A 316LN stainless steel ingot and a preparation method thereof, and a preparation method of a 316LN stainless steel plate
Through the combination of the dual vacuum refining technology of the VODC refining furnace and the combination of protective slag and heating agent, the cleanliness and oxidation pollution problems of 316LN stainless steel ingots for BEST vacuum chambers are solved, and high-quality stainless steel production is achieved.
Patent Information
- Application Number
- CN202410100797.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-25
- Publication Date
- 2024-12-03
- Estimated Expiration
- 2044-01-25
AI Technical Summary
In the existing method, when producing 316LN stainless steel ingots for BEST vacuum chambers, the cleanliness of the ingots have not yet reached the best state, and there is a risk of oxidation and pollution during the processing.
Double vacuum refining is carried out using VODC refining furnace. Through vacuum oxygen blown decarbonization, vacuum carbon deoxygenation and vacuum degassing steps, combined with the use of protective slag and heating agent, the casting temperature and speed are controlled to ensure the accuracy and cleanliness of the steel ingot composition. .
It improves the cleanliness of steel ingots, shortens the production cycle, reduces costs, and meets the product quality requirements. The produced stainless steel has excellent mechanical and corrosion resistance.
Smart Images

Figure SMS_1 
Figure SMS_2 
Figure SMS_3
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of alloy material preparation, and in particular to a method for producing 316LN stainless steel ingots for BEST vacuum chambers by using a VODC refining furnace, a method for preparing 316LN stainless steel ingots for BEST vacuum chambers, and a method for preparing 316LN stainless steel plates for BEST vacuum chambers. Background Art
[0002] Stainless steel is widely used in energy, electricity, chemical industry and other fields due to its excellent mechanical and corrosion resistance. The composition of 316LN stainless steel used in BEST vacuum chamber is 18Cr-12Ni-2.5Mo. Due to the addition of Mo, its corrosion resistance, atmospheric corrosion resistance and high temperature strength are particularly good, and it can be used under harsh conditions; and 316LN stainless steel has excellent work hardening properties (non-magnetic).
[0003] At present, the electric arc furnace smelting + AOD method is usually used to produce 316LN stainless steel ingots, which can effectively prevent the metal from being oxidized and contaminated, but the cleanliness of the ingots needs to be improved. Summary of the invention
[0004] The object of the present invention is to provide a method for producing 316LN stainless steel ingots for BEST vacuum chambers using a VODC refining furnace, a method for preparing 316LN stainless steel ingots for BEST vacuum chambers, and a method for preparing 316LN stainless steel plates for BEST vacuum chambers. The present invention adopts a VODC refining furnace to produce 316LN stainless steel ingots for BEST vacuum chambers, can accurately control the composition of the 316LN stainless steel ingots for BEST vacuum chambers, and improves the cleanliness of the ingots.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides a method for producing 316LN stainless steel ingot for BEST vacuum chamber by using VODC refining furnace, comprising the following steps:
[0007] According to the chemical composition of 316LN stainless steel used in BEST vacuum chamber, the scrap steel raw materials are smelted to obtain molten steel;
[0008] The molten steel and the first slag are mixed and vacuum oxygen blowing and decarburization is performed to obtain a first molten steel; the first slag comprises lime, fluorite and aluminum;
[0009] The first molten steel is subjected to vacuum carbon deoxidation to obtain a second molten steel;
[0010] The second molten steel and second slag are mixed and vacuum degassed to obtain a third molten steel; the second slag comprises lime, fluorite, a reducing agent and aluminum;
[0011] The third molten steel is calmed to obtain a fourth molten steel; the calming time is 8 to 15 minutes;
[0012] The fourth molten steel is poured to obtain a 316LN stainless steel ingot for a BEST vacuum chamber;
[0013] The pouring start temperature is 1530±10°C; protective slag and exothermic agent are added during the pouring process; the amount of protective slag is 2.0-2.5kg / t;
[0014] The dosage of the exothermic agent is 2.5-3kg / t; the method for adding the exothermic agent includes: after the cap mouth is filled with the fourth molten steel to more than two-thirds of the height, adding 40-60% of the exothermic agent, and adding the remaining exothermic agent before the end of pouring.
[0015] Preferably, in proportion to the molten steel, the added amount of the first slag includes: 14-17 kg / t of lime, 1.5-3.0 kg / t of fluorite, and 1-1.5 kg / t of aluminum.
