A high reflective material for colored pavement and its preparation
By using hydrophobic titanium dioxide coated hollow glass microbeads and modified shell powder in the reflective material, combining polydimethylsiloxane and SiO2 nanoparticles to form a highly reflective coating, the easy damage and environment of the reflective material are solved. The pollution problem has improved weather resistance and service life, and is simple and easy to implement.
Patent Information
- Application Number
- CN202410271357.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-11
- Publication Date
- 2024-11-05
- Estimated Expiration
- 2044-03-11
AI Technical Summary
Existing reflective materials are prone to wear, damage, and corrosion in the environment, resulting in poor reflective effects. The added commercial colorants affect the washing color fastness and weather resistance, and the preparation process may pollute the environment, resulting in a short service life and replacement. complex.
A colored pavement adhesive tape consisting of a highly reflective coating, substrate and adhesive layer was designed, and the hydrophobic titanium dioxide coated hollow glass microbeads and modified shell powder were used to combine polydimethylsiloxane. and SiO2 nanoparticles form a highly reflective coating, with good bonding and easy replacement and repair properties.
The weather resistance, durability and service life of reflective materials are improved, damage to the road surface is avoided, the construction method is simple, the construction period is reduced, and environmental pollution is reduced through the use of modified materials.
Smart Images

Figure CN117987022B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of road surface reflective materials, in particular to a high-reflective material for colored road surfaces and a preparation method thereof. Background Art
[0002] Reflective material is a material that can reflect incident light back to the incident medium, also known as retro-reflective material or retro-reflective material. The reason why reflective material can reflect light is mainly because its surface contains a high refractive index prism micro-lattice or glass micro-beads. When a beam of light hits the surface of the material at any angle within a certain range, most of the optical fiber will be concentrated by the glass micro-beads in a very small angle range and reflected back to the light source, forming a retro-reflection phenomenon, making its brightness much higher than other ordinary objects. At present, reflective materials are widely used in signs in the fields of transportation, fire protection, transportation, etc., and are also commonly used as decorative materials for clothing, buildings, etc., and are very common in road surfaces. At present, with the development of urban construction, colored pavements can not only play a beautification and decoration role in urban planning, but also have the effect of clearly indicating crosswalks, accident-prone areas, emergency parking strips, lanes, shoulders, etc. In order to make the markers on the colored pavement not need additional energy to provide electricity to make them glow when the light is weak at night, greatly reducing the dependence on electricity, or improving the decorativeness and aesthetics of the colored pavement according to the design plan, the use of reflective materials can achieve the purpose.
[0003] Since reflective materials are often exposed to the environment, they are very susceptible to wear, damage, corrosion, etc., and fall off, resulting in poor reflective effect. Therefore, strong reflective coefficient, wear resistance, and water washability are important performance indicators of reflective material products. In order to improve the ornamental and functional properties, commercial colorants are often introduced into reflective materials. However, the use of colorants seriously hinders the interaction between the reflective original and the underlying coating, resulting in low color fastness to washing and poor weathering resistance. Not only are reflective materials easily damaged as the exposure time and environment change, but the added colorants will also lose strength and discolor and fade over time; in the preparation process of reflective materials, the added fine inorganic particles are also easy to pollute the surrounding environment, which is not in line with the concept of environmental protection. The poor weather resistance and short service life of reflective materials require frequent replacement and repair during long-term use. If the reflective coating is directly applied on the colored road surface, the replacement is more complicated and the engineering workload is large. Summary of the invention
[0004] In order to solve the above technical problems, the present invention has designed a high-reflective material for colored pavement and its preparation. The material consists of a high-reflective coating, a substrate and an adhesive layer. It is an adhesive tape with high reflective effect that can be used for colored pavement. It has good adhesion to the pavement, not only provides a high-reflective effect, but also can design different markings, patterns and decorations in advance according to the pavement construction and usage conditions and then install them on the pavement. The high-reflective coating is a hydrophobic coating, and the modified hollow glass microbeads used in the preparation are hollow glass microbeads coated with hydrophobicized titanium dioxide. The modified shell powder utilizes natural shells and is an environmentally friendly material. The high-reflective material for colored pavement prepared by the present invention is easy to replace and repair, will not affect the pavement itself, and the construction method is simple and easy.
