Laser additive composite manufacturing system and parts forming method for flammable and explosive materials
By designing a laser additive composite manufacturing system for flammable and explosive materials, combined with in-situ heating and stress relief processing, the problem of repairing complex curved aluminum and magnesium alloy parts has been solved, the problems of hot cracking and explosion have been avoided, and aluminum and magnesium alloys have been realized. Efficient and precise repair and improvement of mechanical properties of alloy parts.
Patent Information
- Application Number
- CN202410019297.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-05
- Publication Date
- 2024-10-15
- Estimated Expiration
- 2044-01-05
AI Technical Summary
Existing laser additive technology is difficult to effectively repair aluminum and magnesium alloy parts on complex curved surfaces, especially while ensuring mechanical properties, and is prone to thermal cracking and explosion problems.
A laser additive composite manufacturing system for flammable and explosive materials is designed, including a laser processing chamber, an air isolation device, a protective gas sensor, a highly sensitive hydrogen oxygen probe, a laser additive head and an industrial robot. It uses high-purity argon gas. Air washing and drying are combined with in-situ heating and stress relief treatment, and scanning paths are generated through 3D modeling software to achieve precise repair of aluminum and magnesium alloy parts.
It realizes the rapid forming of aluminum and magnesium alloy parts from scratch, avoids the problems of hot cracking and explosion, improves the processing flexibility and universality, can perform in-situ near net forming on complex special-shaped curved surfaces, and improves the quality of parts. mechanical properties.
Smart Images

Figure CN117983840B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the field of high-tech equipment development and additive manufacturing technology, and specifically to a laser additive composite manufacturing system for flammable and explosive materials and a part forming method. Background Art
[0002] Laser Engineered Net Shaping (LENS) is a type of laser 3D printing / additive manufacturing technology. It uses laser to generate a molten pool in the deposition area and continuously melt powder or filamentary materials to deposit layer by layer to generate parts with three-dimensional morphology and size. This technology was developed by Sandia National Laboratory in the United States in the 1990s, bringing rapid prototyping technology into a new stage. LENS technology can achieve moldless manufacturing for small and medium-sized parts, saving costs and shortening production cycles. It has great technical application value, especially for high-performance and high-cost parts manufacturing. At the same time, this technology solves a series of problems existing in traditional manufacturing processes for complex curved parts, such as difficult cutting, large material removal, and severe tool wear. In addition, compared with other powder bed 3D printing processes such as selective laser sintering / melting, LENS technology has unique advantages, including the ability to print functional gradient materials and smaller heat-affected zones. The most critical advantage is the ability to repair and remanufacture local areas of parts.
[0003] Taking advantage of the characteristics of LENS technology, there have been reports of several patents that use deposition methods such as laser additives to repair the surface of damaged parts. For example, "A Laser Additive Material and Laser Additive Repair Process for Train Rails" (CN112281082A) uses laser additives to repair Fe-based materials on the surface of train rails. While achieving good results, it also achieves the technical effects of restoring the size of the rails and improving surface performance. However, this patent mainly performs additive repairs on the surface of iron-based materials. As we all know, iron-based materials have good weldability and laser additives are relatively easy. It does not provide solutions to problems such as the many defects and obvious explosions that are prone to occur when adding low-melting-point and poorly weldable alloys such as aluminum and magnesium.
[0004] For example, "A laser selective melting repair method for special-shaped end covers and a special fixture for end covers" (CN115446443B) provides a special fixture and uses a laser additive manufacturing method to perform in-situ precise repairs on the surface of aluminum alloy parts, which can quickly obtain excellent parts repair effects. However, this patent is a customized treatment of aluminum alloys using powder-spreading laser selective melting technology, and does not provide a powder-feeding laser additive method for in-situ repair of aluminum and magnesium alloy parts. In particular, this method only repairs the planar position on the surface of low-melting-point, flammable and explosive, and poorly weldable magnesium and aluminum alloy parts, but it is still difficult to perform contour repairs on special-shaped curved surfaces.