[0016] Preferably, the vacuum degree of the vacuum oxygen decarburization is 80-120 mbar, and the bottom blowing gas of the vacuum oxygen decarburization is argon; the bottom blowing argon flow rate is controlled at 3-6 mbar. 3 / h.
[0017] Preferably, the total amount of oxygen used in the vacuum oxygen blowing decarburization process is obtained according to Formula I:
[0018] O used =O total ×M w , Formula I;
[0019] In the formula I, O used The total amount of oxygen used in the vacuum oxygen decarburization process, in Nm 3 ;O total Oxygen consumption per ton of steel, in Nm 3 / t, calculated by formula II; M w is the weight of molten steel, in t;
[0020] O total =1 / eta×[9.31×(C1-C2)+7.98×Si1+6.22×A1]+3.22×(Cr1-Cr2), formula II;
[0021] In the formula II, eta is oxygen release, and its value is 0.75; C1 is the initial carbon content by mass percentage; C2 is the final carbon content by mass percentage; Si1 is the initial silicon content by mass percentage; Al is the initial aluminum content by mass percentage; Cr1 is the initial chromium content by mass percentage; Cr2 is the expected chromium content by mass percentage.
[0022] Preferably, the vacuum degree of the vacuum carbon deoxidation is less than 5 mbar, the bottom blowing gas of the vacuum carbon deoxidation is argon, and the bottom blowing argon flow rate is controlled at 3-6 mbar. 3 / h, and the treatment time of the vacuum carbon deoxidation is 8 to 12 minutes.
[0023] Preferably, the temperature of the second molten steel is measured, and when the temperature of the second molten steel is ≥1650° C., the temperature is not increased; when the temperature of the second molten steel is <1650° C., the temperature is increased.
[0024] Preferably, in proportion to the second molten steel, the added amount of the second slag includes: 14-17 kg / t of lime, 1.5-3.0 kg / t of fluorite, 5-7 kg / t of reducing agent, and 2-4 kg / t of aluminum.
[0025] The present invention provides a 316LN stainless steel ingot for a BEST vacuum chamber produced by the method described in the above technical solution.
[0026] The present invention provides a method for preparing a 316LN stainless steel plate for a BEST vacuum chamber, comprising the following steps:
[0027] Forging the 316LN stainless steel ingot for BEST vacuum chamber described in the above technical solution to obtain a 316LN stainless steel slab for BEST vacuum chamber;
[0028] The 316LN stainless steel slab is heat treated to obtain a 316LN stainless steel plate for a BEST vacuum chamber.
[0029] Preferably, the heat treatment procedure includes: heating to 1050-1150°C at a heating rate of ≤200°C / h, keeping the temperature for 1.5-3.5h, and then cooling to room temperature with water.
[0030] The present invention provides a method for producing 316LN stainless steel ingots for BEST vacuum chambers by using a VODC refining furnace. The present invention implements double vacuum refining by using VODC equipment, thereby improving the cleanliness of the 316LN stainless steel ingots for BEST vacuum chambers. Moreover, the present invention has a short production cycle, low cost and can meet product quality requirements.
[0031] The invention provides a method for preparing a 316LN stainless steel plate for a BEST vacuum chamber. After forging and heat treatment of the 316LN stainless steel ingot for a BEST vacuum chamber prepared by the invention, a 316LN stainless steel plate for a BEST vacuum chamber with excellent performance is obtained. DETAILED DESCRIPTION
[0032] The present invention provides a method for producing 316LN stainless steel ingot for BEST vacuum chamber by using VODC refining furnace, comprising the following steps:
[0033] According to the chemical composition of 316LN stainless steel used in BEST vacuum chamber, the scrap steel raw materials are smelted to obtain molten steel;
[0034] The molten steel and the first slag are mixed and vacuum oxygen blowing and decarburization is performed to obtain a first molten steel; the first slag comprises lime, fluorite and aluminum;
[0035] The first molten steel is subjected to vacuum carbon deoxidation to obtain a second molten steel;
[0036] The second molten steel and second slag are mixed and vacuum degassed to obtain a third molten steel; the second slag comprises lime, fluorite, a reducing agent and aluminum;
[0037] The third molten steel is calmed to obtain a fourth molten steel; the calming time is 8 to 15 minutes;
[0038] The fourth molten steel is poured to obtain a 316LN stainless steel ingot for a BEST vacuum chamber;
[0039] The pouring start temperature is 1530±10°C; protective slag and exothermic agent are added during the pouring process; the amount of protective slag is 2.0-2.5kg / t;
[0040] The dosage of the exothermic agent is 2.5-3kg / t; the method for adding the exothermic agent includes: after the cap mouth is filled with the fourth molten steel to more than two-thirds of the height, adding 40-60% of the exothermic agent, and adding the remaining exothermic agent before the end of pouring.