[0005] In order to achieve the above goals, the following technical solutions are adopted:
[0006] A high reflective material for colored pavement is composed of the following three parts: a high reflective coating, a substrate and an adhesive layer;
[0007] The high-reflective coating is composed of the following components in parts by weight: 20-40 parts of polydimethylsiloxane, 60-80 parts of environmentally friendly solvent oil, 20-40 parts of modified hollow glass microspheres, 4-10 parts of modified shell powder, 0.1-2 parts of SiO2 nanoparticles, 0.5-2 parts of ultraviolet absorbers, 2-4 parts of antioxidants, 0.25-0.5 parts of curing agents, 2-6 parts of fluorescent powders, and 0-5 parts of pigments; the substrate is a sheet material made of composite rubber with uniform thickness, and the thickness is 0.5-1 mm; the adhesive layer is an epoxy resin adhesive;
[0008] The modified hollow glass microspheres are prepared from the following raw materials: 30-70 g of hollow glass microspheres, 20-60 ml of tetrabutyl titanate, 80-180 ml of anhydrous ethanol, 2-4 ml of acetic acid, 20-40 ml of ethanol, 500 mL of toluene, and 2-5 g of 1H,1H,2H,2H-perfluorooctyltriethyloxysilane;
[0009] Among them, the diameter of the hollow glass microspheres is 90~150μm, the wall thickness is 1~2μm, tetrabutyl titanate, acetic acid, ethanol, anhydrous ethanol, and toluene are all analytical reagents, the purity of tetrabutyl titanate and 1H,1H,2H,2H-perfluorooctyltriethyloxysilane is 98%, and the purity of toluene and acetic acid is 99.5%;
[0010] The modified shell powder is prepared from the following raw materials: 30-50g natural shell, 6-12g silane coupling agent, 0.3-0.6g dispersant, wherein the silane coupling agent is KH-550, and the dispersant is an aqueous sodium acrylate dispersant;
[0011] Among them, the curing agent is one of ethylenediamine, diethylenetriamine, acrylic anhydride, and methyl ethyl ketone, the ultraviolet absorber is one of phenyl salicylate, ultraviolet absorber UV-P, ultraviolet absorber UV-O, ultraviolet absorber UV531, and ultraviolet absorber RMB, the antioxidant is one of 2,6-di-tert-butyl-p-cresol, dibutyl disulfide, and dipropyl dihydroxybenzophenone, the pigment is one of iron chrome black, nickel titanate yellow, cobalt green, cobalt blue, iron oxide red, and ordinary color paste or no pigment is added, and the phosphor is a rare earth metal-doped aluminate fluorescent material.
[0012] Furthermore, the preparation of the modified hollow glass microspheres comprises the following steps:
[0013] S1, respectively measuring sulfuric acid and hydrogen peroxide at a volume ratio of 3:1, immersing the hollow glass microspheres in sulfuric acid, then adding hydrogen peroxide, storing them in a fume hood at room temperature for 4 hours, then taking them out, rinsing them with distilled water 2 to 3 times and drying them at room temperature for 12 hours, to obtain hollow glass microspheres after surface hydrophilic treatment;
[0014] S2, respectively measuring tetrabutyl titanate and anhydrous ethanol, and dropping the tetrabutyl titanate into the anhydrous ethanol under vigorous stirring, wherein the stirring speed of the vigorous stirring is 800-1200 rpm and the stirring time is 5-15 min, to obtain a transparent solution A;
[0015] S3, measuring 5-8 mL of distilled water and ethanol, slowly adding acetic acid under vigorous stirring, adjusting the pH to 2-3, the stirring speed of the vigorous stirring is 500-800 rpm, and the stirring time is 10-20 min, to obtain solution B;
[0016] S4, adding the hollow glass microspheres after the surface hydrophilic treatment obtained in S1 to the transparent solution A obtained in S2, stirring to disperse the hollow glass microspheres after the surface hydrophilic treatment in the transparent solution A, the stirring speed is 400-600 rpm, the stirring time is 10-20 min, and a solution C is obtained;
[0017] S5, slowly adding the solution B obtained in S3 to the solution C at a rate of 1-2 drops / second under vigorous stirring, wherein the vigorous stirring speed is 4000-5000 rpm, and the stirring time is 30-60 min, and a wet gel is obtained after the reaction is completed;
[0018] S6, drying the wet gel obtained in step S5 in an oven at 80° C. for 1 h, grinding until there is no agglomeration and the particle size is uniform, and calcining in a muffle furnace at 500-700° C. for 2 h to obtain titanium dioxide-coated hollow glass microspheres;
[0019] S7, take toluene and 1H,1H,2H,2H-perfluorooctyltriethyloxysilane and mix them evenly, add the titanium dioxide-coated hollow glass microspheres obtained in step S6 to the mixture of toluene and 1H,1H,2H,2H-perfluorooctyltriethyloxysilane, and store them in a fume hood at room temperature for 48 to 72 hours. After the reaction is completed, wash and filter with toluene and store them at room temperature in a fume hood for 2 days until the toluene evaporates, then transfer them to an oven and dry them at 70°C for 1 to 4 hours to obtain titanium dioxide-coated hollow glass microspheres after hydrophobic treatment, which are the modified hollow glass microspheres.
[0020] Furthermore, the preparation of modified shell powder comprises the following steps:
[0021] Q1, soak natural shells in 0.05M hydrochloric acid solution for 10-14h, then soak in 0.2M sodium hydroxide solution for 10-14h, rinse with deionized water and dry in a 100℃ oven for 10-20min to obtain natural shells with impurities removed;
[0022] Q2, the natural shells obtained in step Q1 and freed of impurities are treated in a muffle furnace at 700-900° C. for 6-10 hours, and then transferred to a grinder for ball milling at a speed of 30 rpm for 7-9 hours to obtain shell powder;
[0023] Q3, weigh 20~40g shell powder and 6~12g silane coupling agent, add into 80mL deionized water, heat to 85~95℃ in a water bath, stir at 100~150rpm, slowly add dispersant during heating, wait until the solution turns pure white, cool to room temperature, filter out insoluble matter, and dry in oven at 60℃ for 20min to obtain modified shell powder.