[0005] In addition, the patent "A laser preparation method of porous magnesium alloy for biological organisms" (CN109513940A) mentions a method of using a prefabrication method to transport powder and then laser sintering. However, on the one hand, the magnesium alloy coating prepared by this method has a high porosity and is not suitable for actual parts repair. On the other hand, the pre-setting powder method used is not suitable for the field of local surface repair of complex parts. Moreover, the inventors found that materials such as aluminum and magnesium alloys (A novel hierarchical manufacturing method of the selective laser melted Al 7075alloy) are very likely to experience thermal cracking and other phenomena driven by thermal stress due to the excessive temperature gradient under extremely rapid melting conditions. At present, the main method has not proposed more solutions except for low-temperature preheating.
[0006] Therefore, as the requirements for repairing the surfaces of complex aluminum and magnesium alloy parts become higher and higher, how to achieve accurate repair of complex curved surfaces with oil circuits such as pumps, valves, and housings while ensuring their mechanical properties has become one of the problems that need to be solved at this stage. At the same time, how to simultaneously avoid or even eliminate the thermal cracking problem caused by extremely rapid melting caused by laser additive manufacturing is another problem that needs to be solved today. Summary of the invention
[0007] In order to solve the above technical problems, the present invention proposes a laser additive composite manufacturing system and a part forming method for flammable and explosive materials.
[0008] The technical problem to be solved by the present invention is achieved by adopting the following technical solutions:
[0009] A laser additive composite manufacturing system for flammable and explosive materials, including an external motor control system, a protective gas / powder storage bin / powder delivery system, an optical fiber, an industrial robot, and also includes:
[0010] The laser processing chamber is divided into an upper chamber and a lower chamber, the upper chamber is connected to the protective gas / powder storage bin / powder delivery system, a high-sensitivity hydrogen peroxide probe is arranged inside the upper chamber, a protective gas sensor connected to the high-sensitivity hydrogen peroxide probe is arranged outside the upper chamber, a protective chamber glass is arranged on the front side of the upper chamber, and two protective chamber gloves are arranged on the protective chamber glass;
[0011] a workpiece fixture, located in the upper cabin;
[0012] A heating coil is arranged in the upper cabin, and the heating range of the heating coil is between room temperature and 800° C.;
[0013] The laser additive head and the last joint of the industrial robot are located in the upper cabin and above the heating coil, and are connected to the external motor control system, the protective gas / powder storage bin / powder delivery system, the optical fiber, and the industrial robot. An air separator is provided between the laser additive head and the last joint of the industrial robot and the top of the upper cabin;
[0014] There are two filter elements, which are arranged in the lower compartment and communicated with the upper compartment;
[0015] The powder recovery bin is arranged in the lower cabin and communicated with the upper cabin.
[0016] Preferably, a porous plate is provided above the interior of the upper cabin, and a connection with the protective gas / powder storage bin / powder delivery system is opened on the rear cabin between the porous plate and the top of the upper cabin, and the diameter of the holes on the porous plate is 1mm-2mm, and the hole spacing is 5mm-20mm.
[0017] Preferably, mirror-grade reflective panels are provided on the left, right and rear sides of the interior of the upper cabin.
[0018] Preferably, two forming slides are provided on the left and right sides of the bottom of the upper chamber, and two rows of holes with a diameter of 1mm-2mm and a hole spacing of 5mm-10mm are provided on the two forming slides, and the holes are connected to the two filter elements accordingly.
[0019] Preferably, a heating coil mounting groove is provided in the middle of the bottom of the upper chamber, and the heating coil is arranged in the heating coil mounting groove. The diameter of the heating coil mounting groove is 20mm-30mm and the depth is 2mm-5mm. A through hole with a diameter of 5mm-10mm is provided in the middle of the heating coil mounting groove, and the through hole is connected to the powder recovery bin.
[0020] Preferably, two highly sensitive oxygen sensors are provided, with a detection accuracy of ±2ppm-5ppm, and can detect and find water oxygen content below 50ppm.
