Zinc-iron ferrite magnetic nanoparticles and preparation method thereof
By adjusting the raw material ratio and adding pH sustained-release agent and glycerin dispersant, combined with planetary ball milling technology, the problem of uneven composition and agglomeration of ferrite nanoparticles was solved, the magnetic separation pass rate and fluidity were improved, and better Magnetic properties.
Patent Information
- Application Number
- CN202410165441.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-02-05
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-02-05
Smart Images

Figure BDA0004699562550000071
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of biomedical analysis and detection, and in particular to zinc-iron ferrite magnetic nanoparticles and a preparation method thereof. Background Art
[0002] The most explored magnetic nanoparticles are ferrite nanoparticles Zn x Fe 3-x O 4 The preparation method is mainly chemical coprecipitation, and the reaction equation is:
[0003] xZ 2+ +(1-x)Fe 2+ +2Fe 3+ +8OH - =Zn x Fe 3-x O 4 ↓+4H 2 O
[0004] The existing laboratory preparation method of ferrite nanoparticles includes the following steps:
[0005] (1) Take a certain amount of twice distilled water and heat it to full boiling for 30 minutes, then cool the water to room temperature under nitrogen protection to make oxygen-free distilled water;
[0006] (2) According to the proportion of each component of zinc-iron ferrite, weigh a certain mass proportion of FeCl 3 、FeCl 2 、ZnCl 2 The powder is placed in a beaker, dissolved with deoxygenated distilled water, and additives are added. Then, the mixture is heated in a water bath at 60-100°C (different water bath temperatures for different zinc contents) and stirred rapidly. A diluted ammonia weak base solution is added dropwise, and the pH value of the solution is adjusted to 9-11. Black ferrite particles are generated. The entire reaction process is carried out under nitrogen protection.
[0007] (3) After the reaction is completed, the sample is cooled under nitrogen protection, placed on a permanent magnet for magnetic separation, and ultrasonically cleaned multiple times with twice distilled water. Finally, the clean washed sample is dried at room temperature.
[0008] Since the existing preparation method is to add ammonia water dropwise to the reaction solution, the pH value during the reaction is difficult to control accurately, and it changes repeatedly with the progress of the reaction, resulting in uneven composition of the product after the reaction and a low pass rate during magnetic separation. Even when a dispersant is added, the generated ferrite nanoparticles are severely aggregated, the microscopic particle size distribution of the particles is uneven, and the dispersion is poor, which affects the magnetic properties and the fluidity after being made into a magnetic fluid is poor. These problems have become a major difficulty and pain point in the development of magnetic nanoparticle technology that urgently needs to be broken through. Summary of the invention
[0009] In view of this, the first purpose of the present invention is to provide a zinc-iron ferrite magnetic nanoparticle to improve the qualified rate and agglomeration problem of ferrite nanoparticles during magnetic separation. By innovatively designing the raw material ratio and selecting the raw material ratio based on the characteristics of the raw materials used for the ferrite nanoparticles, the composition uniformity of the ferrite nanoparticles is improved, the qualified rate of the magnetic separation process is improved, and the agglomeration problem of ferrite nanoparticles is solved.
[0010] The second object of the present invention is to provide a method for preparing the above zinc-iron ferrite magnetic nanoparticles, which has a simple production process and is convenient for on-site application.
[0011] In order to achieve the above-mentioned purpose of the present invention, the following technical solutions are particularly adopted:
[0012] The present invention provides a zinc-iron ferrite magnetic nanoparticle, the molecular formula of which is Zn x Fe 3-x O 4 , mainly composed of ferric chloride (FeCl 3 )2mol / L, ferric chloride (FeCl 2 )x mol / L, zinc dichloride (ZnCl 2 )1-x mol / L, wherein the value of x is a combination of one or more of 0, 1 / 6, 1 / 3, 1 / 2, 2 / 3, and a pH sustained-release agent with a concentration of 19-22% (a weak alkaline solution of ammonia water with a concentration of 15%), a glycerol dispersant with a concentration of 5%, and oxygen-free distilled water are added.
[0013] Preferably, the molecular formula of the zinc-iron ferrite magnetic nanoparticles is Zn x Fe 3-x O 4 , mainly composed of ferric chloride (FeCl 3 )2mol / L, ferric chloride (FeCl 2 )x mol / L, zinc dichloride (ZnCl 2)1-x mol / L, wherein the value of x is a combination of one or more of 0, 1 / 6, 1 / 3, 1 / 2, 2 / 3, and a pH sustained-release agent with a concentration of 19.5-21% (a weak alkaline solution of ammonia water with a concentration of 15%), a glycerol dispersant with a concentration of 5%, and oxygen-free distilled water are added.