[0024] Furthermore, a preparation method of a highly reflective material for a colored road surface comprises the following steps:
[0025] P1, weigh polydimethylsiloxane and environmentally friendly solvent oil, mix them in a container, and stir them magnetically at 100-200 rpm for 30-90 min to obtain a mixture 1;
[0026] P2, maintaining stirring, according to the formula ratio, add the modified hollow glass microspheres, modified shell powder, SiO2 nanoparticles, fluorescent powder and pigment to the mixture 1 obtained in step P1 in sequence, and stir at 100-200 rpm for 30-60 min until uniformly dispersed, to obtain mixture 2;
[0027] P3, mixing the ultraviolet absorber, antioxidant and curing agent in a container, stirring at a stirring speed of 60-150 rpm for 10-30 min until uniformly dispersed, to obtain a mixture 3, adding the mixture 3 to the mixture 2 obtained in step P2, stirring at 100-200 rpm for 1-2 h, applying the mixture to the surface of the substrate by spraying, brushing, rolling or dipping, curing and drying the coating to obtain a highly reflective coating;
[0028] P4, cutting the high-reflective coating obtained in step P3 into the required size and shape, coating the bottom or side of the substrate with epoxy resin adhesive to form an adhesive layer, and tightly combining the high-reflective coating, the substrate and the adhesive layer through a hot pressing process, wherein the hot pressing temperature is 80-120°C and the hot pressing time is 2-5 minutes. After cooling to room temperature, the high-reflective material for colored pavement is obtained.
[0029] Furthermore, the curing in step P3 refers to curing at room temperature for 24 hours, and drying is performed at 80° C. for 1 hour.
[0030] Furthermore, the highly reflective material for colored pavement is designed into different markings, patterns or decorations as needed during the construction process. The thickness of the highly reflective material for colored pavement is 1-3 mm. The pavement must be preheated before use and rolled after installation to make it fit the pavement.
[0031] The beneficial effects achieved by the present invention are as follows:
[0032] The present invention designs a highly reflective material for colored pavement, which is a pavement adhesive tape composed of three parts: a highly reflective coating, a substrate and an adhesive layer. Preparing the reflective material into an adhesive tape can avoid damage to the pavement during repair and replacement during use, and the construction method is simple and easy. Different marking lines, patterns and decorations can be directly prepared according to construction requirements and usage conditions and then installed, saving construction time. For the high-reflective coating designed in the present invention, modified hollow glass microspheres are used as optical elements to achieve parallel reflection of incident light to achieve the reflective effect. Compared with the direct use of unmodified glass microspheres, the titanium dioxide introduced by the hydrophobically treated titanium dioxide-coated modified hollow glass microspheres used in the present invention has a higher reflectivity in both the visible light region and the infrared light region, and is a good reflection enhancing filler that can enhance the light reflecting ability of the hollow glass microspheres. In addition, titanium dioxide also has photocatalytic properties, which improves the self-cleaning performance of the highly reflective material; polydimethylsiloxane is used as a film-forming material, and the combination with SiO2 nanoparticles is beneficial to improving the hydrophobicity of the coating. The addition of titanium dioxide and SiO2 nanoparticles can also improve the The strength of the alkane itself; polydimethylsiloxane has a Si-O-Si main chain structure and an organic side chain, so it has both the heat resistance of inorganic polymers and the flexibility of organic polymers, and has good weather resistance. The ultraviolet absorption ability of titanium dioxide itself further alleviates aging and enhances its weather resistance and service life; the shell powder modified by silane coupling agent has a regular shape, a compact structure, a uniform particle size distribution, and effectively alleviates the agglomeration of shell powder. Adding shell powder to the coating is beneficial to improving the adhesion, scrub resistance, flexibility and thermal conductivity of the coating. In addition, the use of shells, a natural low-cost inorganic filler, in the preparation of coatings provides a way to use discarded shells in a green way and avoids environmental pollution caused by the large-scale use of inorganic fillers.
[0033] In summary, the present invention designs a highly reflective material for colored pavement, wherein the highly reflective coating is a hydrophobic coating, and modified hollow glass microbeads are used as optical elements. Titanium dioxide has self-cleaning properties while enhancing reflection, and the combination of hydrophobicized modified hollow glass microbeads, polydimethylsiloxane and SiO2 nanoparticles determines the hydrophobic properties of the coating. Maintaining the super-hydrophobic function of the surface is crucial to improving the durability of the coating with self-cleaning properties. Therefore, the weather resistance, durability and life of the prepared adhesive tape are also optimized to a certain extent. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] In order to more clearly illustrate the embodiments of the present invention or the technical solutions therein, the following briefly introduces the drawings required for use in the descriptions of the embodiments and comparative examples. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative labor.
