Bismuth zinc niobate composite sol and preparation method thereof, bismuth zinc niobate composite film and preparation method thereof

Through the preparation of bismuth zinc niobate composite sol and Ca2+ doping, the problem of high dielectric loss of existing BST ferroelectric films is solved, and the bismuth zinc niobate composite film with high dielectric constant and low dielectric loss is achieved, which simplifies the The preparation process and improves the integrated application potential of materials.

CN117945459BActive Publication Date: 2024-11-08QILU UNIVERSITY OF TECHNOLOGY (SHANDONG ACADEMY OF SCIENCES)
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410160035.5
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-02-05
Publication Date
2024-11-08
Estimated Expiration
2044-02-05

AI Technical Summary

Technical Problem

The existing perovskite structure (BST) ferroelectric films have too high dielectric loss due to internal intrinsic characteristics, which limits their application under high frequency conditions and requires a higher bias voltage electric field to obtain higher The dielectric tuning rate limits the integrated application of BZN films.

Method used

The preparation method of bismuth zinc niobate composite sol was adopted. By doping the chemical composition of Bi1.5CaxZn1-xNbO7 with Ca2+ ions, the dielectric properties were improved by using the matching properties of Ca2+ and Zn2+ ions, and the sol-gel method was used to prepare excellent Dielectric properties of bismuth zinc niobate composite film.

Benefits of technology

A dielectric film with a dielectric constant of 110 to 120 at a frequency of 1MHz and a dielectric loss of ≤0.008 was realized. It has excellent dielectric properties and simplified the preparation process to obtain a dielectric material with uniform components and high purity.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN117945459B_ABST
    Figure CN117945459B_ABST
Patent Text Reader

Abstract

The present invention belongs to the technical field of dielectric materials, and specifically relates to a bismuth zinc niobate composite sol and a preparation method thereof, a bismuth zinc niobate composite film and a preparation method thereof. The present invention provides a bismuth zinc niobate composite sol, the chemical composition of the bismuth zinc niobate composite sol is Bi 1.5 Ca x Zn 1‑x NbO7, the value range of x is 0.1 to 0.25. 2+ Bi-doped 1.5 ZnNbO7 dielectric material. Among them, Ca 2+ Ions and Zn 2+ The ion radius and ion polarizability of the ions are similar, that is, the ion matching is good, and Ca is used. 2+ Doping can improve the pure phase Bi 1.5 The dielectric properties of the ZnNbO7 dielectric material can be seen from the test results of the embodiments that the dielectric film prepared by the bismuth zinc niobate composite sol provided by the present invention has a dielectric constant of 110-120 at a frequency of 1 MHz and a dielectric loss of ≤0.008, and has excellent dielectric properties.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of dielectric materials, and specifically relates to a bismuth zinc niobate composite sol and a preparation method thereof, and a bismuth zinc niobate composite film and a preparation method thereof. Background Art

[0002] Microwave technology is one of the major achievements in the development of modern science and technology. Microwaves have many advantages, such as short wavelength, high frequency, strong directivity, large information capacity, and the ability to penetrate the ionosphere. Therefore, they have been widely used in radar, microwave communication, satellite communication, mobile phones and other fields. Due to the application requirements of new electric field tuning devices such as resonators, couplers, filters, etc. under high frequency conditions, the research on tunable dielectric films has become a hot topic. By researching and developing tunable dielectric films, the performance and efficiency of microwave devices can be improved, further promoting the development and application of microwave technology. This is of great significance to the military, industrial and civilian fields, and helps to improve the performance of communication and radar systems, increase data transmission rates, and promote the development of wireless communication technology.

[0003] Based on the above needs, researchers have studied the perovskite structure (Ba x Sr 1-x )TiO3 (BST) ferroelectric thin films have been studied a lot, but new high-performance dielectric tuning thin film materials are still needed to solve the problem of excessive dielectric loss caused by the internal intrinsic properties of BST ferroelectric films. 1.5 ZnB 1.5 O7 (BZN) dielectric tuning film material not only has low dielectric loss but also exhibits excellent dielectric tunability, with smaller dielectric loss than BST film. However, in order to obtain a higher dielectric tuning rate, a very high bias electric field needs to be loaded on the film, which limits the integrated application of BZN film. Summary of the invention

[0004] The purpose of the present invention is to provide a bismuth zinc niobate composite sol and a preparation method thereof, a bismuth zinc niobate composite film and a preparation method thereof. The composite film prepared from the bismuth zinc niobate composite sol provided by the present invention has excellent dielectric properties.

