absorption peak of amide appears at , indicating that the antioxidant is successfully grafted onto the surface of nano-silica.

[0047] Embodiment 5 The preparation method of modified nano-silicon dioxide comprises the following steps:

[0048] S1. Take 18.6g of dried nano-silica and disperse it in toluene for ultrasonic dispersion. After the ultrasonic dispersion is completed, nitrogen is passed through the reaction. Under magnetic stirring, 28.8g of N-(2-ethylamino)-3-propylaminotrimethoxysilane and 3.9g of triethylamine are added. The mixture is stirred at 70°C and refluxed for 10h. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed repeatedly with toluene and ethanol, and then dried in an oven to prepare surface functionalized nano-silica.

[0049] S2. Weigh 17.4 g of 3,5-di-tert-butyl-4-hydroxybenzoic acid into a three-necked flask, add chloroform, place in a 45° C. magnetic stirring water bath, turn on the condensed water, slowly add distilled thionyl chloride dropwise with a constant pressure dropping funnel, and continue to react for 6 hours. The resulting reaction solution is rotary evaporated to obtain 3,5-di-tert-butyl-4-hydroxybenzoyl chloride;

[0050] S3. Take 11.4 g of the surface functionalized silica obtained in step S1, add toluene and ultrasonically disperse it, evacuate it, and pass nitrogen for protection. Take 3.6 g of 3,5-di-tert-butyl-4-hydroxybenzoyl chloride obtained in step S2, dissolve it in toluene and then slowly add it dropwise, stir and mix, then add triethylamine dropwise, and react at a constant temperature for 20 hours under nitrogen protection. After the reaction is completed, filter it, rinse it with toluene and methanol several times, and dry it in vacuum at 90°C to prepare modified nano-silica.

[0051] Embodiment 6 The preparation method of modified nano-silicon dioxide comprises the following steps:

[0052] S1. Disperse 17.1 g of dried nano-silica in toluene for ultrasonic dispersion. After the ultrasonic dispersion is completed, nitrogen is passed through the reaction. Under magnetic stirring, 31.5 g of N-(2-ethylamino)-3-propylaminotrimethoxysilane and 3.6 g of triethylamine are added. The mixture is stirred at 85° C. and refluxed for 12 h. After the reaction is completed, the mixture is cooled to room temperature, filtered, washed repeatedly with toluene and ethanol, and then dried in an oven to obtain surface functionalized nano-silica.

[0053] S2, weigh 18.0g 3,5-di-tert-butyl-4-hydroxybenzoic acid into a three-necked flask, add chloroform, place in a 60°C magnetic stirring water bath, open the condensed water, slowly add distilled thionyl chloride dropwise with a constant pressure dropping funnel, and continue to react for 5h. The obtained reaction solution is rotary evaporated to prepare 3,5-di-tert-butyl-4-hydroxybenzoyl chloride;

[0054] S3. Take 12.5 g of the surface functionalized silica obtained in step S1, add toluene and ultrasonically disperse it, evacuate it, and pass nitrogen for protection. Take 2.7 g of 3,5-di-tert-butyl-4-hydroxybenzoyl chloride obtained in step S2, dissolve it in toluene and then slowly add it dropwise, stir and mix, then add triethylamine dropwise, and react at a constant temperature for 24 hours under nitrogen protection. After the reaction is completed, filter it, rinse it with toluene and methanol several times, and place it at 90°C for vacuum drying to prepare modified nano-silica.

[0055] Example 7 A soft light water-based light-curing coating comprises the following raw materials in parts by weight: 70 parts of polyurethane acrylate, 32 parts of modified polyacrylate emulsion, 3 parts of photoinitiator, 27 parts of modified nano-silicon dioxide, 0.2 parts of leveling agent, 0.2 parts of defoaming agent, and 10 parts of purified water;

[0056] The preparation method of the above-mentioned soft light water-based photocurable coating comprises the following steps: mixing parts by weight of polyurethane acrylate, modified polyacrylate emulsion, photoinitiator, modified nano-silica, defoamer, leveling agent and purified water, stirring and dispersing for 20 minutes, filtering with a 200-mesh filter screen, and preparing a soft light water-based photocurable coating.