[0035] Figure 1 This is a schematic structural diagram of the high-reflective material for colored pavement prepared by the present invention;
[0036] Figure 2 It is a line graph of the wear resistance and impact resistance test results of each embodiment and comparative example sample;
[0037] Figure 3 It is a line graph of the retroreflection coefficient of each embodiment and comparative example sample at different incident angles. DETAILED DESCRIPTION
[0038] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. The described embodiments are part of the embodiments of the present invention, but not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0039] Embodiment 1: A high-reflective material for colored pavement is composed of the following three parts: a high-reflective coating, a substrate and an adhesive layer;
[0040] The high-reflective coating is composed of the following components in parts by weight: 20 parts of polydimethylsiloxane, 70 parts of environmentally friendly solvent oil, 20 parts of modified hollow glass microspheres, 4 parts of modified shell powder, 1 part of SiO2 nanoparticles, 1.5 parts of phenyl salicylate as an ultraviolet absorber, 3 parts of 2,6-di-tert-butyl-p-cresol as an antioxidant, 0.4 parts of ethylenediamine as a curing agent, 4 parts of aluminate fluorescent material doped with rare earth metals, and 0 parts of pigment; the substrate is a sheet material made of composite rubber with uniform thickness and a thickness of 0.6 mm; the adhesive layer is an epoxy resin adhesive.
[0041] The preparation of modified hollow glass microspheres includes the following steps:
[0042] S1, respectively measure sulfuric acid and hydrogen peroxide at a volume ratio of 3:1, immerse 50g of hollow glass microspheres in sulfuric acid, then add hydrogen peroxide, store at room temperature in a fume hood for 4 hours, then take out, rinse with distilled water 3 times and dry at room temperature for 12 hours to obtain hollow glass microspheres after surface hydrophilic treatment;
[0043] S2, respectively measuring 40 ml of tetrabutyl titanate and 130 ml of anhydrous ethanol, and dropping the tetrabutyl titanate into the anhydrous ethanol under vigorous stirring, wherein the stirring speed of the vigorous stirring is 1000 rpm and the stirring time is 10 min, to obtain a transparent solution A;
[0044] S3, measure 6 mL of distilled water and 30 mL of ethanol, mix them, slowly add 3 mL of acetic acid under vigorous stirring, adjust the pH to 3, the stirring speed of the vigorous stirring is 700 rpm, and the stirring time is 15 min, to obtain solution B;
[0045] S4, adding the surface hydrophilic treated hollow glass microspheres obtained in S1 to the transparent solution A obtained in S2, stirring to disperse the surface hydrophilic treated hollow glass microspheres in the transparent solution A, the stirring speed is 550 rpm, the stirring time is 15 min, and a solution C is obtained;
[0046] S5, slowly adding the solution B obtained in S3 to the solution C at a rate of 2 drops / second under vigorous stirring, wherein the vigorous stirring speed is 4500 rpm and the stirring time is 450 min, and a wet gel is obtained after the reaction is completed;
[0047] S6, drying the wet gel obtained in step S5 in an oven at 80° C. for 1 h, grinding until there is no agglomeration and the particle size is uniform, and calcining in a muffle furnace at 600° C. for 2 h to obtain titanium dioxide-coated hollow glass microspheres;
[0048] S7, taking 500 ml of toluene and 4 g of 1H,1H,2H,2H-perfluorooctyltriethyloxysilane and mixing them evenly, adding the titanium dioxide-coated hollow glass microspheres obtained in step S6 to the mixture of toluene and 1H,1H,2H,2H-perfluorooctyltriethyloxysilane, and storing them in a fume hood at room temperature for 60 hours. After the reaction is completed, wash with toluene, filter, and store them in a fume hood at room temperature for 2 days until the toluene evaporates, and then transfer them to an oven and dry them at 70° C. for 3 hours to obtain titanium dioxide-coated hollow glass microspheres after hydrophobic treatment, which are the modified hollow glass microspheres;
[0049] Among them, the diameter of the hollow glass microspheres is 120μm and the wall thickness is 2μm. Tetrabutyl titanate, acetic acid, ethanol, anhydrous ethanol, and toluene are all analytical grade reagents. The purity of tetrabutyl titanate and 1H,1H,2H,2H-perfluorooctyltriethyloxysilane is 98%, and the purity of toluene and acetic acid is 99.5%.
[0050] The preparation of modified shell powder comprises the following steps:
[0051] Q1, take 40g of natural shells and soak them in 0.05M hydrochloric acid solution for 12h, then soak them in 0.2M sodium hydroxide solution for 12h, rinse them with deionized water and dry them in an oven at 100℃ for 15min to obtain natural shells with impurities removed;
[0052] Q2, the natural shells obtained in step Q1 and freed of impurities are treated at a constant temperature of 800° C. for 8 h in a muffle furnace, and then transferred to a grinder and ball-milled at a speed of 30 rpm for 8 h to obtain shell powder;
[0053] Q3, weigh 30g shell powder and 9g KH-550, add into 80mL deionized water, heat to 90℃ in a water bath, stir at 130rpm, slowly add 0.4g aqueous sodium acrylate dispersant during heating, wait until the solution turns pure white, cool to room temperature, filter out insoluble matter, and dry in an oven at 60℃ for 20min to obtain modified shell powder.
