A low thermal conductivity plate and its preparation method and application
By pretreatment, modification and glue application of wooden veneers, combined with longitudinal paving and hot pressing, the shortcomings of low-density wood window frame materials in building energy consumption and weather resistance are solved, and the low thermal conductivity of plates are achieved The preparation has good weather resistance and mechanical properties, and is suitable for energy-saving door and window profiles.
Patent Information
- Application Number
- CN202410097294.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-01-23
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-01-23
AI Technical Summary
Existing building doors and window materials have shortcomings in taking into account both thermal insulation and weather resistance. In particular, low-density wood window frame materials are prone to warping, cracking, deformation, discoloration, mold and other problems during long-term use, resulting in their construction energy. Poor performance in terms of consumption and thermal comfort.
By pretreating wooden veneers, modifying low molecular weight phenolic resin and applying high molecular weight phenolic resin, combined with longitudinal paving and hot pressing, a low thermal conductivity plate is formed to enhance the uniformity, stability and glue of the material. Connection capacity, reduce heat transfer speed.
The preparation of low thermal conductivity plates has been achieved, with good weather resistance, stability and mechanical strength, and is suitable for door and window profiles, reducing building energy consumption and extending the life of building door and window components.
Smart Images

Figure CN118081918B_ABST
Abstract
Description
Technical Field
[0001] The present application relates to a low thermal conductivity board material and a preparation method and application thereof, belonging to the technical field of wood composite materials. Background Art
[0002] At present, the proportion of building energy consumption in the total social energy consumption is close to 30%. The development and promotion of low-energy buildings has become the key to promoting energy conservation and carbon reduction. After years of development, the insulation effect of building exterior walls and roofs has reached its limit. Building exterior windows are key building components for achieving indoor lighting, lighting, ventilation, landscape and other functions, and are also weak components for thermal insulation. In the total energy consumption of building envelope structures, the energy consumption of building doors and windows accounts for about 50%, and the heat transfer coefficient of windows is about 4 times and 20 times that of walls and floors. Existing energy-saving windows are difficult to take into account the dual performance of building exterior windows as building heat gain and heat loss components. At the same time, with the rapid development of urbanization, the number of residential buildings currently developed is gradually increasing, and the demand for building doors and windows is also showing a trend of increasing year by year. Under the general trend of energy conservation and emission reduction, more energy-saving door and window systems are urgently needed. In addition, for any door and window, the glass is certain, and the window frame is different. The thermal conductivity technology of the window frame directly determines the K value of the window. The energy-saving window frame materials on the current construction market mainly include thermal insulation aluminum alloy windows, plastic windows, wooden windows, etc., especially thermal insulation aluminum alloy windows are the most popular.
[0003] However, the thermal conductivity of aluminum is 203w / mk. The thermal conductivity is high and the heat transfer is too fast, so the thermal insulation performance is poor. Aluminum alloy needs to be thermally insulated, and the technical level of thermal insulation must be improved to make aluminum windows have higher thermal insulation performance, but the cost is greatly increased, so aluminum alloy window frames are gradually replaced. At present, aluminum-clad wood windows can meet the thermal conductivity of 1.0w / m 2 .k, but its scope of application is limited and it is only used in the area north of the Yangtze River.
[0004] Since wood is a porous material, heat flow must be transferred through its substance and pores. However, the thermal conductivity of wood in the pores is much smaller than that of the wood substance. Therefore, the density of wood is positively correlated with its thermal conductivity. The lower the density of wood, the lower its thermal conductivity. When used as an exterior window structure, its thermal insulation effect is also better. When low-density logs are used for building exterior window structures, they are in contact with the outdoors for a long time. Due to their loose structure, soft material, low strength, poor stability and easy decay, external factors such as temperature, humidity and precipitation can easily affect the performance of wooden window frames, resulting in warping, cracking, deformation, discoloration, mildew and other phenomena, which in turn affect the performance of exterior windows. Therefore, when wood is used as window frame material, its weather resistance is also directly related to the indoor thermal comfort and building energy consumption level of the building.
[0005] For the existing materials that can be used for window profiles:
[0006] 1. The compression ratio of traditional reconstituted wood is large (50% to 75%) and the density is high (0.80g / cm 3 ~1.40g / cm 3 ), its various mechanical properties have been improved to varying degrees, providing the prerequisite for its application as a load-bearing structure such as beams and columns in the field of structural engineering. However, when it is used as a non-load-bearing window profile, the heavy material is not conducive to the later processing and installation of the window frame, and increases the production cost of the substrate. In addition, the high density also increases its thermal conductivity and enhances its thermal conductivity, which is not conducive to energy conservation and heat preservation of buildings. Although the density of oak window profiles is low, its mechanical properties cannot be guaranteed. When materials such as glass are applied to the profiles, they will be damaged due to their low ability to withstand external forces, thus failing to ensure the ultra-high light transmittance of the exterior windows.
