A kind of amidoxime-based cryogel and its preparation method and application

The ultra-large interconnected pore charge-balanced hydrogel prepared through freeze polymerization process and grafting method solves the problems of low utilization rate and slow adsorption rate of uranium extraction materials from seawater, achieves efficient uranyl ion adsorption and anti-biopollution, and significantly improves Improve uranium efficiency and material recyclability.

CN117920154BActive Publication Date: 2024-10-01SHENZHEN MSU-BIT UNIVERSITY +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410114431.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-01-25
Publication Date
2024-10-01
Estimated Expiration
2044-01-25

AI Technical Summary

Technical Problem

Existing materials for uranium extraction from seawater have low utilization rates, slow adsorption rates, and are susceptible to biological contamination, making it difficult to effectively extract uranyl ions from seawater.

Method used

Carboxymethyl cellulose hydrogel was prepared using freeze polymerization process, and dinitrile diamine and amidoximation were introduced through grafting method to form ultra-large interconnected pore charge balance hydrogel (AO-PAM/CMC) to improve the adsorbent According to the seawater flux and antibacterial properties, a simulated electric field is constructed to accelerate the adsorption of uranyl ions.

Benefits of technology

The accessibility and adsorption efficiency of uranyl ions are significantly improved. The material has high selectivity and anti-biopollution properties. The adsorption capacity only decreases by 2% after six cycles, and the desorption efficiency exceeds 80%. It is suitable for complex seawater. uranium extraction conditions.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117920154B_ABST
    Figure CN117920154B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of polymer materials, and relates to an amidoxime-based cryogel and its preparation method and application. The present invention first prepares a PAM / CMC three-dimensional continuous super-large porous hydrogel with a fully interpenetrating structure by a cryopolymerization process; then a dinitrile diamine is introduced by a grafting method to obtain a DCD-PAM / CMC hydrogel, and then amidoximation is performed to obtain an ultra-large interconnected pore charge balance hydrogel AO-PAM / CMC. The ultra-large interconnected pores formed by the cryopolymerization process can increase the seawater flux in the adsorbent, and combined with the excellent hydrophilic properties of carboxymethyl cellulose, the accessibility of uranyl ions is significantly enhanced; amidoximated nitrile guanidine is introduced into the hydrogel, while giving the adsorbent antibacterial function, it can achieve charge balance with the deprotonated amidoxime group, construct a simulated electric field, and thus accelerate the adsorption of U(VI); in addition, the cryogel has excellent cyclicity, which improves the application value of the gel in the field of uranium extraction from seawater.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of polymer materials and relates to an amidoxime-based cryogel and a preparation method and application thereof. Background Art

[0002] Contemporary society faces the dual challenge of meeting the growing global energy demand while reducing environmental problems, especially climate change caused by greenhouse gas emissions. In this context, nuclear energy, as a clean and efficient form of energy, has attracted much attention due to its high energy density and zero greenhouse gas emissions. However, the sustainable development of nuclear energy faces a key problem: the limited uranium reserves on land cannot meet the demand continuously. The ocean contains huge uranium resources, about 4.5 billion tons, which is 1,000 times the total uranium reserves on land. Therefore, in order to ensure the sustainable supply of nuclear energy, reduce environmental impact, and solve the problem of uranium shortage, the development of efficient and low-cost seawater uranium extraction technology has become a vital task in the nuclear energy field.

[0003] At present, a variety of physical or chemical methods have been used to extract uranium from seawater, among which adsorption is one of the most practical methods. The amidoxime-based functional materials commonly used in the adsorption method are widely used in the field of uranium extraction from seawater due to their excellent selectivity, high adsorption capacity and low cost. In recent years, various types of amidoxime-based adsorbents have been reported for uranium extraction from seawater, such as metal organic frameworks, covalent organic frameworks, fiber materials and hydrogels. However, most of the above amidoxime-based adsorbents have a dense structure, and uranyl ions are difficult to diffuse into the interior of the material; in addition, the outer layer of the adsorbent will undergo a cross-linking reaction after complexing with uranyl ions, which further reduces the accessibility of uranyl ions in the adsorbent, resulting in a low utilization rate of the adsorbent; and the uranium concentration in seawater is extremely low, and there are a variety of interfering metal ions and microbial species, which poses a challenge to effective adsorption. Therefore, in order to ensure the sustainability of future nuclear energy development and give full play to the potential of nuclear energy as a clean and sustainable energy alternative, it is urgent to develop new highly selective and efficient adsorbents to meet the complex conditions of uranium extraction from seawater. Summary of the invention