[0041] The present invention smelts the scrap steel raw material according to the chemical composition of 316LN stainless steel ingot for BEST vacuum chamber to obtain molten steel. In the present invention, the scrap steel raw material preferably includes high-nickel scrap steel and / or high-chromium scrap steel. In the present invention, the smelting is preferably carried out in an electric furnace; the smelting temperature is preferably ≥1630°C, more preferably ≥1650°C; the smelting time is preferably 80 to 120 minutes, more preferably 90 to 120 minutes. In the present invention, the tapping temperature of the smelting is preferably above 1630°C, more preferably 1650 to 1670°C. In the present invention, the smelting is preferably carried out in a medium-frequency electric furnace.
[0042] In the present invention, after the smelting, the obtained crude molten steel is preferably subjected to slag removal. In the present invention, the slag removal is preferably carried out in a tundish. In the present invention, the amount of residue in the molten steel is preferably <2kg / t, more preferably <1.5kg / t.
[0043] After obtaining molten steel, the present invention mixes the molten steel with a first slag, performs vacuum oxygen blowing decarburization, and obtains a first molten steel. In the present invention, the first slag includes lime, fluorite, and aluminum. In the present invention, according to the proportion of the molten steel, the addition amount of the first slag preferably includes: lime 14-17 kg / t, fluorite 1.5-3.0 kg / t, aluminum 1-1.5 kg / t; more preferably includes: lime 15-16 kg / t, fluorite 2.0-2.5 kg / t, aluminum 1.2-1.4 kg / t.
[0044] In the present invention, the vacuum degree of the vacuum oxygen decarburization is preferably 80-120 mbar, more preferably 80-100 mbar; the bottom blowing gas of the vacuum oxygen decarburization is preferably argon; the bottom blowing argon gas flow rate is preferably controlled at 3-6 mbar. 3 / h, more preferably 5 to 6 m 3 / h. In the vacuum oxygen blowing decarburization process, the present invention closely observes the vacuum degree, exhaust gas temperature and cooling water temperature, and ensures a stable reaction in the furnace by adjusting the vacuum degree, oxygen gun height, oxygen blowing flow rate and bottom blowing argon flow rate.
[0045] In the present invention, the total amount of oxygen used in the vacuum oxygen blowing decarburization process is preferably obtained according to Formula I:
[0046] O used =O total ×M w , Formula I;
[0047] In the formula I, O used The total amount of oxygen used in the vacuum oxygen decarburization process, in Nm 3 ;O total Oxygen consumption per ton of steel, in Nm 3 / t, calculated by formula II; M w is the weight of molten steel, in t;
[0048] O total =1 / eta×[9.31×(C1-C2)+7.98×Si1+6.22×A1]+3.22×(Cr1-Cr2), formula II;
[0049] In the formula II, eta is oxygen release, and its value is 0.75; C1 is the initial carbon content by mass percentage; C2 is the final carbon content by mass percentage; Si1 is the initial silicon content by mass percentage; Al is the initial aluminum content by mass percentage; Cr1 is the initial chromium content by mass percentage; Cr2 is the expected chromium content by mass percentage.
[0050] After obtaining the first molten steel, the present invention performs vacuum carbon deoxidation on the first molten steel to obtain the second molten steel. In the present invention, the vacuum carbon deoxidation is preferably performed directly without breaking the air after the vacuum oxygen blowing decarburization.
[0051] In the present invention, the vacuum degree of the vacuum carbon deoxidation is preferably <5 mbar, more preferably <3 mbar; the bottom blowing gas of the vacuum carbon deoxidation is preferably argon, and the bottom blowing argon flow rate is preferably controlled at 3 to 6 mbar. 3 / h, more preferably 5 to 6 m 3 / h; the treatment time of the vacuum carbon deoxidation is preferably 8 to 12 minutes, more preferably 10 to 12 minutes.
[0052] The present invention closely observes the parameter changes of vacuum degree, cooling water temperature and exhaust gas temperature during the vacuum carbon deoxidation process to ensure a stable reaction in the furnace.