[0021] A method for forming parts by laser additive composite manufacturing of flammable and explosive materials, using the above-mentioned laser additive composite manufacturing system for flammable and explosive materials, comprises the following steps:
[0022] Step 1: Open the protective chamber glass, put the workpiece fixture, heating coil, parts to be repaired and installation tools into the upper chamber of the laser processing chamber in turn and close the protective chamber glass;
[0023] Step 2: Perform gas washing operation. After the water oxygen content in the upper cabin is reduced to less than 50ppm, use protective gloves to connect and clamp the heating coil, workpiece fixture and parts to be repaired in the upper cabin. After confirming that the installation is correct, prepare for laser additive repair;
[0024] Step 3: placing the powder to be processed with a purity of at least 99.0wt% and a particle size range of 90μm to 150μm into a vacuum drying oven at a drying temperature of 120°C to 200°C and a drying pressure of -0.08MPa to -0.1MPa for drying;
[0025] Step 4: Use 3D modeling software to create a 3D model based on the shape of the part to be repaired or the area to be repaired, and import the virtual model into the laser additive manufacturing system to generate programming code for the part scanning path;
[0026] Step 5: Pour the dried powder to be processed into the powder storage bin in the protective gas / powder storage bin / powder delivery system, and repeatedly purge it with argon gas with a purity of 99.999 vol%;
[0027] Step 6: Set the process parameters and form and manufacture the desired parts or remanufacture the parts that need to be repaired under the protection of argon gas;
[0028] Step 7: After each layer of material is added, in-situ heating is performed and extremely low temperature liquid argon is introduced through the protective gas / powder storage bin / powder delivery system to remove in-situ stress. The in-situ heating temperature ranges from 400℃ to 600℃.
[0029] Preferably, the powder to be processed in step three is aluminum alloy powder or magnesium alloy powder.
[0030] Preferably, if the powder to be processed is aluminum alloy powder, the process parameters in step six are: laser power is 2600W-3200W, preheating temperature is 120℃-220℃, scanning speed is 100mm / s-350mm / s, 3mm-5mm circular spot, and powder feeding speed is 6.5g / min-12g / min.
[0031] Preferably, if the powder to be processed is magnesium alloy powder, the process parameters in step six are: laser power is 800W-1250W, preheating temperature is 165℃-200℃, scanning speed is 150mm / s-350mm / s, 1.5mm-4mm circular spot, and powder feeding speed is 8g / min-12g / min.
[0032] The beneficial effects of the present invention are:
[0033] The present invention has a green powder recovery device, an explosion-proof filter element dust removal device and a coil induction heating device, which not only breaks the problems of flammability and explosion caused by traditional additive manufacturing in the atmospheric environment, and the difficulty of powder recovery, but also solves the problems of poor forming and easy cracking of aluminum and magnesium alloys during laser forming;
[0034] The present invention can not only realize the integrated rapid forming of aluminum, magnesium alloy and other materials from scratch, but also can perform in-situ near-net forming of surface defect areas of complex special-shaped surfaces. It has excellent processing flexibility and wide universality, and can be well promoted in powder feeding laser additive manufacturing systems.
[0035] The present invention can propose a solution for in-situ heat treatment and stress relief of the additive area without adding other devices, which can successfully avoid the phenomenon of additive failure caused by large-area cracking due to excessive tissue stress and thermal stress generated after additive manufacturing. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The present invention is further described below in conjunction with the accompanying drawings and embodiments:
[0037] Figure 1 It is a schematic diagram of the main structure of the present invention;
[0038] Figure 2 It is a schematic diagram of the three-dimensional structure of the laser processing chamber of the present invention;
[0039] Figure 3 It is a front structural schematic diagram of the laser processing chamber of the present invention;
[0040] Figure 4 This is the macroscopic surface morphology of the ZL101 aluminum alloy (AlSi7Mg) additive manufacturing sample after laser in-situ additive manufacturing + composite in-situ solution treatment;
[0041] Figure 5 The metallographic structure of the ZL101 aluminum alloy (AlSi7Mg) additive manufacturing sample after laser in-situ additive manufacturing + composite in-situ solution treatment;
[0042] Figure 6This is the macroscopic surface morphology of the AZ91D magnesium alloy additive manufacturing sample after laser in-situ additive manufacturing + composite in-situ solution treatment;
[0043] Figure 7 The metallographic structure of the AZ91D magnesium alloy additive manufacturing sample after laser in-situ additive manufacturing + composite in-situ solution treatment;
[0044] Figure 8 The coating morphology of the laser in-situ additively manufactured ZL101 aluminum alloy (AlSi7Mg) without in-situ solution treatment;
[0045] Fig. 9 This is a real picture of the surface cracks of the laser in-situ additively manufactured AZ91D magnesium alloy part without in-situ solution treatment.