[0054] A preparation method of a highly reflective material for a colored road surface comprises the following steps:
[0055] P1, weigh polydimethylsiloxane and environmentally friendly solvent oil, mix them in a container, and stir them magnetically at 150 rpm for 60 min to obtain mixture 1;
[0056] P2, maintaining stirring, according to the formula ratio, add the modified hollow glass microspheres, modified shell powder, SiO2 nanoparticles, and phosphor powder to the mixture 1 obtained in step P1 in sequence, and stir at 150 rpm for 45 min until uniformly dispersed to obtain a mixture 2;
[0057] P3, mix the ultraviolet absorber, antioxidant and curing agent in a container, stir at a stirring speed of 110 rpm for 20 minutes until uniform dispersion, obtain mixture 3, add the mixture 3 to the mixture 2 obtained in step P2, stir at 150 rpm for 1.5 hours, apply it to the surface of the substrate by spraying, cure the coating at room temperature for 24 hours, and dry at 80° C. for 1 hour to obtain a highly reflective coating;
[0058] P4, cut the high-reflective coating obtained in step P3 into the required size and shape, apply epoxy resin adhesive on the bottom or side of the substrate to form an adhesive layer, and tightly combine the high-reflective coating, substrate and adhesive layer through a hot pressing process, the hot pressing temperature is 100°C, the hot pressing time is 4 minutes, and it is cooled to room temperature to obtain the high-reflective material for colored pavement.
[0059] The highly reflective material for colored pavement is designed into different markings, patterns or decorations as needed during the construction process. The thickness of the highly reflective material for colored pavement is 1.8 mm. The pavement must be preheated before use and rolled after installation to make it fit the pavement.
[0060] Embodiment 2: A high-reflective material for colored pavement is composed of the following three parts: a high-reflective coating, a substrate and an adhesive layer;
[0061] The high-reflective coating is composed of the following components in parts by weight: 30 parts of polydimethylsiloxane, 70 parts of environmentally friendly solvent oil, 30 parts of modified hollow glass microspheres, 7 parts of modified shell powder, 1 part of SiO2 nanoparticles, 1.5 parts of ultraviolet absorber UV-P, 3 parts of dibutyl disulfide as an antioxidant, 0.4 parts of ethylenediamine as a curing agent, 4 parts of aluminate fluorescent material doped with rare earth metals, and 0 parts of pigment; the substrate is a sheet material made of composite rubber with uniform thickness and a thickness of 0.6 mm; the adhesive layer is an epoxy resin adhesive.
[0062] The preparation steps of the modified hollow glass microspheres, the modified shell powder and the high reflective material for colored pavement are the same as those in Example 1.
[0063] Embodiment 3: A high-reflective material for colored pavement is composed of the following three parts: a high-reflective coating, a substrate and an adhesive layer;
[0064] The high-reflective coating is composed of the following components in parts by weight: 40 parts of polydimethylsiloxane, 70 parts of environmentally friendly solvent oil, 40 parts of modified hollow glass microspheres, 10 parts of modified shell powder, 1 part of SiO2 nanoparticles, 1.5 parts of ultraviolet absorber RMB, 3 parts of dipropyl dihydroxybenzophenone as an antioxidant, 0.4 parts of ethylenediamine as a curing agent, 4 parts of aluminate fluorescent material doped with rare earth metals, and 0 parts of pigment; the substrate is a sheet material made of composite rubber with uniform thickness and a thickness of 0.6 mm; the adhesive layer is an epoxy resin adhesive.
[0065] The preparation steps of the modified hollow glass microspheres, the modified shell powder and the high reflective material for colored pavement are the same as those in Example 1.
[0066] Comparative Example 1: Based on Example 3, the difference is that the hollow glass microspheres are used directly without modification, and the other steps are the same as Example 3.
[0067] Comparative Example 2: Based on Example 3, the difference is that no modified shell powder is added, and the other steps are the same as Example 3.
[0068] Experimental example:
[0069] 1. Hydrophilicity and hydrophobicity test:
[0070] The prepared high-reflective material for colored pavement was cut into 5m×5cm samples, and 8μL of water was dropped on the surface of the sample. First, the hydrophilicity and hydrophobicity were judged by the wetting of the water drop on the surface of the sample, that is, the surface that can be wetted is hydrophilic, and the surface that cannot be wetted is hydrophobic. Secondly, the KZS-20 automatic contact angle meter can be used to perform contact angle test to more accurately judge the hydrophilicity and hydrophobicity. The contact angle <90° is hydrophilic, and the contact angle >90° is hydrophobic.
[0071] The hydrophilicity and hydrophobicity test results of the samples of various embodiments and comparative examples are shown in Table 1.