[0004] In order to solve the problems of low utilization rate, slow adsorption rate and microbial attachment of seawater uranium extraction materials and adsorbents in the prior art, the present invention provides a seawater uranium extraction material and preparation method capable of realizing rapid extraction of uranium and anti-biological pollution. The present invention first prepares carboxymethyl cellulose hydrogel by a freezing polymerization process, then introduces dinitrile diamine by a grafting method, and then performs amidoximation to obtain a super large interconnecting pore charge balance hydrogel (AO-PAM / CMC). The super large interconnecting pores formed by the freezing polymerization process can improve the seawater flux in the adsorbent, and the accessibility of uranyl ions is significantly enhanced by combining the excellent hydrophilic properties of carboxymethyl cellulose. The introduction of amidoximated nitrile guanidine imparts antibacterial function to the adsorbent material, while being able to achieve charge balance with the deprotonated amidoxime group, constructing a simulated electric field, thereby accelerating the adsorption of U (VI).

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] A method for preparing amidoxime-based cryogel comprises the following steps:

[0007] Step 1: dissolving sodium carboxymethyl cellulose (CMC-Na) in deionized water, and adding acrylamide (AM) and N,N'-methylenebisacrylamide (MBA) to disperse uniformly to obtain a mixed solution;

[0008] Add ammonium persulfate (APS) to the mixed solution, purge with N2, then lower the temperature to -10°C to 0°C, add N,N,N',N'-tetramethylethylenediamine (TEMED), stir continuously to form a reaction solution; quickly pour the reaction solution into a silica gel mold, react at -50 to -20°C; then melt, wash, and dry to obtain a three-dimensional continuous ultra-large pore PAM / CMC hydrogel with a fully interpenetrating structure;

[0009] Step 2: Place the PAM / CMC hydrogel in step 1 in a reaction container, add N-hydroxysuccinimide (NHS) and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride (EDC), and add deionized water, add dinitrile diamine (DCD) after 20 to 60 minutes, and then add N,N-dimethylformamide, and then heat in a water bath to 45 to 70° C., reflux reaction, and after the reaction is completed, cool, wash, and dry to obtain DCD-PAM / CMC hydrogel;

[0010] Step 3: Place the DCD-PAM / CMC hydrogel in step 2 in a reaction container, add hydroxylamine hydrochloride and Na2CO3, then add deionized water and methanol, heat in a water bath to 55-85°C, keep warm for reaction, cool, wash and dry to obtain AO-PAM / CMC hydrogel.

[0011] Preferably, the mass volume ratio of the sodium carboxymethyl cellulose, acrylamide, N,N'-methylenebisacrylamide, deionized water, ammonium persulfate, and N,N,N',N'-tetramethylethylenediamine in step 1 is (0.3-0.7 g): (1.2-2.0 g): (0.2-0.5 g): (10-30 mL): (0.02-0.05 g): 20 μL.

[0012] Preferably, in step 1, N2 is purged for 0.5 to 2 hours; the reaction is carried out at -50 to -20°C for 15 to 30 hours; the washing is performed by ultrasonic cleaning with deionized water and ethanol until the mixture becomes neutral to remove unreacted monomers; and the drying is performed in an oven at 60 to 90°C for 8 to 16 hours.

[0013] Preferably, in step 2, the mass volume ratio of the PAM / CMC hydrogel, N-hydroxysuccinimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, deionized water, dinitrile diamine, and N,N-dimethylformamide is (0.05-0.3 g): (0.1-0.4 g): (0.2-0.5 g): (5-30 mL): (0.3-0.9 g): (5-10 mL).

[0014] Preferably, the reaction time in step 2 is 5 to 20 hours; the washing is performed by ultrasonic cleaning with deionized water and ethanol until neutral; and the drying is performed in an oven at 70 to 90° C. for 8 to 16 hours.

[0015] Preferably, the mass volume ratio of the DCD-PAM / CMC hydrogel, hydroxylamine hydrochloride, Na2CO3, deionized water and methanol in step 3 is (0.05-0.3 g): (0.3-0.8 g): (0.5-1 g): (5-20 mL): (5-20 mL).

[0016] Preferably, the reaction time in step 3 is 5 to 20 hours; the washing is performed by ultrasonic cleaning with deionized water and ethanol until neutral; and the drying is performed in an oven at 70 to 90° C. for 8 to 16 hours.

[0017] More preferably, step 1 is reacted at -40 to -10°C for 12 to 36 hours.

[0018] The present invention also provides amidoxime-based cryogel prepared by the above preparation method.

[0019] The amidoxime-based cryogel is used in extracting uranium from seawater.