[0046] In the figure: 1. Laser processing chamber; 2. Air isolation device; 3. Protective gas sensor; 4. High-sensitivity hydrogen sensor; 5. Laser additive head and the last joint of the industrial robot; 6. Protective chamber gloves; 7. Protective chamber glass; 8. Workpiece fixture; 9. Heating coil; 10. Filter element; 11. Powder recovery chamber; 12. Porous plate; 13. Mirror-grade reflector; 14. Forming slide; 15. Heating coil installation slot. DETAILED DESCRIPTION
[0047] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further described below with reference to the accompanying drawings and embodiments.
[0048] like Figures 1 to 3 As shown, a laser additive composite manufacturing system for flammable and explosive materials includes a laser processing chamber 1, a gas isolation device 2, a protective gas sensor 3, a high-sensitivity hydrogen sensor 4, a laser additive head and the last joint of an industrial robot 5, two protective bin gloves 6, a protective bin glass 7, a workpiece fixture 8, a heating coil 9, two filter elements 10, a powder recovery bin 11, an external motor control system, a protective gas / powder storage bin / powder delivery system, an optical fiber, and an industrial robot.
[0049] The laser processing chamber 1 includes an upper chamber and a lower chamber. A porous plate 12 is arranged on the upper part of the upper chamber, and mirror-grade reflective plates 13 are arranged on the left, right and rear sides of the interior. Two forming slides 14 are arranged on the left and right sides of the bottom of the upper chamber, and the two forming slides 14 are correspondingly connected to the two filter elements 10. A heating coil installation groove 15 is arranged in the middle of the bottom of the upper chamber, and the heating coil 9 is correspondingly installed in the heating coil installation groove 15.
[0050] An air hole is provided on the rear side chamber of the upper chamber and between the porous plate 12 and the top of the upper chamber, through which the upper chamber is connected to the protective gas / powder storage bin / powder delivery system.
[0051] The diameter of the holes on the porous plate 12 is 1mm-2mm, and the hole spacing is 5mm-20mm, so that after the high-density argon gas is introduced from the back of the upper chamber, the argon gas can be evenly introduced from the upper part of the porous plate and fill the entire upper chamber, the filter element 10 and the powder recovery bin 11, so as to ensure that all powder storage areas are filled with argon gas to avoid combustion and explosion.
[0052] In this embodiment, specifically, the diameter of the holes on the porous plate 12 is 1.5 mm, and the hole spacing is 10 mm.
[0053] The mirror-grade reflector 13 is a 316L stainless steel plate with a zinc film coated on its surface after electrochemical polishing, so as to ensure that the operator can see all the items in the upper cabin through the mirror-grade reflector 13 at the rear and both sides without opening the cabin during use, thereby facilitating practical operation.
[0054] Two rows of holes with a diameter of 1mm-2mm and a hole spacing of 5mm-10mm are provided on the two forming carriages 14. The two rows of holes are axially symmetrical. The holes are distributed in a rectangular gap 1.5mm away from the plane of the forming carriage 14. The holes are directly connected to the filter element 10 to ensure that the repaired powder, residue, etc. can fall into them; in addition, the concave part can also facilitate the placement of tools such as screwdrivers, brushes, air bags, etc. used for cleaning the workbench and slag powder on its surface to prevent the tools from being missed due to multiple operations.
[0055] In this embodiment, specifically, the diameter of the holes on the forming carriage 14 is 1.5 mm, and the hole spacing is 8 mm.
[0056] The diameter of the heating coil installation groove 15 is 20mm-30mm and the depth is 2mm-5mm. A through hole with a diameter of 5mm-10mm is set in the middle of the heating coil installation groove 15. The through hole is connected to the powder recovery bin 11, so that when the heating coil 9 is placed, it is also convenient to collect and recover the excess powder through the through hole to achieve the purpose of graded recovery and recycling.