[0053] After obtaining the second molten steel, the present invention mixes the second molten steel with the second slag and performs vacuum degassing to obtain the third molten steel. In the present invention, the second molten steel is preferably degassed before mixing with the second slag.
[0054] In the present invention, after obtaining the second molten steel, it is preferred to first measure the temperature of the second molten steel. When the temperature of the second molten steel is ≥1650°C, the temperature is not increased; when the temperature of the second molten steel is <1650°C, the temperature is increased. In the present invention, the temperature increase is preferably performed by vacuum aluminothermic method. In the present invention, the vacuum degree of the vacuum aluminothermic method is preferably 350-450 mbar, more preferably 400-450 mbar; the bottom blowing gas of the vacuum aluminothermic method is preferably argon, and the bottom blowing argon gas flow rate is preferably controlled at 3-6 m 3 / h, more preferably 5 to 6 m 3 / h.
[0055] In the present invention, the amount of oxygen used to burn aluminum during the vacuum aluminothermic method is preferably calculated by formula III;
[0056] O' total =0.62×m Al , Formula III;
[0057] In the formula III, O' total The amount of oxygen used to burn aluminum during the vacuum aluminothermic process, in Nm 3 ;m Al is the mass of aluminum added, in kg; 0.62 is the coefficient, in Nm 3 / kg.
[0058] In the present invention, after the second molten steel is heated, it is preferred that vacuum degassing is directly performed without breaking the vacuum.
[0059] In the present invention, the second slag includes lime, fluorite, a reducing agent and aluminum. In the present invention, according to the proportion of the second molten steel, the addition amount of the second slag preferably includes: lime 14-17 kg / t, fluorite 1.5-3.0 kg / t, reducing agent 5-7 kg / t, aluminum 2-4 kg / t; more preferably includes: lime 15-16 kg / t, fluorite 2.0-2.5 kg / t, reducing agent 6-6.5 kg / t, aluminum 3-3.5 kg / t. In the present invention, the reducing agent preferably includes ferrosilicon; the ferrosilicon is preferably baked ferrosilicon.
[0060] In the present invention, after adding the second slag, alloy is preferably added according to the sampling result to meet the chemical composition requirements of the 316LN stainless steel ingot for the BEST vacuum chamber.
[0061] In the present invention, the vacuum degree of the vacuum degassing is preferably ≤5 mbar, more preferably 2-3 mbar; the bottom blowing gas of the vacuum degassing is preferably argon, and the bottom blowing argon gas flow rate is preferably controlled at 2-6 mbar. 3 / h, more preferably 5 to 6 m 3 / h.
[0062] After obtaining the third molten steel, the present invention calms the third molten steel to obtain a fourth molten steel. In the present invention, the calming time is 8 to 15 minutes, preferably 10 to 12 minutes. In the present invention, the argon flow rate during the calming process is preferably adjusted to 1 to 2.5 Nm 3 / h, more preferably 1.5 to 2.0 Nm 3 / h. The present invention facilitates the floating of inclusions and the removal of brittle inclusions such as carbon nitride through the calming.
[0063] After obtaining the fourth molten steel, the present invention pours the fourth molten steel to obtain a 316LN stainless steel ingot for a BEST vacuum chamber. In the present invention, the pouring preferably uses a fully enclosed argon protection device. In the present invention, the argon pressure of the pouring is preferably controlled at more than 0.5MPa, and more preferably 0.8MPa. In the present invention, the pouring start temperature of the pouring is 1530±10℃, preferably 1520~1530℃. In the present invention, the pouring speed is preferably 0.8~2.0 tons / minute, and more preferably 1.6~1.8 tons / minute. In a specific embodiment of the present invention, the pouring is opened and the seedlings are opened fully during pouring, and the protective slag begins to fall and is controlled at 1.7~1.8 tons / minute. After pouring 2 / 3, it is increased to 1.9~2.0 tons / minute, and the pouring riser time is preferably greater than 2 / 3 of the pouring ingot body time. The present invention controls the pouring start temperature and pouring speed of the pouring within the above range, which is conducive to improving the surface quality of the steel ingot.
[0064] In the present invention, protective slag and exothermic agent are added during the pouring process. In the present invention, the amount of protective slag used is 2.0-2.5 kg / t, preferably 2.2-2.3 kg / t. In the present invention, the protective slag is preferably titanium steel protective slag; in terms of mass percentage, the main components of the titanium steel protective slag preferably include Al2O315.7%, C 4.1%, CaO 23.6%, SiO243.6%, and H2O 0.35%. The present invention uses less protective slag, which prevents the steel slag from crusting and allows the molten steel to rise steadily, which not only improves the surface quality, but also prevents the molten steel from rolling up slag.