[0072] 2. Self-cleaning behavior:
[0073] The prepared highly reflective material for colored pavement was cut into 5cm×5cm samples. Red iron oxide powder was used as the contamination medium. The powder was evenly sprinkled in the middle of the sample. Water was then dripped on the top of the sample with a dropper. Visual observation was made to see whether the pollutants on the surface of the sample were washed away when water flowed through and whether there were any pollutants remaining in the flushing path.
[0074] The self-cleaning behavior test results of the samples of various embodiments and comparative examples are shown in Table 1.
[0075] 3.Thickness:
[0076] The thickness of the samples prepared in different embodiments and comparative examples was measured using a thickness gauge, and the thickness was measured at three different points and the average value was obtained as the thickness.
[0077] The thickness test results of the samples of various embodiments and comparative examples are shown in Table 1.
[0078] 4. Impact resistance test:
[0079] The impact resistance test is carried out in accordance with the specification of GB / T 1732-2020.
[0080] Place the impact tester on a stable platform, with the guide tube perpendicular to the horizontal plane. Adjust the weight of the impact tester to a certain height through the weight controller. Place the reflective surface of the sample flat on the base with the edge of the sample facing upwards. The distance between the edge of the sample where the impact is applied is 10mm, and the distance between the edges of adjacent impact points is 10mm. Press the weight controller button, and the weight will drop from the ground onto the punch. Take out the sample and observe whether the high-reflective coating on the sample has cracks, wrinkles, or peeling under natural sunlight.
[0081] If no cracks, wrinkles or peeling are observed, repeat the test at higher positions until cracks, wrinkles or peeling are observed, with each increase in height being 5 cm; if cracks, wrinkles or peeling are observed, repeat the test at lower positions until no cracks, wrinkles or peeling are observed, with each decrease in height being 5 cm. The results are expressed as the maximum height (cm) at which no cracks, wrinkles or peeling are observed in three tests.
[0082] The impact resistance test results of the samples of various embodiments and comparative examples are shown in Table 1. Figure 2 shown.
[0083] 5. Wear resistance determination:
[0084] Spray the high-reflective coating prepared in each embodiment and comparative example on a clean and dry base plate, spray two layers, with a time interval of 24 hours between the two layers, and dry for 48 hours; fix the sample on the working turntable of the wear tester, the required load on the pressure arm and the refurbished rubber grinding wheel, add a balance weight with the same weight as the grinding wheel at the end of the arm, and gently lower the pressure arm. Lower the dust nozzle and adjust it to 1mm away from the sample. Turn on the main switch, the dust cleaner switch, and the turntable switch in turn. Grind the sample for 50 turns to form a relatively flat surface. Turn off the power and take out the sample. Gently wipe off the floating debris with a brush and weigh it (accurate to 0.001g).
[0085] Adjust the counter according to the product standard and conduct the experiment. Stop when the specified wear-resistant revolutions are reached. Take out the sample, wipe off the shavings, and weigh it. The difference between the weight before and after is the weight loss of the paint film. The test is carried out at room temperature, and the parallel test is carried out twice. The difference between the average values each time is 5% of the average value, and the arithmetic mean of the result is taken.
[0086] The wear resistance test results of the samples of various embodiments and comparative examples are shown in Table 1. Figure 2 shown.
[0087] 6. Retroreflection coefficient:
[0088] Tested in accordance with JT / T 690-2022.
[0089] Select an appropriate minimum aperture to ensure that the entire retroreflector can be observed from the light receiver and the light source can be observed from the retroreflector. Place the incident aperture of the illuminance meter at the sample position and use the illuminance meter to replace the sample to measure the normal illuminance on the sample surface, recorded as m2 (i.e. E ⊥); Place the illuminometer and the sample back to their original positions, and use a light receiver to measure the reflected illuminance of the sample, recorded as m1 (or I1, L1); replace the sample with a black surface with the same shape and area as the sample and whose surface gloss does not affect the reading, measure the size of the stray light, and subtract the stray light reading m0 (or I0, L0) from the reading m1 (or I1, L1) to obtain m'1 (or I, L).
[0090] The direct luminous intensity method uses the following formula to calculate the retroreflection coefficient:
[0091] R A =I / (AE ⊥ );
[0092] R A ——Retroreflection coefficient, in candela per lux square meter [cd / (l x ·m 2 )];
[0093] A——the area of the sample, in square meters (m 2 ).
[0094] The test results of the retroreflection coefficient of each embodiment and comparative example sample at different incident angles are as follows: Figure 3 shown.
[0095] 7. Anti-aging:
[0096] The aging resistance was evaluated through ultraviolet irradiation experiments. Different samples were irradiated under the same ultraviolet light for 100 hours. After the experiment, the contact angle in the ultraviolet irradiation area was measured to compare whether the hydrophobic performance was weakened.
[0097] Table 1 Performance test results of various embodiments and comparative examples
[0098]
[0099] The present invention proposes a high reflective material for colored pavement, the structural schematic diagram of which is shown in FIG. Figure 1 As shown, it consists of a high reflective coating, a substrate and an adhesive layer.