[0057] In this embodiment, specifically, the diameter of the heating coil installation groove 15 is 25 mm and the depth is 2.5 mm; the diameter of the through hole is 8 mm.
[0058] The air isolation device 2 is arranged between the laser additive head and the last joint 5 of the industrial robot and the upper cabin, and is used to isolate the laser additive head and the last joint 5 of the industrial robot from the outside world. To ensure that the laser additive head has enough space for movement in the upper cabin, the air isolation device 2 is a detachable and variable-size device to ensure that the last joint of the industrial robot can partially or completely enter the upper cabin according to needs. Furthermore, the upper port diameter of the air isolation device 2 is equal to the diameter of the last joint of the industrial robot. It is protected by tin foil during processing and sealed with a sealed bag to prevent leakage of protective gas.
[0059] In this embodiment, the air barrier 2 is made of high temperature resistant rubber tightly connected to the laser processing chamber 1. It has extremely high softness, high temperature resistance and sealing properties, and can completely seal the laser additive head and the last joint 5 of the industrial robot in the laser processing chamber 1. The air barrier 2 can not only ensure that there is no air leakage during the air washing process, but also ensure that there is no leakage and other problems due to the shaking of the additive head during the laser additive process. Furthermore, the air barrier 2 is connected to the laser processing chamber 1 by gluing. After the air barrier 2 wraps the laser additive head and the last joint 5 of the industrial robot, it is sealed and connected by hot melt adhesive.
[0060] The protective gas sensor 3 is arranged outside the upper cabin, and the high-sensitivity hydrogen peroxide probe 4 is arranged inside the upper cabin. The protective gas sensor 3 mainly reflects the content of water, oxygen and argon. To ensure accurate detection, two high-sensitivity hydrogen peroxide probes 4 are generally required to be installed, and the detection accuracy of the high-sensitivity hydrogen peroxide probe 4 is ±2-5ppm, which can detect and find the water oxygen content within 50ppm.
[0061] In this embodiment, specifically, the detection accuracy of the high-sensitivity oxygen sensor 4 is ±3ppm.
[0062] The laser additive head and the last joint 5 of the industrial robot are located above the upper chamber and extend into the upper chamber through the porous plate 12. The laser additive head and the last joint 5 of the industrial robot can not only select the length of the extension into the upper chamber according to the shape and size of the required processed parts, but also, in order to avoid the need to remove the processed aluminum and magnesium alloy parts and then perform stress relief or solution annealing, the processed area is introduced with extremely low temperature liquid argon after laser surface heat treatment to achieve the effect of in-situ annealing.
[0063] In the present embodiment, two protective bin gloves 6 are provided, which are fixed to the protective bin glass 7 by gluing and screwing. The two protective bin gloves 6 are made of materials such as polyurethane (PU), fluororubber (FKM), polyphenylene sulfide (PPS) that can withstand high temperatures above 200 degrees. They not only have good flexibility but also have excellent sealing performance, which can ensure that there will be no air leakage, powder leakage and the like due to excessive temperature during actual operation, and can also facilitate the operator to put his hand into the rubber gloves to operate in the cabin.
[0064] In this embodiment, the protective chamber glass 7 is a heat-resistant laser-specific protective glass with filtering effect, so as to ensure that injuries and burns to the eyes, limbs, etc. of personnel caused by laser radiation are avoided during use.
[0065] In this embodiment, the protective chamber glass 7 is polymethyl methacrylate laser protective glass, which can filter out infrared light waves of 1064nm-1070nm.
[0066] The heating coil 9 is installed in the heating coil installation groove 15. The heating temperature range of the heating coil 9 can be heated from room temperature to 800°C, and can be maintained for a long time to avoid problems such as failure to add material and cracking of aluminum and magnesium alloys due to long melting range and poor deformability at room temperature during addition.
[0067] In this embodiment, the two filter elements 10 are permanent filter elements and contain quicklime, kerosene and other flame retardants to prevent dust from flying and causing explosion problems.