[0005] In order to achieve the above object, the present invention provides the following technical solutions:

[0006] The present invention provides a bismuth zinc niobate composite sol, wherein the chemical composition of the bismuth zinc niobate composite sol is Bi 1.5 Ca x Zn 1-x NbO7, the value range of x is 0.1 to 0.25.

[0007] The present invention also provides a method for preparing the bismuth zinc niobate composite sol described in the above technical solution, comprising the following steps:

[0008] mixing a solution containing a niobium source and a precipitant to obtain a Nb(OH)5 precipitate;

[0009] Mixing the Nb(OH)5 precipitate and the chelating agent to obtain a precursor solution;

[0010] The precursor solution, the solution containing a bismuth source, the solution containing a calcium source and the solution containing a zinc source are mixed, the pH value of the obtained mixed solution is adjusted to be acidic, and then a gel reaction is performed to obtain the bismuth zinc niobate composite sol.

[0011] Preferably, the solution containing a niobium source is a NbF5 solution;

[0012] The preparation method of the NbF5 solution comprises the following steps: mixing Nb2O5 with hydrofluoric acid, reacting to obtain the NbF5 solution;

[0013] The mass concentration of the hydrofluoric acid is 99.99%, and the molar ratio of Nb2O5 to hydrofluoric acid is 1:10-15; the reaction temperature is 150°C, and the reaction time is 2-3 hours.

[0014] Preferably, the precipitant comprises ammonium bicarbonate and concentrated aqueous ammonia, and the molar ratio of the ammonium bicarbonate to the concentrated aqueous ammonia is 1:3-5.

[0015] Preferably, the chelating agent comprises tartaric acid and citric acid, and the molar ratio of tartaric acid to citric acid is 1:4;

[0016] Calculated on the molar amount of niobium, the molar ratio of the Nb(OH)5 precipitate to the chelating agent is 1:6-8.

[0017] Preferably, the bismuth source in the bismuth source-containing solution includes BiCl3 or Bi(NO3)3·5H2O; the solvent of the bismuth source-containing solution is an acidic reagent; the molar ratio of the bismuth source to the acidic reagent is 1:1.2-1.5;

[0018] The calcium source in the solution containing the calcium source includes CaCl2 or Ca(NO3)2·4H2O; the solvent of the solution containing the calcium source is an acidic reagent; the molar ratio of the calcium source to the acidic reagent is 1:1.2-1.5;

[0019] The zinc source in the solution containing the zinc source includes ZnCl2 or Zn(NO3)2·6H2O; the solvent of the solution containing the zinc source is an acidic reagent; the molar ratio of the zinc source to the acidic reagent is 1:1.2-1.5.

[0020] Preferably, the acidic pH value is 3 to 5;

[0021] The temperature of the gel reaction is 70-80°C.

[0022] The present invention also provides a bismuth zinc niobate composite film, which is obtained by coating with a sol as a raw material, wherein the sol is the bismuth zinc niobate composite sol described in the above technical scheme or the bismuth zinc niobate composite sol prepared by the preparation method described in the above technical scheme.

[0023] The present invention also provides a method for preparing the bismuth zinc niobate composite film described in the above technical solution, comprising the following steps:

[0024] The sol is coated on the surface of the substrate, and drying and crystallization treatments are performed in sequence to obtain the bismuth zinc niobate composite film.

[0025] Preferably, the drying temperature is 110-150°C and the drying time is 10 minutes;

[0026] The temperature of the crystallization treatment is 600-650° C., and the insulation time is 1 hour.

[0027] The present invention provides a bismuth zinc niobate composite sol, wherein the chemical composition of the bismuth zinc niobate composite sol is Bi 1.5 Ca x Zn 1-x NbO7, the value range of x is 0.1 to 0.25. 2+ Bi-doped 1.5 ZnNbO7 dielectric material. Among them, Ca 2+ Ions and Zn 2+ The ion radius and ion polarizability of the ions are similar, that is, the ion matching is good, and Ca is used. 2+ Doping can improve the pure phase Bi 1.5 Dielectric properties of ZnNbO7 dielectric materials: According to the test results of the examples, the dielectric film prepared from the bismuth zinc niobate composite sol provided by the present invention has a dielectric constant of 110-120 at a frequency of 1 MHz and a dielectric loss of ≤0.008, and has excellent dielectric properties.