[0065] In the present invention, the composition and properties of the heat-generating agent are shown in Table 1. In the present invention, the amount of the heat-generating agent is 2.5-3kg / t, preferably 2.6-2.8kg / t. In the present invention, the method of adding the heat-generating agent comprises: after the cap mouth is filled with the fourth molten steel to a height greater than two-thirds, 40-60% of the heat-generating agent is added, and the remaining heat-generating agent is added before the end of pouring; more preferably, after the cap mouth is filled with the fourth molten steel to a height greater than two-thirds, 50% of the heat-generating agent is added, and the remaining heat-generating agent is added before the end of pouring. The present invention controls the amount of the heat-generating agent within the above range, advances the actual control point of addition, can improve the heating effect, reduce the shrinkage compensation of the ingot riser, and reduce the riser shrinkage cavity.
[0066] Table 1 Main components and properties of heating agent
[0067]
[0068] The present invention provides a 316LN stainless steel ingot for a BEST vacuum chamber produced by the method described in the above technical solution. The chemical composition of the 316LN stainless steel ingot for a BEST vacuum chamber is preferably as shown in Table 2.
[0069] Table 2 Chemical composition of 316LN stainless steel ingot for BEST vacuum chamber
[0070]
[0071]
[0072] The present invention provides a method for preparing a 316LN stainless steel plate for a BEST vacuum chamber, comprising the following steps:
[0073] The BEST vacuum chamber described in the above technical solution is forged with 316LN stainless steel ingot to obtain a 316LN stainless steel slab;
[0074] The 316LN stainless steel slab is heat treated to obtain a 316LN stainless steel plate for a BEST vacuum chamber.
[0075] The present invention forges the BEST vacuum chamber described in the above technical solution with 316LN stainless steel ingot to obtain 316LN stainless steel slab. The present invention has no special requirements for the forging, and the forging process well known to those skilled in the art can be used.
[0076] After obtaining the 316LN stainless steel slab, the present invention heat treats the 316LN stainless steel slab to obtain a 316LN stainless steel plate for a BEST vacuum chamber. In the present invention, the heat treatment procedure preferably includes: heating to 1050-1150°C with a furnace, keeping warm for 1.5-3.5 hours, and then water cooling to room temperature. In the present invention, the heating rate of the furnace heating is preferably ≤200°C / h, more preferably 160-180°C / h. In the present invention, the atmosphere of the heat treatment is preferably an air atmosphere.
[0077] In the present invention, the size of the 316LN stainless steel plate for the BEST vacuum chamber is preferably 70-71 mm×596-598 mm×8580-8600 mm.
[0078] In the present invention, the elastic modulus of the 316LN stainless steel plate used for the BEST vacuum chamber is ≥190GPa, the yield strength is ≥250MPa, the tensile strength is ≥480MPa, and the elongation after fracture is ≥40%.
[0079] In the present invention, the 316LN stainless steel plate for BEST vacuum chamber does not contain any ferrite and σ phase. In the present invention, the magnetic permeability μ≤1.03 of the 316LN stainless steel plate for BEST vacuum chamber. In the present invention, the grain size of the 316LN stainless steel plate for BEST vacuum chamber is within the range of ±1 equivalent grain number and is uniformly distributed near the true average value; the grain size is ≥3 levels.
[0080] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0081] Example 1
[0082] 1. Electric furnace melting scrap steel process
[0083] The electric furnace uses all scrap steel for smelting. High-nickel scrap steel and high-chromium scrap steel are heated by electric arc. After the scrap steel is dissolved and reaches 1660℃, the top slag is removed, the temperature is controlled at 1650℃ to allow steel tapping, and then the molten steel is poured into the tundish.
[0084] 2. VODC molten steel refining process
[0085] 2.1. Pulling slag
[0086] After the crude molten steel comes out of the furnace, the slag removal operation is carried out in the tundish, and the slag amount of the molten steel is less than 1.8kg / t.
[0087] 2.2、Steel
[0088] After the molten steel is poured into the VODC furnace, samples are taken to measure the temperature, and slag is added: 15kg / t lime, 2.5kg / t fluorite, and 1.2kg / t aluminum.
[0089] 2.3. VOD (Vacuum Oxygen Decarburization)
[0090] The vacuum degree is 100mbar, and the bottom blowing flow rate is controlled at 5.8m 3 / h.