[0068] A method for forming parts by laser additive composite manufacturing of flammable and explosive materials, using the above-mentioned laser additive composite manufacturing system for flammable and explosive materials, comprises the following steps:
[0069] Step 1: Open the protective chamber glass 7, put the workpiece fixture 8, the heating coil 9, the part to be repaired and the installation tool into the upper chamber of the laser processing chamber 1 in sequence and close the protective chamber glass 7.
[0070] Step 2: Perform gas washing operation. After the water oxygen content in the upper cabin is reduced to less than 50ppm, use the protective warehouse gloves 6 to connect and clamp the heating coil 9, workpiece fixture 8 and the parts to be repaired in the upper cabin. After confirming that the installation is correct, prepare for laser additive repair.
[0071] Step 3: Place the powder to be processed with a purity of at least 99.0wt% and a particle size range of 90μm to 150μm into a vacuum drying oven with a drying temperature of 120°C to 200°C and a drying pressure of -0.08MPa to -0.1MPa for drying.
[0072] Step 4: Use 3D modeling software to create a 3D model based on the shape of the part to be repaired or the area to be repaired, and import the virtual model into the laser additive manufacturing system to generate programming code for the part scanning path.
[0073] In this embodiment, specifically, the three-dimensional modeling software is dedicated modeling software such as UG, Solidworks, and CATIA.
[0074] Step 5: Pour the dried powder to be processed into the powder storage bin in the protective gas / powder storage bin / powder delivery system, and repeatedly purge it with argon gas with a purity of 99.999 vol%.
[0075] Step 6: Set the process parameters and form and manufacture the desired parts or remanufacture the parts that need to be repaired under the protection of argon gas.
[0076] Step 7: After each layer of material is added, in-situ heating is performed and extremely low temperature liquid argon is introduced through the protective gas / powder storage bin / powder delivery system to remove in-situ stress. The in-situ heating temperature ranges from 400℃ to 600℃.
[0077] Furthermore, the powder to be processed in step three is aluminum or magnesium alloy powder with low boiling point and flammability. Since the process parameters of aluminum alloy powder and magnesium alloy powder are different, the following two embodiments are listed.
[0078] Embodiment 1
[0079] The powder to be processed is aluminum alloy powder. Specifically, additive manufacturing of the same material is performed on the surface of a complex part made of ZL101 aluminum alloy (AlSi7Mg).
[0080] Process parameters in step six: laser power is 2600W-3200W, preheating temperature is 120℃-220℃, scanning speed is 100mm / s-350mm / s, 3mm-5mm circular spot, powder feeding speed is 6.5g / min-12g / min.
[0081] In this embodiment, the laser power is 2800W, the preheating temperature is 180°C, the scanning speed is 200mm / s, the circular spot is 4mm, the powder feeding speed is 8g / min, and the water oxygen content is measured and controlled at 26±2ppm.
[0082] In step 7, the laser power is 780W for the additive area, the scanning speed is unchanged, the preheating temperature is raised to 520℃, and liquid argon cooling is performed for local solution treatment. Figure 4 and Figure 5 As shown, the laser additive layer after processing has good surface quality and only a small number of holes in the cross section, indicating that the processing method of laser in-situ additive composite heat treatment proposed in this patent has good application prospects.
[0083] Embodiment 2
[0084] The powder to be processed is a magnesium alloy powder. Specifically, the AZ91D magnesium alloy additive manufacturing is performed on the surface of an AZ91D magnesium alloy substrate.
[0085] Process parameters in step six: laser power is 800W-1250W, preheating temperature is 165℃-200℃, scanning speed is 150mm / s-350mm / s, 1.5mm-4mm circular spot, powder feeding speed is 8g / min-12g / min.
[0086] In this embodiment, the laser power is 1100 W, the preheating temperature is 185° C., the scanning speed is 300 mm / s, the circular spot is 2 mm, the powder feeding speed is 10 g / min, and the water oxygen content is measured and controlled at 27±3 ppm.
[0087] In step 7, the laser power is 560W for the additive area, the scanning speed is unchanged, the preheating temperature is raised to 420℃, and liquid argon cooling is performed for local solution treatment. Figure 6 and Figure 7 As shown in the figure, the processed AZ91D magnesium alloy laser additive layer has a good macroscopic morphology, and no obvious holes are seen after the surface is polished with sandpaper; and the structure after further surface polishing and corrosion is found that the structure inside the additive layer is mainly composed of fine equiaxed crystals, showing good anisotropy.