[0057] Example 8 A soft light water-based light-curing coating comprises the following raw materials in parts by weight: 78 parts of polyurethane acrylate, 38 parts of modified polyacrylate emulsion, 5 parts of photoinitiator, 30 parts of modified nano-silicon dioxide, 1 part of leveling agent, 1 part of defoaming agent, and 15 parts of purified water;

[0058] The preparation method of the above-mentioned soft light water-based photocurable coating is the same as that of Example 7.

[0059] Example 9 A soft light water-based light-curing coating comprises the following raw materials in parts by weight: 85 parts of polyurethane acrylate, 47 parts of modified polyacrylate emulsion, 8 parts of photoinitiator, 38 parts of modified nano-silicon dioxide, 2 parts of leveling agent, 2 parts of defoaming agent, and 25 parts of purified water;

[0060] The preparation method of the above-mentioned soft light water-based photocurable coating is the same as that of Example 7.

[0061] Comparative Example 1 A soft light water-based photocurable coating comprises the following raw materials in parts by weight: 78 parts of polyurethane acrylate, 35 parts of polyacrylate emulsion, 7 parts of photoinitiator, 30 parts of modified nano-silica, 0.7 parts of leveling agent, 0.8 parts of defoaming agent, and 12 parts of purified water;

[0062] The preparation method of the above-mentioned soft light water-based photocurable coating is the same as that of Example 7.

[0063] Comparative Example 2 A soft light water-based photocurable coating comprises the following raw materials in parts by weight: 82 parts of polyurethane acrylate, 41 parts of modified polyacrylate emulsion, 6 parts of photoinitiator, 32 parts of nano-silicon dioxide, 1.2 parts of leveling agent, 1.2 parts of defoaming agent, and 20 parts of purified water;

[0064] The preparation method of the above-mentioned soft light water-based photocurable coating is the same as that of Example 7.

[0065] Performance testing:

[0066] The soft light water-based photocurable coating prepared in Examples 7-9 and Comparative Examples 1-2 was used to prepare a film, and the photocurable coating was coated on tinplate with a wire rod. After standing for 15 seconds, it was cured into a film by a photocuring machine, and the performance was tested after being placed at room temperature for 24 hours.

[0067] The adhesion of the film was determined by the cross-hatch method according to GB / T9286-2021; the pencil hardness of the film was determined according to GB / T6739-2022; the impact resistance of the film was determined according to GB / T1732-2020; the aging resistance of the film was determined according to GB / T1865-2009: according to GB / T9274-1988, the film was placed in a 5% by mass hydrochloric acid solution and a 5% by mass sodium hydroxide aqueous solution, respectively, and the phenomenon of bubbling and falling off of the film on the tinplate was recorded at regular intervals, and the solvent resistance of the film was determined. The test results are shown in Table 1.

[0068] Table 1 Film performance test results

[0069]

[0070] It can be seen from the data in Table 1 that the soft light water-based photocurable coatings prepared in Examples 7-8 have excellent adhesion, excellent mechanical properties and antioxidant effects. In Comparative Example 1, no hydrogenated rosin was added to modify the polyacrylate emulsion, and its adhesion, pencil hardness, acid resistance, alkali resistance and impact resistance were significantly reduced. In Comparative Example 2, no nano-silica was modified, and its aging resistance was significantly reduced, and the pencil hardness and impact resistance were slightly reduced.

[0071] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0072] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.