[0020] Compared with the prior art, the present invention has the following advantages:

[0021] (1) The present invention adopts a freeze polymerization process to prepare a carboxymethyl cellulose hydrogel, then introduces a dinitrile diamine by a grafting method, and then performs amidoximation to obtain a super-large interconnected pore charge-balanced hydrogel (AO-PAM / CMC); the super-large interconnected pores formed by the freeze polymerization process can increase the seawater flux in the adsorbent, and combined with the excellent hydrophilicity of carboxymethyl cellulose, significantly enhance the accessibility of uranyl ions.

[0022] (2) The present invention introduces amidoxime-modified nitrile guanidine into the hydrogel, which not only imparts antibacterial function to the adsorbent material, but also achieves charge balance with the deprotonated amidoxime group, constructs a simulated electric field, and thus accelerates the adsorption of U(VI).

[0023] (3) The cryogel of the present invention has excellent recyclability. After six adsorption-desorption cycles, the adsorption amount of AO-PAM / CMC hydrogel only decreased by about 2%, and the desorption efficiency was always over 80%. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 The figure is a flow chart of the preparation of the cryogel of the present invention.

[0025] Figure 2 These are the morphology pictures of PAM / CMC, DCD-PAM / CMC and AO-PAM / CMC of Example 3 of the present invention.

[0026] Figure 3 The contact angle test diagrams of PAM / CMC, DCD-PAM / CMC and AO-PAM / CMC of Example 3 of the present invention are shown.

[0027] Figure 4 It is the antibacterial test diagram of PAM / CMC, DCD-PAM / CMC and AO-PAM / CMC of Example 3 of the present invention. DETAILED DESCRIPTION

[0028] The present invention will be further described below in conjunction with specific embodiments, and the advantages and features of the present invention will become clearer as the description proceeds. However, the embodiments are exemplary only and do not constitute any limitation to the scope of the present invention. It should be understood by those skilled in the art that the details and forms of the technical solution of the present invention may be modified or replaced without departing from the spirit and scope of the present invention, but these modifications and replacements all fall within the scope of protection of the present invention.

[0029] Example 1

[0030] A method for preparing amidoxime-based cryogel for charge balance-promoting uranium extraction from seawater comprises the following steps:

[0031] Step 1: Dissolve 0.5g sodium carboxymethyl cellulose in 20mL deionized water, and dissolve 1.777g acrylamide monomer and 0.308g N,N'-methylenebisacrylamide in the sodium carboxymethyl cellulose solution under stirring to form a mixed solution. After all the solution is dissolved, add 0.032g ammonium persulfate and purge with N2 for 1h. Place the mixed solution in a -40℃ refrigerator for precooling. When the temperature drops to -5℃~0℃, add 20μL N,N,N',N'-tetramethylethylenediamine to the mixed solution, stir continuously to form a mixed reaction solution. Quickly pour the mixed reaction solution into a silica gel mold, maintain the temperature at -40℃, and react for 15h. Take out the hydrogel and melt it, and ultrasonically clean it with a large amount of deionized water and ethanol until it is neutral to remove unreacted monomers. Dry the hydrogel in a 90℃ oven for 10h to obtain a fully interpenetrating PAM / CMC three-dimensional continuous ultra-large porous hydrogel.

[0032] Step 2: Take 0.1g of PAM / CMC hydrogel in a 50mL beaker, add 0.15g of N-hydroxysuccinimide and 0.3g of 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and then add 5mL of deionized water. After activating the carboxyl group for half an hour, add 0.7g of dinitrile diamine, and then add 5mL of N,N-dimethylformamide to completely dissolve the dinitrile diamine. Then heat the water bath to 70°C and reflux for 5h. Cool to room temperature, take out the hydrogel, and ultrasonically clean it with a large amount of deionized water and ethanol until it is neutral. Dry the hydrogel in a 90°C oven for 10h to obtain DCD-PAM / CMC hydrogel.

[0033] Step 3: Take 0.1g DCD-PAM / CMC hydrogel in a 50mL beaker, add 0.6g hydroxylamine hydrochloride and 0.7626g Na2CO3, then add 5mL deionized water to completely dissolve hydroxylamine hydrochloride and Na2CO3, and then add 5mL methanol. Then heat to 80℃ in a water bath and keep warm for 5h. Cool to room temperature, take out the hydrogel, and ultrasonically clean it with a large amount of deionized water and ethanol until it is neutral. Dry the hydrogel in a 90℃ oven for 10h to obtain AO-PAM / CMC hydrogel.