[0091] After the oxygen blowing is completed, VCD operation can be carried out directly without breaking the air.
[0092] The total oxygen consumption in the VOD stage is obtained according to Formula I:
[0093] O used =O total ×M w , Formula I;
[0094] In the formula I, O used Total oxygen consumption in the VOD stage, in Nm 3 ;O total Oxygen consumption per ton of steel, in Nm 3 / t, calculated by formula II; M w is the weight of molten steel, in t;
[0095] O total =1 / eta×[9.31×(C1-C2)+7.98×Si1+6.22×A1]+3.22×(Cr1-Cr2), formula II;
[0096] In the formula II, eta is oxygen release, and its value is 0.75; C1 is the initial carbon content by mass percentage; C2 is the final carbon content by mass percentage; Si1 is the initial silicon content by mass percentage; Al is the initial aluminum content by mass percentage; Cr1 is the initial chromium content by mass percentage; Cr2 is the expected chromium content by mass percentage.
[0097] 2.4. VCD (Vacuum Carbon Deoxidation)
[0098] Vacuum degree <3mbar, bottom blowing argon flow rate controlled at 5~6m 3 / h.
[0099] VCD processing time is 10 to 12 minutes.
[0100] 2.5. VOH (vacuum aluminum thermal method heating)
[0101] After VCD, the vacuum is broken and the temperature is measured. The temperature of the molten steel is 1650℃, and there is no need for VOH operation.
[0102] 2.6. VD (vacuum degassing)
[0103] After VCD is completed, the vacuum is broken and slag is added: lime 15kg / t, fluorite 2.3kg / t, reducing agent ferrosilicon 6kg / t, aluminum 3kg / t, and alloy is added according to the sampling results.
[0104] After VOH, the vacuum is not broken and VD operation is performed directly.
[0105] VD stage parameters: vacuum degree is 2mbar, bottom blowing argon flow rate is controlled at 5.5m 3 / h.
[0106] 2.7. Steel placement
[0107] After VD is completed, temperature measurement and sampling are carried out. When the composition enters the control range and the temperature is ≥ the pouring temperature + 70℃, a steel release signal is issued;
[0108] The ladle should be fully baked before lifting, and the slide device should be installed and adjusted to ensure it is well installed.
[0109] After the ladle is in place, it is connected to argon gas, checked to make sure there are no leaks in the pipeline, and then hoisted into the pit.
[0110] Turn on the argon gas before placing the steel. Pay attention to the surface of the molten steel during the placing process and adjust the argon gas flow rate to prevent the molten steel from being exposed.
[0111] 3. Pouring process:
[0112] 3.1. Adjust the argon flow rate to 2.0Nm before pouring 3 / h, and sedation is carried out for 12 minutes to allow the inclusions to fully float up;
[0113] 3.2. After the quenching is completed, align the ladle outlet with the bell mouth of the center pouring pipe for pouring. During the pouring, a fully enclosed argon protection device is used, the argon pressure is controlled at 0.8MPa, the molten steel temperature is 1520℃, and the pouring operation is carried out;
[0114] 3.3. When pouring, start pouring fully, and start to collect the protective slag as it falls. Control the rate at 1.8 tons / minute. Increase to 1.9 tons / minute after pouring 2 / 3. Pour the ingot body in three stages. The shrinkage time of the riser (the time for pouring the riser) is greater than 2 / 3 of the time for pouring the ingot body to ensure good shrinkage compensation.
[0115] 3.4. Titanium steel protective slag is used as protective slag, and the amount added is 2.1kg / t in a hanging manner to ensure that the slag surface does not show redness or crust;
[0116] 3.5. After the molten steel is filled to more than two-thirds of the cap mouth, add 1.5kg / t of exothermic agent. When the pouring is almost finished, add another 1.5kg / t of exothermic agent to obtain 316LN stainless steel ingot for BEST vacuum chamber.
[0117] Example 2
[0118] The preparation method is basically the same as that of Example 1, except that the vacuum is broken after VCD and the temperature is measured, and the temperature of the molten steel is 1600°C;
[0119] During VOH operation, aluminum is added to increase the temperature by thermite method. The heat released by oxidation of 1kg / t aluminum is calculated to increase by 20°C (temperature loss during oxygen blowing is not considered).
[0120] VOH stage parameters: vacuum degree 400mbar, bottom blowing argon flow rate 5.5m 3 / h.