[0100] It can be seen from the test data in Table 1 that all samples have good hydrophobicity, and their hydrophobicity comes from the combination of dimethylsiloxane and silica particles. After the modified hollow glass microspheres are added, the surface is hydrophobically modified, so that titanium dioxide not only does not affect the hydrophobic performance of the high-reflective coating, but enhances it; the self-cleaning test results show that the self-cleaning properties of titanium dioxide and the hydrophobic properties of the high-reflective coating work together to give it good self-cleaning performance, and the hydrophobic surface ensures the durability of the self-cleaning property of the material; the thickness of different samples is measured, showing that their thickness is relatively uniform and there is no significant difference between them; the impact resistance and wear resistance of the samples are tested, and the test results are shown in Tables 1 and Figure 2 As shown, the addition of modified shell powder as an inorganic filler has a significant effect on improving the mechanical properties of the material, showing good wear resistance and impact resistance. By comparing the aging resistance tests on the samples, it can be seen that the introduction of titanium dioxide into the material through modified hollow glass microbeads not only has the effect of improving the reflectivity of the coating, but its inherent ultraviolet absorption ability can effectively alleviate the aging of the material, further improving its weather resistance and service life.
[0101] From the relationship between the retroreflection coefficient and the incident angle of each embodiment and comparative sample, it can be seen that the retroreflection coefficient of all samples shows a trend of being maximum at 0° and decreasing toward both ends as the contact angle changes. At the same time, as the amount of modified hollow glass microspheres added increases, the retroreflection coefficient shows an overall increasing trend. Compared with the sample with unmodified hollow glass microspheres added, the retroreflection coefficient is significantly improved, reflecting that the presence of titanium dioxide is beneficial to the enhancement of the reflective ability of the sample.
[0102] The present invention and its embodiments are described above. The described embodiments are only some embodiments of the present invention, not all embodiments. The drawings are only one of many embodiments of the present invention. The detailed description of the embodiments of the present invention is not intended to limit the scope of the invention claimed for protection, but only represents the selected embodiments of the present invention. Based on this, other specific embodiments of the present invention obtained by those skilled in the art under the inspiration of the technical solution without creative labor should fall within the protection scope of the present invention.
Claims
1. A highly reflective material for colored pavement, characterized in that: It consists of the following three parts: high reflective coating, substrate and adhesive layer; The high-reflective coating is composed of the following components in parts by weight: 20-40 parts of polydimethylsiloxane, 60-80 parts of environmentally friendly solvent oil, 20-40 parts of modified hollow glass microspheres, 4-10 parts of modified shell powder, 0.1-2 parts of SiO2 nanoparticles, 0.5-2 parts of ultraviolet absorbers, 2-4 parts of antioxidants, 0.25-0.5 parts of curing agents, 2-6 parts of fluorescent powders, and 0-5 parts of pigments; the substrate is a sheet material made of composite rubber with uniform thickness, and the thickness is 0.5-1 mm; the adhesive layer is an epoxy resin adhesive; The modified hollow glass microspheres are prepared from the following raw materials: 30-70 g of hollow glass microspheres, 20-60 ml of tetrabutyl titanate, 80-180 ml of anhydrous ethanol, 2-4 ml of acetic acid, 20-40 ml of ethanol, 500 ml of toluene, and 2-5 g of 1H,1H,2H,2H-perfluorooctyltriethyloxysilane; The hollow glass microspheres have a diameter of 90-150 μm and a wall thickness of 1-2 μm. The tetrabutyl titanate, acetic acid, ethanol, anhydrous ethanol, and toluene are all analytically pure reagents. The purity of 1H, 1H, 2H, 2H-perfluorooctyl triethyloxysilane is 98%; The modified shell powder is prepared from the following raw materials: 30-50g natural shell, 6-12g silane coupling agent, 0.3-0.6g dispersant, the silane coupling agent is KH-550, and the dispersant is an aqueous sodium acrylate dispersant; The curing agent is one of ethylenediamine, diethylenetriamine, and acrylic anhydride; the ultraviolet absorber is one of phenyl salicylate, ultraviolet absorber UV-P, ultraviolet absorber UV-O, ultraviolet absorber UV531, and ultraviolet absorber RMB; the antioxidant is one of 2,6-di-tert-butyl-p-cresol and dibutyl disulfide; the pigment is one of iron chrome black, nickel titanate yellow, cobalt green, cobalt blue, iron oxide red, and ordinary color paste or no pigment is added; and the phosphor is a rare earth metal-doped aluminate fluorescent material; The preparation of the modified hollow glass microspheres comprises the following steps: S1, respectively measuring sulfuric acid and hydrogen peroxide at a volume ratio of 3:1, immersing the hollow glass microspheres in sulfuric acid, then adding hydrogen peroxide, storing them in a fume hood at room temperature for 4 hours, then