[0028] The present invention also provides a method for preparing the bismuth zinc niobate composite sol described in the above technical solution, comprising the following steps: mixing a solution containing a niobium source and a precipitant to obtain a Nb(OH)5 precipitate; mixing the Nb(OH)5 precipitate and a chelating agent to obtain a precursor solution; mixing the precursor solution, a solution containing a bismuth source, a solution containing a calcium source, and a solution containing a zinc source, adjusting the pH value of the obtained mixed solution to be acidic, and then performing a gel reaction to obtain the bismuth zinc niobate composite sol. The present invention uses a sol-gel method to prepare a bismuth zinc niobate composite sol. Compared with the prior art, the preparation process is simple, and a dielectric material with uniform components and high purity can be obtained. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 The XRD diagram of the bismuth zinc niobate composite film obtained in Examples 1 to 4;

[0030] Figure 2 The SEM images of the bismuth zinc niobate composite films obtained in Examples 1 to 4;

[0031] Figure 3 The dielectric properties test results of the bismuth zinc niobate composite films obtained in Examples 1 to 4;

[0032] Figure 4 The present invention provides a schematic flow chart of the preparation method. DETAILED DESCRIPTION

[0033] The present invention provides a bismuth zinc niobate composite sol, wherein the chemical composition of the bismuth zinc niobate composite sol is Bi 1.5 Ca x Zn 1-x NbO7, the value range of x is 0.1 to 0.25.

[0034] In the present invention, the value range of x is 0.1 to 0.25, and more preferably 0.15 to 0.2.

[0035] In the present invention, the bismuth zinc niobate composite sol preferably has a cubic pyrochlore structure, and the space group is preferably Fd-3m (227).

[0036] The present invention also provides a method for preparing the bismuth zinc niobate composite sol described in the above technical solution, comprising the following steps:

[0037] mixing a solution containing a niobium source and a precipitant to obtain a Nb(OH)5 precipitate;

[0038] Mixing the Nb(OH)5 precipitate and the chelating agent to obtain a precursor solution;

[0039] The precursor solution, the solution containing a bismuth source, the solution containing a calcium source and the solution containing a zinc source are mixed, the pH value of the obtained mixed solution is adjusted to be acidic, and then a gel reaction is performed to obtain the bismuth zinc niobate composite sol material.

[0040] In the present invention, unless otherwise specified, all preparation raw materials are commercially available products well known to those skilled in the art.

[0041] The present invention mixes a solution containing a niobium source and a precipitant to obtain a Nb(OH)5 precipitate.

[0042] In the present invention, the solution containing niobium source is preferably NbF5 solution. In the present invention, the method for preparing the NbF5 solution preferably comprises the following steps: mixing Nb2O5 and hydrofluoric acid, reacting to obtain the NbF5 solution. In the present invention, the purity of Nb2O5 is preferably 99.99%. In the present invention, the mass concentration of hydrofluoric acid is preferably 99.99%; the molar ratio of Nb2O5 to hydrofluoric acid is preferably 1:10-15. In the present invention, the reaction temperature is preferably 150°C, and the reaction time is preferably 2-3h.

[0043] In the present invention, the precipitant preferably comprises ammonium bicarbonate and concentrated ammonia water, the mass concentration of the concentrated ammonia water is preferably 25-28%, and the molar ratio of the ammonium bicarbonate to the concentrated ammonia water is preferably 1:3-5. In the present invention, the preparation method of the precipitant preferably comprises the following steps: mixing a saturated ammonium bicarbonate solution and ammonia water to obtain the precipitant.

[0044] The present invention has no particular limitation on the ratio of the solution containing the niobium source and the precipitant, and the pH value of the mixed solution can be adjusted to 8-10.

[0045] After the mixing, the present invention also preferably includes centrifuging the obtained mixed system and performing solid-liquid separation.

[0046] After obtaining the Nb(OH)5 precipitate, the present invention mixes the Nb(OH)5 precipitate with a chelating agent to obtain a precursor solution.

[0047] In the present invention, the chelating agent preferably includes tartaric acid (TA) and citric acid (CA), and the molar ratio of tartaric acid to citric acid is preferably 1:4. In the present invention, the molar ratio of the Nb(OH)5 precipitate to the chelating agent is preferably 1:6-8 based on the molar amount of niobium. In the present invention, the preparation method of the chelating agent preferably includes the following steps: dissolving tartaric acid and citric acid in deionized water to obtain a composite chelating agent. The present invention has no special limitation on the amount of deionized water, and the amount familiar to those skilled in the art can be used. In the present invention, citric acid and tartaric acid with stronger complexing ability are used as composite chelating agents when preparing the sol, which is beneficial to improving the stability of the sol, thereby making the dielectric properties of the prepared film better.

[0048] In the present invention, the Nb(OH)5 precipitate and the chelating agent are preferably mixed under stirring; the stirring temperature is preferably 70-80° C. The present invention has no particular limitation on the stirring time, as long as the Nb(OH)5 precipitate is completely dissolved.