[0121] The amount of oxygen used to burn aluminum is calculated by formula III;
[0122] O' total =0.62×m Al , Formula III;
[0123] In the formula III, O' total The amount of oxygen used to burn aluminum, in Nm 3 ;m Al is the mass of aluminum added, in kg; 0.62 is the coefficient, in Nm 3 / kg.
[0124] The chemical composition of the 316LN stainless steel ingots for BEST vacuum chambers prepared in Example 1 and Example 2 is shown in Table 3.
[0125] Table 3 Chemical composition of 316LN stainless steel ingot for BEST vacuum chamber
[0126]
[0127] Example 3
[0128] The BEST vacuum chamber prepared in Example 1 is forged with a 316LN stainless steel ingot to obtain a 316LN stainless steel slab;
[0129] The 316LN stainless steel plate blank was heated to 1120° C. at a heating rate of 160° C. / h in an air atmosphere, kept at that temperature for 3 hours, and then water-cooled to room temperature to obtain a 316LN stainless steel plate for a BEST vacuum chamber.
[0130] Test Case
[0131] (1) The size of the 316LN stainless steel plate for BEST vacuum chamber prepared in Example 3 is 70 mm × 596 mm × 8580 mm. The overall straightness and flatness of the 316LN stainless steel plate for BEST vacuum chamber are ≤10 mm, and the straightness and flatness of each 2 m are ≤3 mm. After removing the oxide scale and polishing or processing to bright finish, Ra≤6.3 μm.
[0132] (2) The 316LN stainless steel plate for the BEST vacuum chamber prepared by the present invention does not need to be pickled and passivated before use.
[0133] (3) The mechanical properties of the 316LN stainless steel plate for BEST vacuum chamber prepared in Example 3 are shown in Table 4, and the standard for testing each property is GB / T4237-2015.
[0134] Table 4 Mechanical properties of 316LN stainless steel plate for BEST vacuum chamber prepared in Example 3
[0135]
[0136] (4) The ferrite content of the material is analyzed as required. The material should be in the austenite region above the 0% ferrite line on the Delong diagram (JIS Z3119 Figure 2). According to GB / T 13305 (or ASTM E562), no ferrite and σ phase can be seen in the 316LN stainless steel plate prepared in Example 3 when observed under a microscope at a certain magnification.
[0137] (5) The relative magnetic permeability of the 316LN stainless steel plate for the BEST vacuum chamber prepared in Example 3 was measured at room temperature. The relative magnetic permeability μ was measured using a Forster magnetometer using the ASTM A342 standard. The magnetic permeability μ of the material was 0.8.
[0138] (6) According to the standard GB / T 6394, the equivalent grain size of the 316LN stainless steel plate for BEST vacuum chamber prepared in Example 3 is determined. The grain size is within the range of ±1 equivalent grain number and is evenly distributed near the true average value. The grain size is level 5.
[0139] (7) Test the number of inclusions according to ASTM E45 method D.
[0140] 1) Microscopic inclusions (intrinsic inclusions detectable with a microscope): Method D is applicable. For inclusions of types A, B, C and D, the severity level of the 316LN stainless steel plate for BEST vacuum chamber prepared in Example 3 is 1. The allowable error is limited to within half a level of the maximum level and cannot exceed 2% of the observation area.
[0141] 2) Macro inclusions (some non-inherent slag inclusions and refractory materials): The 316LN stainless steel plate for BEST vacuum chamber prepared in Example 3 does not contain any macro inclusions.
[0142] (8) Observed under a 500x microscope, there were no carbides or carbonitrides in the 316LN stainless steel plate for BEST vacuum chamber prepared in Example 3. The test was conducted according to the A method of GB / T 4334 and compared with the image in the standard. The result of intergranular corrosion was qualified. If the microscopic photographs taken are inconsistent with the standard, the test should be conducted again according to the E method of GB / T4334, and the test results shall be based on the E method of GB / T 4334.
[0143] (9) Ultrasonic testing: in accordance with EN10307 standard Table 4 internal S3 and Table 5 edge E4 level.