[0007] 2. The window profiles currently on the market are made of oak, poplar and other broad-leaved wood. Although the reconstituted wood prepared by debonding veneer and ordinary phenolic resin has stable performance, the broad-leaved wood itself is loose, has a large diameter of the duct, has a small density, low strength, and is light and soft. In addition, the broad-leaved wood is composed of ducts, wood rays and fibers, which are more complex in structure than coniferous wood, with irregular arrangement and uneven material. When it is used as a building exterior window structure in a long-term harsh outdoor environment, it is prone to cracking, deformation and other problems. In addition, the cured water-soluble phenolic resin is brittle and not impact-resistant. When the bonding part is subjected to external force, cracks are easily generated and rapidly expand, resulting in cracking of the adhesive layer and fatigue resistance. In addition, the inaccurate control of the process flow during the production process makes it more prone to cracking and poor overall weather resistance.
[0008] 3. Yuexiu Wood-PL series products use radiata pine veneer and impregnated phenolic / modified phenolic resin as the basic raw materials. The impregnated phenolic resin has a low foaming rate during the curing process; the thermal conductivity of the radiata pine veneer does not decrease significantly after impregnation and compression. Yuexiu Wood-PL products are mainly used for outdoor flooring and have not been used for door and window materials. It can press 21mm thick boards, but cannot be used for window profiles. At the same time, the thermal conductivity of the material is not taken into consideration.
[0009] In summary, there is an urgent need to develop a low-density, lightweight solid wood window profile that has low thermal conductivity, good weather resistance, stability, and good mechanical strength. This is of great significance for improving the indoor thermal environment, reducing building energy consumption, increasing wood utilization, and extending the life of building door and window components. Summary of the invention
[0010] In order to solve the above problems, a low thermal conductivity board material and a preparation method and application thereof are provided. The wood veneer is pretreated and then subjected to a low molecular weight phenolic resin modification treatment and a high molecular weight phenolic resin sizing treatment respectively. The low molecular weight phenolic resin can penetrate into the interior of the wood, thereby improving the uniformity and stability of the wood. The gluing enhances the bonding ability between veneer layers. The synergistic effect of the two makes the overall thermal conductivity of the board material low, and it has good weather resistance and stability.
[0011] According to one aspect of the present application, a method for preparing a low thermal conductivity plate is provided, comprising the following steps:
[0012] (1) Pretreatment: pretreating the wood veneer with an alkaline solution;
[0013] (2) Modification: vacuum impregnation of wood veneer with low molecular weight phenolic resin;
[0014] (3) Gluing: Use high molecular weight phenolic resin for surface treatment and evenly apply the modified wood veneer;
[0015] (4) Laying: Lay several glued wood veneers longitudinally and pre-press them;
[0016] (5) Pressing: Pressing the pre-pressed sheet, and stacking and cold pressing after demoulding to obtain the low thermal conductivity sheet.
[0017] Optionally, the mass concentration of the alkaline solution in step (1) is 2-5‰, and the alkaline substance used is one of sodium hydroxide, sodium bicarbonate or sodium carbonate.
[0018] Optionally, the material of the wooden veneer in step (1) is poplar, pine or birch;
[0019] The pretreatment time is 20-60 minutes, and the temperature is 40-100°C.
[0020] Specifically, by using alkaline solution for pretreatment, the surface tension and lignin structure of the wood are destroyed, the porosity and permeability of the wood are increased, and surface pollutants are removed. Water-soluble substances in the wood can be extracted, making the wood easier to absorb subsequent modified phenolic resins, easier to modify thoroughly, and improving the uniformity and corrosion resistance of the material, and making the thermal conductivity of the material more uniform.
[0021] Optionally, the molecular weight of the low molecular weight phenolic resin in step (2) is 100-400, the vacuum degree in vacuum impregnation is: negative pressure -0.05 to -0.12 MPa, time 5-30 min, pressurization pressure 0.6-1.5 MPa, time 30-60 min, and the treatment time is 35-90 min.
[0022] Optionally, the molecular weight of the high molecular weight phenolic resin in step (3) is 300-800, and the dosage is 0.07-0.11 g / cm 3 .
[0023] Specifically, the solid content of the low molecular weight phenolic resin is 15-21%, and the solid content of the high molecular weight phenolic resin is 45-55%.
[0024] Specifically, low molecular weight phenolic resin can enter the cell wall, cell cavity and intercellular space to fill and modify the wood. This deep modification makes the wood tighter and stronger, thereby reducing the speed of heat transfer through the wood.
[0025] Optionally, in step (4), the pre-pressing pressure is 5-10 MPa and the time is 30-60 min.
[0026] Optionally, in step (5), the pressing temperature is 115-130° C., the time is 30-90 min, and the stacking cold pressing time is 3-6 days.
[0027] Optionally, in step (5), if the material of the wooden veneer is pine or poplar, the hot pressing pressure is 4-6 MPa; if the material is birch, the hot pressing pressure is 5-7 MPa.
[0028] According to another aspect of the present application, a low thermal conductivity plate is also provided, which is prepared by the above preparation method.
[0029] According to another aspect of the present application, there is also provided an application of the low thermal conductivity sheet material, wherein the low thermal conductivity sheet material is used for door and window profiles.