[0088] In order to further compare the hardness of the material prepared by this method with that of traditional materials, Table 1 statistically shows the hardness of the samples prepared by the process used in Examples 1-2 and the hardness of the corresponding casting alloys. It can be seen that the hardness of the alloy samples manufactured by this system and this method far exceeds the standard or reported value in the literature, and has good application prospects.
[0089] Table 1. Comparison of hardness measured in the examples and standard hardness
[0090]
[0091] In addition, a comparative example 1 and a comparative example 2 are made to compare the embodiment 1 and the embodiment 2.
[0092] Comparative Example 1
[0093] The parameters used are completely consistent with the aluminum alloy materials and parameters used in Example 1. The only difference is that the laser material addition is performed in the atmospheric environment without preheating and the laser in-situ heat treatment is not used. At this time, the water and oxygen content in the atmospheric environment is extremely high; Figure 8As shown, it is shown that there are a large number of holes inside the ZL101 aluminum alloy layer that is additively manufactured on the surface of the ZL101 aluminum alloy substrate, resulting in poor final mechanical properties, indicating that it is inappropriate to use only ordinary laser for laser additive manufacturing.
[0094] Comparative Example 2
[0095] The parameters used are completely consistent with the magnesium alloy materials and parameters used in Example 2. The only difference is that the laser material addition is performed in the atmosphere without preheating and the laser in-situ heat treatment is not used. At this time, the water and oxygen content in the atmosphere is extremely high. Fig. 9 As shown, the in-situ repair of AZ91D magnesium alloy parts without the system and corresponding method provided by the present invention is shown. It can be seen that due to the lack of synchronous preheating and in-situ heat treatment, deep cracks are left on the surface after rapid solidification due to the existence of great internal stress; and when adding magnesium alloy, since it is done in an open environment, the scattered magnesium alloy powder is very easy to ignite the surrounding flammable and explosive items, causing fires, and ultimately leading to casualties and property losses. Therefore, it is an extremely inappropriate method to use only ordinary lasers for laser addition of magnesium alloys.
[0096] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments. The above embodiments and descriptions only describe the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, which fall within the scope of the present invention. The scope of protection of the present invention is defined by the attached claims and their equivalents.
Claims
1. A laser additive composite manufacturing system for flammable and explosive materials, comprising an external motor control system, a protective gas / powder storage bin / powder delivery system, an optical fiber, and an industrial robot, characterized in that: Also includes: A laser processing chamber (1) is divided into an upper chamber and a lower chamber, the upper chamber is connected to the protective gas / powder storage bin / powder delivery system, a high-sensitivity hydrogen peroxide probe (4) is arranged inside the upper chamber, a protective gas sensor (3) connected to the high-sensitivity hydrogen peroxide probe (4) is arranged outside the upper chamber, a protective chamber glass (7) is arranged at the front side of the upper chamber, and two protective chamber gloves (6) are arranged on the protective chamber glass (7); A workpiece fixture (8), located in the upper cabin; A heating coil (9) is arranged in the upper chamber, and the heating range of the heating coil (9) is between room temperature and 800° C.; The laser material-additive head and the last joint (5) of the industrial robot are located in the upper cabin and above the heating coil (9), and are connected to the external motor control system, the protective gas / powder storage bin / powder delivery system, the optical fiber, and the industrial robot. An air barrier (2) is provided between the laser material-additive head and the last joint (5) of the industrial robot and the top of the upper cabin; Two filter elements (10) are provided, and the two filter elements (10) are arranged in the lower compartment and communicated with the upper compartment; The powder recovery bin (11) is arranged in the lower chamber and communicated with the upper chamber.
2. A laser additive composite manufacturing system for flammable and explosive materials according to claim 1, characterized in that: A porous plate (12) is arranged above the interior of the upper cabin, and a connection with the protective gas / powder storage bin / powder delivery system is opened on the rear cabin between the porous plate (12) and the top of the upper cabin. The diameter of the holes on the porous plate (12) is 1mm-2mm, and the hole spacing is 5mm-20mm.