[0049] After obtaining the precursor solution, the present invention mixes the precursor solution, a solution containing a bismuth source, a solution containing a calcium source and a solution containing a zinc source, adjusts the pH value of the obtained mixed solution to be acidic, and then performs a gel reaction to obtain the bismuth zinc niobate composite sol material.

[0050] In the present invention, the bismuth source in the bismuth source-containing solution preferably includes BiCl3 or Bi(NO3)3·5H2O; the purity of the bismuth source is preferably 99.99%; the solvent of the bismuth source-containing solution is preferably an acidic reagent; when the bismuth source is BiCl3, the acidic reagent is preferably hydrochloric acid, and the mass concentration of the hydrochloric acid is preferably 37%; when the bismuth source is Bi(NO3)3·5H2O, the acidic reagent is preferably nitric acid; the mass concentration of the nitric acid is preferably 65%; the molar ratio of the bismuth source to the acidic reagent is preferably 1:1.2-1.5. In the present invention, the method for preparing the bismuth source-containing solution preferably includes: dissolving the bismuth source in the acidic reagent to obtain the bismuth source-containing solution.

[0051] In the present invention, the calcium source in the solution containing the calcium source preferably includes CaCl2 or Ca(NO3)2·4H2O; the purity of the calcium source is preferably 99.99%; the solvent of the solution containing the calcium source is preferably an acidic reagent; when the calcium source is CaCl2, the acidic reagent is preferably hydrochloric acid, and the mass concentration of the hydrochloric acid is preferably 37%; when the calcium source is Ca(NO3)2·4H2O, the acidic reagent is preferably nitric acid; the mass concentration of the nitric acid is preferably 65%; the molar ratio of the calcium source to the acidic reagent is preferably 1:1.2-1.5. In the present invention, the preparation method of the solution containing the calcium source preferably includes: dissolving the calcium source in the acidic reagent to obtain the solution containing the calcium source.

[0052] In the present invention, the zinc source in the solution containing the zinc source preferably includes ZnCl2 and / or Zn(NO3)2·6H2O; the purity of the zinc source is preferably 99.99%; the solvent of the solution containing the zinc source is preferably an acidic reagent; when the zinc source is ZnCl2, the acidic reagent is preferably hydrochloric acid, and the mass concentration of the hydrochloric acid is preferably 37%; when the zinc source is ZnCl2, the acidic reagent is preferably nitric acid; the mass concentration of the nitric acid is preferably 65%; the molar ratio of the zinc source to the acidic reagent is preferably 1:1.2-1.5. In the present invention, the method for preparing the solution containing the zinc source preferably includes: dissolving the zinc source in the acidic reagent to obtain the solution containing the zinc source.

[0053] In the present invention, the process of mixing the precursor solution, the solution containing a bismuth source, the solution containing a calcium source and the solution containing a zinc source is preferably: under stirring, the solution containing a bismuth source, the solution containing a calcium source and the solution containing a zinc source are dripped into the precursor solution; the stirring temperature is preferably 70-80°C.

[0054] In the present invention, the acidic pH value is preferably 3 to 5; the reagent used for the adjustment is preferably ammonia water. In the present invention, the temperature of the gel reaction is preferably 70 to 80°C. In the present invention, when the solution containing the bismuth source, the solution containing the calcium source and the solution containing the zinc source are dripped into the precursor solution, the gel reaction begins to occur; after the dripping is completed, it is also preferably included to continue stirring; the continuous stirring time is preferably 1 to 2 hours, that is, the gel reaction time of the present application includes the dripping time and the continuous stirring time.

[0055] After the gel reaction, the present invention also preferably includes aging the obtained sol, and the aging time is preferably 24 hours. In the present invention, the aging is preferably carried out under sealed conditions.

[0056] The present invention also provides a bismuth zinc niobate composite film, which is obtained by coating with a sol as a raw material, wherein the sol is the bismuth zinc niobate composite sol described in the above technical scheme or the bismuth zinc niobate composite sol prepared by the preparation method described in the above technical scheme.

[0057] In the present invention, the bismuth zinc niobate composite film preferably has a cubic pyrochlore structure.

[0058] The present invention also provides a method for preparing the bismuth zinc niobate composite film described in the above technical solution, comprising the following steps:

[0059] The sol is coated on the surface of the substrate, and drying and crystallization treatments are performed in sequence to obtain the bismuth zinc niobate composite film.