taking them out, rinsing them with distilled water 2 to 3 times and drying them at room temperature for 12 hours, to obtain hollow glass microspheres after surface hydrophilic treatment; S2, respectively measuring tetrabutyl titanate and anhydrous ethanol, and dropping the tetrabutyl titanate into the anhydrous ethanol under vigorous stirring, wherein the stirring speed of the vigorous stirring is 800-1200 rpm and the stirring time is 5-15 min, to obtain a transparent solution A; S3, measuring 5-8 mL of distilled water and ethanol, slowly adding acetic acid under vigorous stirring, adjusting the pH to 2-3, the stirring speed of the vigorous stirring is 500-800 rpm, and the stirring time is 10-20 min, to obtain solution B; S4, adding the hollow glass microspheres after the surface hydrophilic treatment obtained in S1 to the transparent solution A obtained in S2, stirring to disperse the hollow glass microspheres after the surface hydrophilic treatment in the transparent solution A, the stirring speed is 400-600 rpm, the stirring time is 10-20 min, and a solution C is obtained; S5, slowly adding the solution B obtained in S3 to the solution C at a rate of 1-2 drops / second under vigorous stirring, wherein the vigorous stirring speed is 4000-5000 rpm, and the stirring time is 30-60 min, and a wet gel is obtained after the reaction is completed; S6, drying the wet gel obtained in step S5 in an oven at 80° C. for 1 h, grinding until there is no agglomeration and the particle size is uniform, and calcining in a muffle furnace at 500-700° C. for 2 h to obtain titanium dioxide-coated hollow glass microspheres; S7, taking toluene and 1H,1H,2H,2H-perfluorooctyltriethyloxysilane and mixing them evenly, adding the titanium dioxide-coated hollow glass microspheres obtained in step S6 to the mixture of toluene and 1H,1H,2H,2H-perfluorooctyltriethyloxysilane, and storing them in a fume hood at room temperature for 48 to 72 hours, washing with toluene after the reaction, filtering and storing them in a fume hood at room temperature for 2 days until the toluene evaporates, and then transferring them to an oven and drying them at 70° C. for 1 to 4 hours to obtain the titanium dioxide-coated hollow glass microspheres after hydrophobic treatment, which are the modified hollow glass microspheres; The preparation of the modified shell powder comprises the following steps: Q1, soak natural shells in 0.05M hydrochloric acid solution for 10-14h, then soak in 0.2M sodium hydroxide solution for 10-14h, rinse with deionized water and dry in a 100℃ oven for 10-20min to obtain natural shells with impurities removed; Q2, the natural shells obtained in step Q1 and freed of impurities are treated in a muffle furnace at 800-900° C. for 6-10 hours, and then transferred to a grinder for ball milling at a speed of 30 rpm for 7-9 hours to obtain shell powder; Q3, weigh 20~40g shell powder and 6~12g silane coupling agent, add into 80mL deionized water, heat to 85~95℃ in a water bath, stir at 100~150rpm, slowly add dispersant during heating, wait until the solution turns pure white, cool to room temperature, filter out insoluble matter, and dry in oven at 60℃ for 20min to obtain modified shell powder.
2. A method for preparing a highly reflective material for a colored pavement according to claim 1, characterized in that: The following steps are involved: P1, weigh polydimethylsiloxane and environmentally friendly solvent oil, mix them in a container, and stir them magnetically at 100-200 rpm for 30-90 min to obtain a mixture 1; P2, maintaining stirring, according to the formula ratio, add the modified hollow glass microspheres, modified shell powder, SiO2 nanoparticles, fluorescent powder and pigment to the mixture 1 obtained in step P1 in sequence, and stir at 100-200 rpm for 30-60 min until uniformly dispersed, to obtain mixture 2; P3, mixing the ultraviolet absorber, antioxidant and curing agent in a container, stirring at a stirring speed of 60-150 rpm for 10-30 min until uniformly dispersed, to obtain a mixture 3, adding the mixture 3 to the mixture 2 obtained in step P2, stirring at 100-200 rpm for 1-2 h, applying the mixture to the surface of the substrate by spraying, brushing, rolling or dipping, curing and drying the coating to obtain a highly reflective coating; P4, cutting the high-reflective coating obtained in step P3 into the required size and shape, coating the bottom or side of the substrate with epoxy resin adhesive to form an adhesive layer, and tightly combining the high-reflective coating, the substrate and the adhesive layer through a hot pressing process, wherein the hot pressing temperature is 80-120°C and the hot pressing time is 2-5 minutes. After cooling to room temperature, the high-reflective material for colored pavement is obtained.
3. The method for preparing a highly reflective material for a colored pavement according to claim 2, characterized in that: The curing in step P3 is carried out at room temperature for 24 hours, and the drying is carried out at 80° C. for 1 hour.
4. The method for preparing a highly reflective material for a colored road surface according to claim 3, characterized in that: The highly reflective material for colored pavement is designed into different markings, patterns or decorations as needed during the construction process. The thickness of the highly reflective material for colored pavement is 1-3 mm. The pavement must be preheated before use and rolled after installation to make it fit the pavement.