[0014] Preferably, the molecular formula of the zinc-iron ferrite magnetic nanoparticles is Zn x Fe 3-x O 4 , mainly composed of ferric chloride (FeCl 3 )2mol / L, ferric chloride (FeCl 2 )x mol / L, zinc dichloride (ZnCl 2 )1-x mol / L, wherein the value of x is a combination of one or more of 0, 1 / 6, 1 / 3, 1 / 2, 2 / 3, and a pH sustained-release agent with a concentration of 20% (a weak alkaline solution of ammonia water with a concentration of 15%), a glycerol dispersant with a concentration of 5%, and oxygen-free distilled water are added.
[0015] The present invention also provides a method for preparing zinc-iron ferrite magnetic nanoparticles, which is used to prepare the zinc-iron ferrite magnetic nanoparticles as described above, comprising the following steps:
[0016] A. Prepare oxygen-free distilled water;
[0017] B. Add FeCl in a molar ratio of 2:x:1-x 3 、FeCl 2 、ZnCl 2 Add oxygen-free distilled water to prepare a coprecipitation solution. No other additives are added at this time. Heat in a water bath and stir rapidly.
[0018] C. Rapidly dropwise adding a pH sustained-release agent (15% weak alkaline ammonia solution) with a concentration of 19-22% to the coprecipitation solution can stabilize the pH value during the reaction at about 10;
[0019] D. After the reaction is completed, magnetic separation is performed using a NdFeB permanent magnet, and after multiple washings with distilled water, a 5% concentration of glycerol dispersant is added to make a magnetic fluid;
[0020] Under different pH ranges, the precipitation reaction ratios of zinc and iron are different, resulting in differences in the final ferrite components, which in turn result in differences in the magnetic properties of the ferrite components. Ferrites with high zinc content have weak magnetism and cannot be adsorbed and separated by permanent magnets, while ferrites with low zinc content have high magnetism and are easily adsorbed by permanent magnets. The present invention stabilizes the pH value of the coprecipitation solution to about 10, improves the uniformity of the reaction product components, and improves the qualified rate (yield rate) of the magnetic separation process.
[0021] E. Grind the magnetic fluid using planetary ball milling technology to destroy the existing agglomeration structure of zinc-iron ferrite magnetic nanoparticles and improve dispersibility and fluidity.
[0022] The invention adds a dispersant after the reaction and performs a planetary ball milling process. Compared with adding a dispersant during the reaction, the magnetic fluid obtained by the invention has better fluidity and dispersion effect and is less likely to agglomerate.
[0023] Furthermore, the water bath heating temperature in step A is 60-100°C.
[0024] Furthermore, the pH value of the coprecipitation solution after the pH sustained-release agent (15% weak alkaline ammonia solution) with a concentration of 20% is added dropwise in step C is about 10.
[0025] Furthermore, the grinding speed in step E is above 960 r / min.
[0026] Furthermore, the grinding time in step E is 2 to 3 hours.
[0027] Compared with the prior art, the present invention has the following beneficial effects:
[0028] The present invention can stabilize the pH value of the solution during the reaction at about 10 by adding a pH sustained-release agent during the reaction, thereby improving the uniformity of the reaction product components and improving the qualified rate (yield) of the magnetic separation process; glycerol is added as a dispersant after the reaction is completed, and planetary ball milling is performed. Compared with the existing method of adding a dispersant during the reaction, the dispersion effect is better, the fluidity of the obtained magnetic fluid is better, and it is not easy to agglomerate, which effectively solves the agglomeration problem of ferrite nanoparticles. DETAILED DESCRIPTION
[0029] The embodiments of the present invention will be described in detail below in conjunction with the examples, but it will be appreciated by those skilled in the art that the following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention. If specific conditions are not specified in the examples, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer is not specified for the reagents or instruments used, they are all conventional products that can be purchased commercially.
[0030] Example 1
[0031] preparing oxygen-free distilled water;
[0032] Add FeCl in a molar ratio of 2:x:1-x 3 、FeCl 2 、ZnCl 2Add oxygen-free distilled water to prepare a coprecipitation solution. Do not add other additives at this time. Heat the water bath to 60-100°C and stir rapidly.