[0060] In the present invention, the substrate preferably includes an ITO substrate. Before the coating, the present invention also preferably includes pre-treating the substrate; the pre-treatment preferably includes: placing the substrate in deionized water, acetone, anhydrous ethanol and deionized water in sequence for ultrasonication, and the ultrasonication time in each solvent is preferably 15 minutes, and the impurities on the surface of the substrate are removed by pre-treatment.

[0061] In the present invention, the coating method is preferably vacuum spin coating. The present invention has no special limitation on the vacuum spin coating process, and the method well known to those skilled in the art can be used.

[0062] In the present invention, the drying temperature is preferably 110-150° C., and the drying time is preferably 10 min. In the present invention, the crystallization temperature is preferably 600-650° C., and the holding time is preferably 1 h.

[0063] In the present invention, the above-mentioned coating, drying and crystallization treatment processes are preferably repeated until a bismuth zinc niobate composite film of a desired thickness is obtained; the number of repetitions is preferably 5 to 7 times.

[0064] The schematic flow diagram of the preparation method provided by the present invention is as follows Figure 4 shown.

[0065] To further illustrate the present invention, a bismuth zinc niobate composite sol and a preparation method thereof, a bismuth zinc niobate composite film and a preparation method thereof provided by the present invention are described in detail below in conjunction with the accompanying drawings and examples, but they should not be construed as limiting the scope of protection of the present invention.

[0066] Example 1

[0067] The chemical composition of the bismuth zinc niobate composite sol obtained in this example is Bi 1.5 Ca 0.1 Zn 0.9 NbO7, weigh the required raw materials according to the stoichiometric ratio;

[0068] Weigh high-purity (99.99%) Nb2O5, put Nb2O5 and hydrofluoric acid (HF, mass concentration of 99.99%) into a reactor at a molar ratio of 1:10, and react at 150°C for 2h to obtain a NbF5 solution;

[0069] Preparation of precipitant: The precipitant is a mixture of saturated ammonium bicarbonate and concentrated ammonia water, with a molar ratio of 1:3;

[0070] Adding a precipitant to the NbF5 solution, adjusting the pH value to 8; centrifuging the solution, and performing solid-liquid separation to obtain Nb(OH)5 precipitate;

[0071] Tartaric acid (TA) and citric acid (CA) were dissolved in deionized water to prepare a composite chelating agent, wherein the molar ratio of tartaric acid to citric acid was 1:4;

[0072] The Nb(OH)5 precipitate was added to the composite chelating agent, heated in a water bath at 70°C and stirred until the precipitate dissolved to obtain a precursor solution, wherein Nb 5+ The molar ratio with the complex chelating agent is 1:6;

[0073] Weigh high-purity (99.99%) BiCl3 and dissolve it in 37% HCl. To ensure complete dissolution, the molar ratio of bismuth chloride to HCl is 1:1.2 to obtain BiCl3.3+ Precursor fluid;

[0074] Weigh high-purity (99.99%) ZnCl2 and dissolve it in 37% HCl with a molar ratio of zinc chloride to HCl of 1:1.2 to obtain Zn 2+ Precursor fluid;

[0075] Weigh high-purity (99.99%) CaCl2 and dissolve it in 37% HCl with a molar ratio of calcium chloride to HCl of 1:1.2 to obtain CaCl2. 2+ Precursor fluid;

[0076] Bi 3+ Precursor, Zn 2+ Precursor solution and Ca 2+ The precursor solution is slowly added dropwise to the precursor solution, and the solution is heated and stirred in a water bath at 70° C. during the whole process. After the addition is completed, the pH value of the solution is adjusted to 3 using aqueous ammonia. After continuing to heat and stir for 1 hour, the sol is taken out to obtain the sol. In order to improve the purity of the sol, the sol is sealed and aged for 24 hours to obtain the bismuth zinc niobate composite sol.

[0077] The ITO glass substrate was placed in deionized water, acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 15 minutes each to remove impurities on the substrate surface; the obtained bismuth zinc niobate composite sol was coated on the pretreated ITO glass substrate using a vacuum spin coater, and the substrate covered with the wet film was placed on a heating plate, dried at 150°C for 10 minutes, and then placed in a tube furnace for crystallization at 600°C for 1 hour to obtain a layer of doped bismuth zinc niobate (BCZN) film on the substrate. The above operation was repeated 5 times until the desired thickness was obtained, and finally a BCZN composite film with a cubic pyrochlore structure was obtained.