[0144] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A method for producing 316LN stainless steel ingots for BEST vacuum chambers using a VODC refining furnace. The following steps are involved: According to the chemical composition of 316LN stainless steel used in BEST vacuum chamber, the scrap steel raw materials are smelted to obtain molten steel; The molten steel and the first slag are mixed and vacuum oxygen blowing and decarburization is performed to obtain a first molten steel; the first slag comprises lime, fluorite and aluminum; The total amount of oxygen used in the vacuum oxygen blowing decarburization process is obtained according to Formula I: O used =O total ×M w , Formula I; In the formula I, O used The total amount of oxygen used in the vacuum oxygen decarburization process, in Nm 3 ;O total Oxygen consumption per ton of steel, in Nm 3 / t, calculated by formula II; M w is the weight of molten steel, in t; O total = 1 / eta × [9.31 × (C 1 - C 2 ) + 7.98 × Si 1 + 6.22 × Al] + 3.22 × (Cr 1 - Cr 2 ), Equation II; In the formula II, eta is oxygen release, and its value is 0.75; C 1 is the initial carbon content mass percentage; C 2 is the final carbon content mass percentage; Si 1 is the mass percentage of initial silicon content; Al is the mass percentage of initial aluminum content; Cr 1 is the initial chromium content mass percentage; Cr 2 is the estimated chromium content in mass percentage; The first molten steel is subjected to vacuum carbon deoxidation to obtain a second molten steel; The second molten steel and second slag are mixed and vacuum degassed to obtain a third molten steel; the second slag comprises lime, fluorite, a reducing agent and aluminum; According to the proportion of the second molten steel, the amount of the second slag material added includes: 14-17 kg / t of lime, 1.5-3.0 kg / t of fluorite, 5-7 kg / t of reducing agent, and 2-4 kg / t of aluminum; The third molten steel is calmed to obtain a fourth molten steel; the calming time is 8 to 15 minutes; The fourth molten steel is poured to obtain a 316LN stainless steel ingot for a BEST vacuum chamber; The pouring start temperature is 1530±10℃; protective slag and heating agent are added during the pouring process; the amount of protective slag is 2.0~2.5kg / t; the protective slag is titanium steel protective slag; the main component of the titanium steel protective slag is Al 2 O 3 15.7%, C 4.1%, CaO 23.6%, SiO 2 43.6%, H 2 O 0.35%; the amount of the exothermic agent is 2.5~3kg / t; the method for adding the exothermic agent comprises: after the fourth molten steel is filled to more than two-thirds of the height at the cap mouth, 40~60% of the exothermic agent is added, and the remaining exothermic agent is added before the end of pouring; The composition of the 316LN stainless steel ingot for the BEST vacuum chamber is as follows, by mass percentage: Cr 17.00-18.50; Ni 12.00-14.00; C 0.024; Si ≤1.00; Mn 1.50-2.00; Mo 2.25-3.00; N 0.185; P ≤0.030; S ≤0.020; Co ≤0.10; Nb ≤0.05; B ≤0.03; Fe and the rest; delta ferrite = 0%.
2. The method according to claim 1, It is characterized in that According to the proportion of the first slag to the molten steel, the addition amount of the first slag includes: 14-17 kg / t of lime, 1.5-3.0 kg / t of fluorite, and 1-1.5 kg / t of aluminum.
3. The method according to claim 1, It is characterized in that The vacuum degree of the vacuum oxygen decarburization is 80-120 mbar, and the bottom blowing gas of the vacuum oxygen decarburization is argon; the bottom blowing argon flow rate is controlled at 3-6 m 3 / h.
4. The method according to claim 1, It is characterized in that The vacuum degree of the vacuum carbon deoxidation is less than 5mbar, the bottom blowing gas of the vacuum carbon deoxidation is argon, and the bottom blowing argon flow rate is controlled at 3-6m 3 / h, and the treatment time of the vacuum carbon deoxidation is 8-12min.
5. The method according to claim 1, It is characterized in that The temperature of the second molten steel is measured. When the temperature of the second molten steel is ≥1650° C., the temperature is not increased; when the temperature of the second molten steel is <1650° C., the temperature is increased.
6. 316LN stainless steel ingot for BEST vacuum chamber produced by the method according to any one of claims 1 to 5.
7. A method for preparing 316LN stainless steel plate for BEST vacuum chamber, The following steps are involved: Forging the BEST vacuum chamber of claim 6 with a 316LN stainless steel ingot to obtain a 316LN stainless steel slab; The 316LN stainless steel slab is heat treated to obtain a 316LN stainless steel plate for a BEST vacuum chamber.
8. The preparation method according to claim 7, It is characterized in that The heat treatment procedure includes: heating to 1050-1150° C. at a heating rate of ≤200° C. / h, keeping the temperature for 1.5-3.5 hours, and then cooling to room temperature with water.