[0033] Rapidly dropwise add a 20% pH sustained-release agent (15% weak alkaline ammonia solution) to the coprecipitation solution;
[0034] After the reaction is completed, the magnetic separation is carried out using a NdFeB permanent magnet, and after being washed with distilled water for multiple times, a 5% concentration of glycerol dispersant is added to make a magnetic fluid;
[0035] The magnetic fluid is ground by planetary ball milling technology at a grinding speed of more than 960 r / min for 2 to 3 hours to destroy the existing agglomeration structure of zinc-iron ferrite magnetic nanoparticles and improve the dispersibility and fluidity.
[0036] Example 2
[0037] preparing oxygen-free distilled water;
[0038] Add FeCl in a molar ratio of 2:x:1-x 3 、FeCl 2 、ZnCl 2 Add oxygen-free distilled water to prepare a coprecipitation solution. Do not add other additives at this time. Heat the water bath to 60-100°C and stir rapidly.
[0039] Rapidly dropwise add a 19% pH sustained-release agent (15% weak alkaline ammonia solution) to the coprecipitation solution;
[0040] After the reaction is completed, the magnetic separation is carried out using a NdFeB permanent magnet, and after being washed with distilled water for multiple times, a 5% concentration of glycerol dispersant is added to make a magnetic fluid;
[0041] The magnetic fluid is ground by planetary ball milling technology at a grinding speed of more than 960 r / min for 2 to 3 hours to destroy the existing agglomeration structure of zinc-iron ferrite magnetic nanoparticles and improve the dispersibility and fluidity.
[0042] Example 3
[0043] preparing oxygen-free distilled water;
[0044] Add FeCl in a molar ratio of 2:x:1-x 3 、FeCl 2 、ZnCl 2 Add oxygen-free distilled water to prepare a coprecipitation solution. Do not add other additives at this time. Heat the water bath to 60-100°C and stir rapidly.
[0045] Rapidly dropwise add a 22% pH sustained-release agent (15% weak alkaline ammonia solution) to the coprecipitation solution;
[0046] After the reaction is completed, the magnetic separation is carried out using a NdFeB permanent magnet, and after being washed with distilled water for multiple times, a 5% concentration of glycerol dispersant is added to make a magnetic fluid;
[0047] The magnetic fluid is ground by planetary ball milling technology at a grinding speed of more than 960 r / min for 2 to 3 hours to destroy the existing agglomeration structure of zinc-iron ferrite magnetic nanoparticles and improve the dispersibility and fluidity.
[0048] Example 4
[0049] The other conditions were the same as those in Example 1, except that a glycerol dispersant with a concentration of 4% was used.
[0050] Example 5
[0051] The other conditions are the same as those in Example 1, except that a weak alkaline ammonia solution with a concentration of 14% is used.
[0052] Comparative Example 1
[0053] Different from the process of Example 1, the process of adding 5% glycerol dispersant is placed before the reaction is completed.
[0054] Comparative Example 2
[0055] Different from the concentration of the pH sustained-release agent in the raw material in Example 1, a pH sustained-release agent with a concentration of 14% (a weak alkaline ammonia solution with a concentration of 15%) was added dropwise.
[0056] Comparative Example 3
[0057] Different from the process of step E in Example 1, the grinding rotation speed is 800 r / min.
[0058] Comparative Example 4
[0059] Different from the process of step E in Example 1, the grinding time is 1 hour.
[0060] Test Results
[0061] The test data is shown in Table 1 below:
[0062] Table 1
[0063]
[0064] It can be seen from the data in Table 1 that, with a reasonable raw material component ratio, the qualified rate of magnetic separation of the zinc-iron ferrite magnetic nanoparticles of the present invention is better than the qualified rate of magnetic separation of Comparative Examples 1 to 4. And the ratio adopted in Example 1 of the present invention produces the most excellent effect.
[0065] For the comparison results between Comparative Example 1 and Example 1, when the step of adding 5% glycerol dispersant is placed before the completion of the reaction, the weakened effect of the glycerol dispersant has a certain influence on the effect of magnetic separation, thereby reducing the qualified rate of magnetic separation.
[0066] For the comparison results between Comparative Example 2 and Example 1, when a pH sustained-release agent with a concentration of 14% (a weak alkaline ammonia solution with a concentration of 15%) is added dropwise, the concentration of the pH sustained-release agent decreases, affecting the effect of magnetic separation, thereby reducing the qualified rate of magnetic separation.
[0067] As for the comparison results between Comparative Example 3 and Example 1, when the grinding rotation speed is 800 r / min, the grinding rate is reduced, which affects the effect of magnetic separation and thus reduces the qualified rate of magnetic separation.