[0078] Example 2

[0079] The chemical composition of the bismuth zinc niobate composite sol obtained in this example is Bi 1.5 Ca 0.15 Zn 0.85 NbO7, weigh the required raw materials according to the stoichiometric ratio;

[0080] Weigh high-purity (99.99%) Nb2O5, put Nb2O5 and hydrofluoric acid (HF, mass concentration of 99.99%) into a reactor at a molar ratio of 1:12, and react at 150°C for 2h to obtain a NbF5 solution;

[0081] Preparation of precipitant: The precipitant is a mixture of saturated ammonium bicarbonate and concentrated ammonia water, with a molar ratio of 1:5;

[0082] Adding a precipitant to the NbF5 solution, adjusting the pH value to 9; centrifuging the solution, and performing solid-liquid separation to obtain Nb(OH)5 precipitate;

[0083] Tartaric acid (TA) and citric acid (CA) were dissolved in deionized water to prepare a composite chelating agent, wherein the molar ratio of tartaric acid to citric acid was 1:4;

[0084] The Nb(OH)5 precipitate was added to the composite chelating agent, heated in a water bath at 75°C and stirred until the precipitate dissolved to obtain a precursor solution, wherein Nb 5+ The molar ratio with the complex chelating agent is 1:6;

[0085] Weigh high-purity (99.99%) BiCl3 and dissolve it in 37% HCl. To ensure complete dissolution, the molar ratio of bismuth chloride to HCl is 1:1.3 to obtain BiCl3. 3+ Precursor fluid;

[0086] Weigh high-purity (99.99%) ZnCl2 and dissolve it in 37% HCl with a molar ratio of zinc chloride to HCl of 1:1.3 to obtain Zn 2+ Precursor fluid;

[0087] Weigh high-purity (99.99%) CaCl2 and dissolve it in 37% HCl with a molar ratio of calcium chloride to HCl of 1:1.3 to obtain CaCl2. 2+ Precursor fluid;

[0088] Bi 3+ Precursor, Zn 2+ Precursor solution and Ca 2+ The precursor solution was slowly added dropwise to the precursor solution, and the solution was heated and stirred in a water bath at 75° C. during the whole process. After the addition was completed, the pH value of the solution was adjusted to 4 using aqueous ammonia. The solution was taken out after continuing to heat and stir for 1.5 hours to obtain the sol. To improve the purity of the sol, the sol was sealed and aged for 24 hours to obtain the bismuth zinc niobate composite sol.

[0089] The ITO glass substrate was placed in deionized water, acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 15 minutes each to remove impurities on the substrate surface; the obtained bismuth zinc niobate composite sol was coated on the pretreated ITO glass substrate using a vacuum spin coater, and the substrate covered with the wet film was placed on a heating plate, dried at 120°C for 10 minutes, and then placed in a tube furnace for crystallization at 625°C for 1 hour to obtain a layer of doped bismuth zinc niobate (BCZN) film on the substrate. The above operation was repeated 6 times until the desired thickness was obtained, and finally a BCZN composite film with a cubic pyrochlore structure was obtained.

[0090] Example 3

[0091] The chemical composition of the bismuth zinc niobate composite sol obtained in this example is Bi 1.5 Ca 0.2 Zn 0.8 NbO7, weigh the required raw materials according to the stoichiometric ratio;

[0092] Weigh high-purity (99.99%) Nb2O5, put Nb2O5 and hydrofluoric acid (HF, mass concentration of 99.99%) into a reactor at a molar ratio of 1:15, and react at 150°C for 2h to obtain a NbF5 solution;

[0093] Preparation of precipitant: The precipitant is a mixture of saturated ammonium bicarbonate and concentrated ammonia water, with a molar ratio of 1:4;

[0094] Adding a precipitant to the NbF5 solution, adjusting the pH value to 9; centrifuging the solution, and performing solid-liquid separation to obtain Nb(OH)5 precipitate;

[0095] Tartaric acid (TA) and citric acid (CA) were dissolved in deionized water to prepare a composite chelating agent, wherein the molar ratio of tartaric acid to citric acid was 1:4;

[0096] The Nb(OH)5 precipitate was added to the composite chelating agent, heated in a water bath at 80°C and stirred until the precipitate dissolved to obtain a precursor solution, wherein Nb 5+ The molar ratio with the complex chelating agent is 1:8;

[0097] Weigh high-purity (99.99%) BiCl3 and dissolve it in 37% HCl. To ensure complete dissolution, the molar ratio of bismuth chloride to HCl is 1:1.5 to obtain BiCl3. 3+ Precursor fluid;

[0098] Weigh high-purity (99.99%) ZnCl2 and dissolve it in 37% HCl with a molar ratio of zinc chloride to HCl of 1:1.5 to obtain Zn 2+ Precursor fluid;

[0099] Weigh high-purity (99.99%) CaCl2 and dissolve it in 37% HCl with a molar ratio of calcium chloride to HCl of 1:1.5 to obtain CaCl2. 2+ Precursor fluid;

[0100] Bi 3+ Precursor, Zn 2+ Precursor solution and Ca 2+The precursor solution was slowly added dropwise to the precursor solution, and the solution was heated and stirred in a water bath at 75° C. during the whole process. After the addition was completed, the pH value of the solution was adjusted to 5 using aqueous ammonia. The solution was taken out after continuing to heat and stir for 1.5 hours to obtain the sol. In order to improve the purity of the sol, the sol was sealed and aged for 24 hours to obtain the bismuth zinc niobate composite sol.