3. The laser additive composite manufacturing system for flammable and explosive materials according to claim 1, characterized in that: Mirror-grade reflective plates (13) are arranged on the left side, right side and rear side of the interior of the upper cabin.
4. The laser additive composite manufacturing system for flammable and explosive materials according to claim 1, characterized in that: Two forming carriages (14) are arranged on the left and right sides of the bottom of the upper chamber, and the two forming carriages (14) are each provided with two rows of holes with a diameter of 1 mm-2 mm and a hole spacing of 5 mm-10 mm, and the holes are correspondingly connected to the two filter elements (10).
5. The laser additive composite manufacturing system for flammable and explosive materials according to claim 1, characterized in that: A heating coil mounting groove (15) is provided in the middle of the bottom of the upper chamber, and the heating coil (9) is arranged in the heating coil mounting groove (15). The diameter of the heating coil mounting groove (15) is 20mm-30mm and the depth is 2mm-5mm. A through hole with a diameter of 5mm-10mm is provided in the middle of the heating coil mounting groove (15), and the through hole is connected to the powder recovery bin (11).
6. The laser additive composite manufacturing system for flammable and explosive materials according to claim 1, characterized in that: The highly sensitive oxygen probes (4) are provided with two, and the detection accuracy is ±2ppm-5ppm, and can detect and find the water oxygen content below 50ppm.
7. A method for forming parts by laser additive manufacturing of flammable and explosive materials, characterized in that: A laser additive composite manufacturing system for flammable and explosive materials according to any one of claims 1 to 6 comprises the following steps: Step 1: Open the protective chamber glass (7), place the workpiece fixture (8), the heating coil (9), the part to be repaired and the installation tool into the upper chamber of the laser processing chamber (1) in sequence and close the protective chamber glass (7); Step 2: Perform gas washing operation. After the water oxygen content in the upper chamber is reduced to less than 50 ppm, use the protective chamber gloves (6) to connect and clamp the heating coil (9), the workpiece fixture (8) and the parts to be repaired in the upper chamber. After confirming that the installation is correct, prepare for laser additive repair; Step 3: placing the powder to be processed with a purity of at least 99.0wt% and a particle size range of 90μm to 150μm into a vacuum drying oven at a drying temperature of 120°C to 200°C and a drying pressure of -0.08MPa to -0.1MPa for drying; Step 4: Use 3D modeling software to create a 3D model based on the shape of the part to be repaired or the area to be repaired, and import the virtual model into the laser additive manufacturing system to generate programming code for the part scanning path; Step 5: Pour the dried powder to be processed into the powder storage bin in the protective gas / powder storage bin / powder delivery system, and repeatedly purge it with argon gas with a purity of 99.999 vol%; Step 6: Set the process parameters and form and manufacture the desired parts or remanufacture the parts that need to be repaired under the protection of argon gas; Step 7: After each layer of material is added, in-situ heating is performed and extremely low temperature liquid argon is introduced through the protective gas / powder storage bin / powder delivery system to remove in-situ stress. The in-situ heating temperature ranges from 400℃ to 600℃.
8. The method for forming parts by laser additive manufacturing of flammable and explosive materials according to claim 7, characterized in that: In step 3, the powder to be processed is aluminum alloy powder or magnesium alloy powder.
9. The method for forming parts by laser additive manufacturing of flammable and explosive materials according to claim 8, characterized in that: If the powder to be processed is aluminum alloy powder, the process parameters in step six are: laser power is 2600W-3200W, preheating temperature is 120℃-220℃, scanning speed is 100mm / s-350mm / s, 3mm-5mm circular spot, and powder feeding speed is 6.5g / min-12g / min.
10. The method for forming parts by laser additive manufacturing of flammable and explosive materials according to claim 8, characterized in that: If the powder to be processed is magnesium alloy powder, the process parameters in step six are: laser power is 800W-1250W, preheating temperature is 165℃-200℃, scanning speed is 150mm / s-350mm / s, 1.5mm-4mm circular spot, and powder feeding speed is 8g / min-12g / min.