[0068] As for the comparison results between Comparative Example 4 and Example 1, when the grinding time is 1 hour, the grinding time is reduced, which affects the effect of magnetic separation and thus reduces the qualified rate of magnetic separation.
[0069] Comparing Example 1 with Example 2 and Example 3 in Table 1, it can be seen that the qualified rate of magnetic separation is the best when the 15% ammonia weak alkaline solution is added with an amount of pH sustained-release agent with an intermediate concentration within the range.
[0070] In summary, the zinc-iron ferrite magnetic nanoparticles prepared in the embodiment of the present invention can stabilize the pH value of the solution during the reaction at about 10 by adding a pH sustained-release agent during the reaction, thereby improving the uniformity of the reaction product components and the qualified rate (yield) of the magnetic separation process; glycerol is added as a dispersant after the reaction is completed, and planetary ball milling is performed. Compared with the existing method of adding a dispersant during the reaction, the dispersion effect is better, the fluidity of the obtained magnetic fluid is better, and it is not easy to agglomerate, which effectively solves the agglomeration problem of ferrite nanoparticles.
[0071] Although the present invention has been illustrated and described with specific embodiments, it will be appreciated that many other changes and modifications may be made without departing from the spirit and scope of the present invention. Therefore, it is intended to include all such changes and modifications within the scope of the present invention in the appended claims.
Claims
1. A zinc-iron ferrite magnetic nanoparticle, characterized in that: The molecular formula is Zn x Fe 3-x O4, mainly composed of 2 mol / L ferric chloride, x mol / L ferric chloride, 1-x mol / L zinc chloride in molar ratio, wherein the value of x is a combination of one or more of 0, 1 / 6, 1 / 3, 1 / 2, 2 / 3, 15% ammonia weak alkaline solution to which a pH sustained-release agent with a concentration of 19-22% is added, 5% glycerol dispersant, and oxygen-free distilled water; The method for preparing the zinc-iron ferrite magnetic nanoparticles comprises the following steps: A. Prepare oxygen-free distilled water; B. Add FeCl3, FeCl2 and ZnCl2 in a molar ratio of 2:x:1-x into oxygen-free distilled water to prepare a coprecipitation solution. No other additives are added at this time. Heat in a water bath and stir rapidly. C. Rapidly dropwise add a 15% weak alkaline ammonia solution to which a pH sustained-release agent having a concentration of 19-22% is added into the coprecipitation solution; D. After the reaction is completed, a permanent magnet is used for magnetic separation, and after multiple washings with distilled water, a 5% concentration of glycerol dispersant is added to make a magnetic fluid; E. Grind the magnetic fluid using planetary ball milling technology to destroy the existing agglomeration structure of zinc-iron ferrite magnetic nanoparticles and improve dispersibility and fluidity.
2. The zinc-iron ferrite magnetic nanoparticles according to claim 1, characterized in that: The molecular formula is Zn x Fe 3-x O4 is mainly composed of 2 mol / L ferric chloride, x mol / L ferric chloride and 1-x mol / L zinc chloride in molar ratio, wherein the value of x is a combination of one or more of 0, 1 / 6, 1 / 3, 1 / 2 and 2 / 3, and a 15% ammonia weak alkaline solution to which a pH sustained-release agent with a concentration of 19.5-21% is added, a 5% glycerol dispersant and oxygen-free distilled water.
3. The zinc-iron ferrite magnetic nanoparticles according to claim 1, characterized in that: The molecular formula is Zn x Fe 3-x O4 is mainly composed of 2 mol / L ferric chloride, x mol / L ferric chloride and 1-x mol / L zinc chloride in molar ratio, wherein the value of x is a combination of one or more of 0, 1 / 6, 1 / 3, 1 / 2 and 2 / 3, and a 15% ammonia weak alkaline solution to which a pH sustained-release agent with a concentration of 20% is added, a 5% glycerol dispersant and oxygen-free distilled water.
4. The method for preparing zinc-iron ferrite magnetic nanoparticles according to claim 1, characterized in that: The water bath heating temperature in step A is 60-100°C.
5. The method for preparing zinc-iron ferrite magnetic nanoparticles according to claim 1, characterized in that: The pH value of the coprecipitation solution after the weak alkaline solution of 15% ammonia water with 20% concentration of pH sustained-release agent added dropwise in step C is 10.
6. The method for preparing zinc-iron ferrite magnetic nanoparticles according to claim 1, characterized in that: The grinding speed in step E is above 960 r / min.
7. The method for preparing zinc-iron ferrite magnetic nanoparticles according to claim 1, characterized in that: The grinding time of step E is 2 to 3 h.