[0101] The ITO glass substrate was placed in deionized water, acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 15 minutes each to remove impurities on the substrate surface; the obtained bismuth zinc niobate composite sol was coated on the pretreated ITO glass substrate using a vacuum spin coater, and the substrate covered with the wet film was placed on a heating plate, dried at 130°C for 10 minutes, and then placed in a tube furnace for crystallization at 625°C for 1 hour to obtain a layer of doped bismuth zinc niobate (BCZN) film on the substrate. The above operation was repeated 6 times until the desired thickness was obtained, and finally a BCZN composite film with a cubic pyrochlore structure was obtained.

[0102] Example 4

[0103] The chemical composition of the bismuth zinc niobate composite sol obtained in this example is Bi 1.5 Ca 0.25 Zn 0.75 NbO7, weigh the required raw materials according to the stoichiometric ratio;

[0104] Weigh high-purity (99.99%) Nb2O5, put Nb2O5 and hydrofluoric acid (HF, mass concentration of 99.99%) into a reactor at a molar ratio of 1:15, and react at 150°C for 2h to obtain a NbF5 solution;

[0105] Preparation of precipitant: The precipitant is a mixture of saturated ammonium bicarbonate and concentrated ammonia water, with a molar ratio of 1:4;

[0106] Adding a precipitant to the NbF5 solution, adjusting the pH value to 9; centrifuging the solution, and performing solid-liquid separation to obtain Nb(OH)5 precipitate;

[0107] Tartaric acid (TA) and citric acid (CA) were dissolved in deionized water to prepare a composite chelating agent, wherein the molar ratio of tartaric acid to citric acid was 1:4;

[0108] The Nb(OH)5 precipitate was added to the composite chelating agent, heated in a water bath at 70°C and stirred until the precipitate dissolved to obtain a precursor solution, wherein Nb 5+ The molar ratio with the complex chelating agent is 1:8;

[0109] Weigh high-purity (99.99%) BiCl3 and dissolve it in 37% HCl. To ensure complete dissolution, the molar ratio of bismuth chloride to HCl is 1:1.4 to obtain BiCl3. 3+ Precursor fluid;

[0110] Weigh high-purity (99.99%) ZnCl2 and dissolve it in 37% HCl with a molar ratio of zinc chloride to HCl of 1:1.4 to obtain Zn 2+ Precursor fluid;

[0111] Weigh high-purity (99.99%) CaCl2 and dissolve it in 37% HCl with a molar ratio of calcium chloride to HCl of 1:1.4 to obtain CaCl2. 2+ Precursor fluid;

[0112] Bi 3+ Precursor, Zn 2+ Precursor solution and Ca 2+ The precursor solution is slowly added dropwise to the precursor solution, and the solution is heated and stirred in a water bath at 80° C. during the whole process. After the addition is completed, the pH value of the solution is adjusted to 4 using aqueous ammonia. The solution is taken out after continuing to heat and stir for 1 hour to obtain a sol. To improve the purity of the sol, the sol is sealed and aged for 24 hours to obtain the bismuth zinc niobate composite sol.

[0113] The ITO glass substrate was placed in deionized water, acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 15 minutes each to remove impurities on the substrate surface; the obtained bismuth zinc niobate composite sol was coated on the pretreated ITO glass substrate using a vacuum spin coater, and the substrate covered with the wet film was placed on a heating plate, dried at 150°C for 10 minutes, and then placed in a tube furnace for crystallization at 650°C for 1 hour to obtain a layer of doped bismuth zinc niobate (BCZN) film on the substrate. The above operation was repeated 7 times until the desired thickness was obtained, and finally a BCZN composite film with a cubic pyrochlore structure was obtained.

[0114] Performance Testing

[0115] Test Example 1

[0116] Figure 1 The XRD patterns of the bismuth zinc niobate composite films obtained in Examples 1 to 4 are shown in FIG. 0.1 Z 0.9 N is Example 1, BC 0.25 Z 0.85 N is Example 2, BC 0.2 Z 0.8 N is Example 3, BC 0.25 Z 0.75 N is Example 4; Figure 1 It can be seen that BZN still maintains the cubic pyrochlore structure, Ca 2+ The incorporation of MgO did not destroy its original crystal structure.