[0034] Example 2

[0035] The preparation method of AO-PAM / CMC hydrogel is different from that of Example 1 in that, in step 1, the material polymerization temperature is maintained at -30°C and the reaction is carried out for 20 hours; in step 2, the amount of dinitrile diamine is 0.5 g, and then the water bath is heated to 50°C and the reaction is refluxed for 15 hours; in step 3, the amount of hydroxylamine hydrochloride is 0.4 g, and the water bath is heated to 65°C and the reaction is kept warm for 15 hours. The amounts of the remaining substances are the same as those of Example 1.

[0036] Example 3

[0037] The preparation method of AO-PAM / CMC hydrogel is different from that of Example 1 in that, in step 1, the material polymerization temperature is maintained at -20°C and the reaction is carried out for 24 hours; in step 2, the amount of dinitrile diamine is 0.6 g, and then the water bath is heated to 60°C and the reflux reaction is carried out for 10 hours; in step 3, the amount of hydroxylamine hydrochloride is 0.5 g, and the water bath is heated to 75°C and the reaction is carried out for 10 hours. The amounts of the remaining substances are the same as those of Example 1.

[0038] The PAM / CMC, DCD-PAM / CMC and AO-PAM / CMC hydrogels prepared in Example 3 were tested by scanning electron microscopy. Figure 1 As shown. Figure 1 It can be seen that PAM / CMC has abundant micron-scale open pores. Due to the use of non-directional freezing process, the pores are interconnected and the wall surface is smooth, which is conducive to reducing the resistance to liquid flow while increasing the specific surface area of ​​the pores. After DCD grafting, the pore structure is retained, but the pore size is slightly increased. Finally, after DCD-PAM / CMC is treated with amidoximation, the morphology and structure remain basically unchanged, and the pore size is further increased.

[0039] The contact angle test was performed on the PAM / CMC, DCD-PAM / CMC and AO-PAM / CMC hydrogels prepared in Example 3. The test results are shown in FIG. Figure 3 As shown in , when the contact time is 0.1s, the average contact angle of PAM / CMC hydrogel is 0°, and the average contact angles of DCD-PAM / CMC and AO-PAM / CMC hydrogels are 33.5° and 56.8°, respectively. This may be attributed to the fact that the introduction of DCD consumes the strongly hydrophilic carboxyl groups, resulting in a slight decrease in hydrophilic properties. As the contact time increases, all three hydrogels are completely wetted at 0.2 seconds and no longer show obvious contact angles. Therefore, AO-PAM / CMC hydrogel has excellent hydrophilic properties.

[0040] The antibacterial properties of the PAM / CMC, DCD-PAM / CMC and AO-PAM / CMC hydrogels prepared in Example 3 were tested using the inhibition zone method. Figure 4 As shown in the figure, the PAM / CMC hydrogel without guanidine groups showed no obvious inhibition zone against Escherichia coli (a), Staphylococcus aureus (b) and Vibrio alginolyticus (c). In contrast, the AO-PAM / CMC hydrogel containing guanidine groups showed good antibacterial effects against all three bacteria. In addition, the AO-PAM / CMC hydrogel had the largest inhibition zone against Staphylococcus aureus, indicating that it had the best antibacterial effect against Staphylococcus aureus.

[0041] Application Examples

[0042] The uranium adsorption performance of the PAM / CMC and AO-PAM / CMC hydrogels prepared in Example 3 was tested: 10 mg of the adsorbent was added to a conical flask containing 50 mL of a 50 mg / L uranium-containing aqueous solution, and placed in a constant temperature water bath oscillator for 48 h, the water bath oscillator temperature was adjusted to 25° C., and the rotation speed was set to 160 r / min. The U(VI) concentration before and after the adsorption reaction was measured using a UV-visible spectrophotometer or ICP-MS.

[0043] By adjusting the pH of different uranium solutions, the adsorption performance of PAM / CMC and AO-PAM / CMC hydrogels on uranium was tested, as shown in Table 1. It can be seen that the uranium adsorption capacity of AO-PAM / CMC hydrogel is better than that of PAM / CMC hydrogel. The uranium extraction performance of AO-PAM / CMC hydrogel is best at pH 5.0. As shown in Table 2, after six adsorption-desorption cycles, the adsorption amount of AO-PAM / CMC hydrogel only decreased by about 2%, and the desorption efficiency was always over 80%.

[0044] The good reusability of AO-PAM / CMC hydrogel may be attributed to its charge-balanced structure, which enhances its stability in the eluent. Table 3 shows the adsorption of AO-PAM / CMC hydrogel in real seawater. It can be seen that after the adsorbent was in contact with real seawater for 25 days, the uranium adsorption capacity reached 12.95 mg g -1 .