Claims

1. A soft light water-based light-curing coating, characterized in that: The invention comprises the following raw materials in parts by weight: 70-90 parts of polyurethane acrylate, 30-50 parts of modified polyacrylate emulsion, 3-8 parts of photoinitiator, 25-40 parts of modified nano-silicon dioxide, 0.2-2 parts of leveling agent, 0.2-2 parts of defoaming agent and 10-25 parts of purified water; The modified polyacrylate emulsion is a hydrogenated rosin modified polyacrylate emulsion containing epoxy groups; The modified nano-silica is prepared by functionalizing the surface of the nano-silica with N-(2-aminoethyl)-3-aminopropyltrimethoxysilane, and then grafting 3,5-di-tert-butyl-4-hydroxybenzoic acid hindered phenol antioxidant; The modified polyacrylate emulsion comprises the following raw materials in parts by weight: 10-25 parts of butyl acrylate, 10-25 parts of methyl methacrylate, 2-5 parts of hydroxyethyl acrylate, 3-10 parts of hydrogenated rosin, 1-3.5 parts of glycidyl methacrylate, 0.1-0.5 parts of ammonium persulfate aqueous solution, 1-5 parts of compound emulsifier, and 20-50 parts of purified water; The preparation method of the modified polyacrylate emulsion comprises the following steps: A. Mixing alkylphenol polyoxyethylene ether and sodium lauryl sulfate to obtain a composite emulsifier, and stirring and mixing the composite emulsifier with purified water to prepare a pre-emulsion; B. Take butyl acrylate, methyl methacrylate, hydroxyethyl acrylate, glycidyl methacrylate, compound emulsifier, hydrogenated rosin and purified water, stir and mix, emulsify at 400-700r / min for 20-40min. After emulsification, adjust the stirring rate to 100-250r / min, heat to 70-80℃, add initiator ammonium persulfate aqueous solution dropwise, and heat to 80-90℃; C. Slowly drop the pre-emulsion prepared in step A with a dropping funnel, drop 1 mL of ammonium persulfate aqueous solution every 30 min, pour the remaining ammonium persulfate aqueous solution after the pre-emulsion is added, keep warm for 2-4 h, cool to 30-50 ° C, and prepare modified polyacrylate; The preparation method of the modified nano silicon dioxide comprises the following steps: S1. Disperse the dried nano-silica in toluene for ultrasonic dispersion. After the ultrasonic dispersion is completed, nitrogen is passed through the reaction. Under magnetic stirring, N-(2-ethylamino)-3-propylaminotrimethoxysilane and triethylamine are added, and the mixture is stirred at 70-90°C and refluxed for 9-12 hours. After the reaction is completed, the mixture is cooled to room temperature, filtered, repeatedly washed with toluene and ethanol, and then dried in an oven to prepare surface functionalized nano-silica. S2. Weigh 3,5-di-tert-butyl-4-hydroxybenzoic acid into a three-necked flask, add chloroform, place in a 40-60° C. magnetic stirring water bath, open the condensed water, slowly add distilled thionyl chloride dropwise with a constant pressure dropping funnel, and continue to react for 4-6 hours. The obtained reaction solution is subjected to rotary evaporation to prepare 3,5-di-tert-butyl-4-hydroxybenzoyl chloride; S3, taking the surface functionalized silica obtained in step S1, adding toluene to ultrasonically disperse, evacuating, passing nitrogen protection, taking the 3,5-di-tert-butyl-4-hydroxybenzoyl chloride obtained in step S2, dissolving it in toluene and then slowly adding dropwise, stirring and mixing, then adding triethylamine dropwise, reacting at a constant temperature for 18 to 24 hours under nitrogen protection, filtering after the reaction is completed, washing with toluene and methanol for multiple times, and drying under vacuum at 70 to 90° C. to prepare modified nano-silica; In the step S1, the mass ratio of nano-silicon dioxide, N-(2-ethylamino)-3-propylaminotrimethoxysilane and triethylamine is 3-8:6-10:1; In the step S3, the mass ratio of the surface functionalized silica to 3,5-di-tert-butyl-4-hydroxybenzoyl chloride is 2-5:

1.

2. The soft light water-based light-curing coating according to claim 1, characterized in that: The photoinitiator is one or more combinations of 1-hydroxy-cyclohexyl phenyl ketone, 2-hydroxy-2-methyl-1-phenyl-1-propanone, benzophenone, dialkoxyacetophenone, and α-hydroxyalkyl benzophenone; the leveling agent is one or a combination of BYK333 and BYK349; the defoamer is one or more combinations of tributyl phosphate, defoamer Deqian 3100, defoamer BYK088, and defoamer BYK028.

3. The soft light water-based light-curing coating according to claim 1, characterized in that: The mass ratio of alkylphenol polyoxyethylene ether to sodium lauryl sulfate in the composite emulsifier is 1:1, and the mass fraction of the ammonium persulfate aqueous solution is 2.5%.

4. The method for preparing the soft light water-based light-curing coating according to claim 1, characterized in that: The method comprises the following steps: mixing parts by weight of polyurethane acrylate, modified polyacrylate emulsion, photoinitiator, modified nano-silicon dioxide, defoamer, leveling agent and purified water, stirring and dispersing for 15 to 30 minutes, filtering with a 200 to 300 mesh filter screen, and preparing a soft light water-based light-curing coating.