[0117] Figure 1The SEM images of the bismuth zinc niobate composite films obtained in Examples 1 to 4 are shown in FIG. Figure 2 It can be seen that the film is uniform, dense and crack-free. 2+ As the doping concentration increases, the average grain size of the sample increases, and Ca 2+ Doping can promote grain growth to a certain extent.

[0118] Test Example 2

[0119] The dielectric properties of the bismuth zinc niobate composite films obtained in Examples 1 to 4 were tested. The testing method was as follows: an Au electrode with a diameter of 400 μm was prepared on the surface of the composite film by vacuum evaporation, and the dielectric properties were tested.

[0120] At 1MHz frequency, the test results are shown in Table 1 and Figure 3 As shown:

[0121] Table 1 Dielectric properties of bismuth zinc niobate composite films obtained in Examples 1 to 4

[0122] Dielectric constant Dielectric loss Example 1 128 0.008 Example 2 120 0.0065 Example 3 118 0.0062 Example 4 115 0.0076

[0123] From Table 1 and Figure 3 It can be seen that Ca 2+ The incorporation of makes the BZN material have lower dielectric loss. Its dielectric constant is 110-120 at a frequency of 1MHz, and the dielectric loss is ≤0.008.

[0124] Although the above embodiment describes the present invention in detail, it is only a part of the embodiments of the present invention, not all of the embodiments. Other embodiments can be obtained based on this embodiment without creativity, and these embodiments all fall within the protection scope of the present invention.

Claims

1. A method for preparing a bismuth zinc niobate composite film, characterized in that: The following steps are involved: According to the stoichiometric ratio Bi 1.5 Ca 0.2 Zn 0.8 Nb 1.5 O7 weighs the required raw materials; Weigh 99.99% pure Nb2O5, put Nb2O5 and 99.99% hydrofluoric acid in a molar ratio of 1:15 into a reactor, and react at 150°C for 2h to obtain a NbF5 solution; Preparation of precipitant: The precipitant is a mixture of saturated ammonium bicarbonate and concentrated ammonia water, with a molar ratio of 1:4; Adding a precipitant to the NbF5 solution, adjusting the pH value to 9; centrifuging the solution, and performing solid-liquid separation to obtain Nb(OH)5 precipitate; Tartaric acid and citric acid are dissolved in deionized water to prepare a composite chelating agent, wherein the molar ratio of tartaric acid to citric acid is 1:4; The Nb(OH)5 precipitate was added to the composite chelating agent, heated in a water bath at 80°C and stirred until the precipitate dissolved to obtain a precursor solution, wherein Nb 5+ The molar ratio with the complex chelating agent is 1:8; Weigh 99.99% pure BiCl3 and dissolve it in 37% HCl. To ensure complete dissolution, the molar ratio of bismuth chloride to HCl is 1:1.5 to obtain BiCl3. 3+ Precursor fluid; Weigh 99.99% pure ZnCl2 and dissolve it in 37% HCl with a molar ratio of zinc chloride to HCl of 1:1.5 to obtain ZnCl2. 2+ Precursor fluid; Weigh 99.99% pure CaCl2 and dissolve it in 37% HCl with a molar ratio of calcium chloride to HCl of 1:1.5 to obtain CaCl2. 2+ Precursor fluid; Bi 3+ Precursor, Zn 2+ Precursor solution and Ca 2+ The precursor solution was slowly added dropwise to the precursor solution, and the solution was heated and stirred in a water bath at 75° C. during the whole process. After the addition was completed, the pH value of the solution was adjusted to 5 using aqueous ammonia. The solution was taken out after continuing to heat and stir for 1.5 hours to obtain the sol. In order to improve the purity of the sol, the sol was sealed and aged for 24 hours to obtain the bismuth zinc niobate composite sol. The ITO glass substrate was sequentially placed in deionized water, acetone, anhydrous ethanol, and deionized water for ultrasonic cleaning for 15 minutes each to remove impurities on the substrate surface; the obtained bismuth zinc niobate composite sol was coated on the pretreated ITO glass substrate using a vacuum spin coater, and the substrate covered with the wet film was placed on a heating plate, dried at 130°C for 10 minutes, and then placed in a tube furnace for crystallization at 625°C for 1 hour to obtain a layer of doped bismuth zinc niobate film on the substrate; the above operation was repeated 6 times until the desired thickness was obtained, and finally a BCZN composite film with a cubic pyrochlore structure was obtained.