[0045] Table 1 Effect of different pH on uranium removal rate

[0046]

[0047] Table 2 Recycling performance of AO-PAM / CMC hydrogel

[0048]

[0049] Table 3 Real seawater adsorption performance of AO-PAM / CMC hydrogel

[0050] Adsorption time (days) Adsorption capacity (mg / g) 0 0 2 8.40 4 10.53 7 10.76 10 11.91 15 12.10 20 12.19 25 12.94 .

Claims

1. A method for preparing amidoxime-based cryogel, It is characterized in that The following steps are involved: Step 1: dissolving sodium carboxymethyl cellulose in deionized water, and adding acrylamide and N,N'-methylenebisacrylamide to disperse uniformly to obtain a mixed solution; Ammonium persulfate was added to the mixed solution and N 2 Purge, then lower the temperature to -10℃~0℃, add N,N,N',N'-tetramethylethylenediamine, stir continuously to form a reaction solution; quickly pour the reaction solution into a silica gel mold, react at -50~-20℃; then melt, wash and dry to obtain a three-dimensional continuous ultra-large pore PAM / CMC hydrogel with a fully interpenetrating structure; Step 2: Place the PAM / CMC hydrogel described in step 1 in a reaction container, add N-hydroxysuccinimide and 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, and add deionized water, add dinitrile diamine after 20 to 60 minutes, and then add N,N-dimethylformamide, and then heat in a water bath to 45 to 70° C., reflux reaction, and after the reaction is completed, cool, wash, and dry to obtain DCD-PAM / CMC hydrogel; Step 3: Place the DCD-PAM / CMC hydrogel described in step 2 in a reaction vessel, add hydroxylamine hydrochloride and Na 2 CO 3 , deionized water and methanol were added, and the mixture was heated in a water bath to 55-85°C, and the reaction was kept warm. After cooling, washing and drying, AO-PAM / CMC hydrogel was obtained.

2. The method for preparing the amidoxime-based cryogel according to claim 1, It is characterized in that The mass volume ratio of sodium carboxymethyl cellulose, acrylamide, N,N'-methylenebisacrylamide, deionized water, ammonium persulfate, and N,N,N',N'-tetramethylethylenediamine in step 1 is (0.3-0.7 g):(1.2-2.0 g):(0.2-0.5 g):(10-30 mL):(0.02-0.05 g):20 μL.

3. The method for preparing the amidoxime-based cryogel according to claim 1, It is characterized in that Step 1N 2 Purging for 0.5 to 2 hours; reacting at -50 to -20°C for 15 to 30 hours; washing with deionized water and ethanol ultrasonic cleaning until neutrality to remove unreacted monomers; and drying in an oven at 60 to 90°C for 8 to 16 hours.

4. The method for preparing the amidoxime-based cryogel according to claim 1, It is characterized in that In step 2, the mass volume ratio of the PAM / CMC hydrogel, N-hydroxysuccinimide, 1-(3-dimethylaminopropyl)-3-ethylcarbodiimide hydrochloride, deionized water, dinitrile diamine, and N,N-dimethylformamide is (0.05-0.3 g):(0.1-0.4 g):(0.2-0.5 g):(5-30 mL):(0.3-0.9 g):(5-10 mL).

5. The method for preparing the amidoxime-based cryogel according to claim 1, It is characterized in that The reaction time of step 2 is 5 to 20 hours; the washing is performed by ultrasonic cleaning with deionized water and ethanol until neutral; and the drying is performed in an oven at 70 to 90° C. for 8 to 16 hours.

6. The method for preparing the amidoxime-based cryogel according to claim 1, It is characterized in that Step 3: DCD-PAM / CMC hydrogel, hydroxylamine hydrochloride, Na 2 CO 3 , the mass volume ratio of deionized water and methanol is (0.05g~0.3g):(0.3g~0.8g):(0.5g~1g):(5mL~20mL):(5mL~20mL).

7. The method for preparing the amidoxime-based cryogel according to claim 1, It is characterized in that The reaction time of step 3 is 5 to 20 hours; the washing is performed by ultrasonic cleaning with deionized water and ethanol until neutral; and the drying is performed in an oven at 70 to 90° C. for 8 to 16 hours.

8. The method for preparing the amidoxime-based cryogel according to any one of claims 1 to 7, It is characterized in that In the step 1, the reaction is carried out at -40 to -10°C for 12 to 36 hours.

9. The amidoxime-based cryogel prepared according to the preparation method according to any one of claims 1 to 7.