[0030] The beneficial effects of this application include but are not limited to:
[0031] 1. According to the preparation method of the low thermal conductivity board material of the present application, by carrying out different pre-treatments on materials of different tree species, the water-soluble organic matter in the logs can be effectively removed, the corrosion resistance of the material can be improved, and the alkaline solution can destroy some chemical bonds in the wood (such as the bonds between lignin and cellulose), remove grease and impurities on the surface of the wood, and improve the effect of its subsequent treatment. In addition, the alkali treatment can increase the porosity of the wood, making the subsequent modified phenolic resin easier to penetrate.
[0032] 2. According to the preparation method of the low thermal conductivity board material of the present application, a low molecular weight resin is first used to penetrate into the micropores of the wood to fill the cell walls, cell cavities, etc., and then integrated with the lignin in the wood after curing to form a body structure, thereby improving the dimensional stability of the material. The deep-level modification makes the wood tighter and stronger, thereby reducing the speed of heat transfer through the wood and achieving the effect of reducing the thermal conductivity.
[0033] 3. According to the preparation method of the low thermal conductivity board material of the present application, the surface of the material is treated with a high molecular weight toughened phenolic resin after modification, which effectively improves the bonding ability of the bonding layer, forms an interlayer water-blocking layer, reduces the influence of moisture on the material, and improves the dimensional stability of the material.
[0034] 4. According to the preparation method of the low thermal conductivity board material of the present application, the use of two phenolic resins with specific molecular weight forms micro-foamed pores during the curing process. The two work synergistically to impart the low thermal conductivity of the resin itself to the material, and then cooperate with the wood itself to form a material with better thermal insulation effect.
[0035] 5. According to the preparation method of the low thermal conductivity board of the present application, by adopting full longitudinal paving, the maximum compressive strength of the raw materials along the grain can be exerted. In addition, the longitudinal paving follows the growth direction of the logs, the number of splicing in the length direction is small, and the number of splicing seams in the transverse paving is large. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] The drawings described herein are used to provide a further understanding of the present application and constitute a part of the present application. The illustrative embodiments of the present application and their descriptions are used to explain the present application and do not constitute an improper limitation on the present application. In the drawings:
[0037] Figure 1 This is a schematic diagram of the low thermal conductivity plate structure involved in Example 1 of the present application. DETAILED DESCRIPTION
[0038] The present application is described in detail below with reference to embodiments, but the present application is not limited to these embodiments.
[0039] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. The reagents or raw materials used in the present invention can be purchased through conventional channels. Unless otherwise specified, the reagents or raw materials used in the present invention are used in a conventional manner in the art or in accordance with the product instructions. In addition, any method and material similar or equivalent to the described content can be applied to the method of the present invention. The preferred implementation methods and materials described in this patent are for demonstration purposes only.
[0040] The low molecular weight small molecule phenolic resin in the present application is a commercially available small molecule water-based phenolic resin.
[0041] Example 1: Using radiata pine core material + birch veneer to press a board with a thickness of 60 mm
[0042] The preparation method comprises the following steps:
[0043] (1) Pretreatment: The peeled radiata pine veneer and birch veneer were pretreated with a sodium carbonate solution with a mass concentration of 3‰ at 80°C for 45 min;
[0044] (2) Modification: The veneer was vacuum impregnated with a low molecular weight phenolic resin with a solid content of 20% and a molecular weight of 200-400 for 45 min (vacuuming to -0.05 MPa for 15 min, and then pressurizing at 1.0 MPa for 30 min);
[0045] (3) Gluing: Use a 50% toughened phenolic resin with a molecular weight of 300-800 for surface treatment and evenly apply it to the modified veneer. The amount is 0.08g / cm 3 ;
[0046] (4) Paving: 50 sheets of 1.3 mm thick radiata pine veneers were longitudinally laid as the core, and 3 sheets of 1.5 mm thick birch veneers were longitudinally laid on each side, and pre-pressed with a pre-pressing pressure of 7 MPa for 45 min;
[0047] (5) Pressing: Pressing at 125°C for 65 min, hot pressing pressure 5 MPa, and stacking and cold pressing after demolding, pressing time 4 days;
[0048] Example 2: Using radiata pine to press a board with a thickness of 85 mm
[0049] The preparation method comprises the following steps:
[0050] (1) Pretreatment: The peeled radiata pine veneer was pretreated with a sodium bicarbonate solution with a mass concentration of 5‰ at 60°C for 60 min;
[0051] (2) Modification: The veneer was vacuum impregnated with a low molecular weight phenolic resin with a solid content of 18% and a molecular weight of 200-400 for 50 min (vacuuming to -0.08 MPa for 10 min, then pressurizing at 0.6 MPa for 40 min);
[0052] (3) Gluing: Use a toughened phenolic resin with a solid content of 53% and a molecular weight of 300-800 for surface treatment and evenly apply it to the modified veneer. The amount used is 0.07g / cm 3 ;
[0053] (4) Paving: 79 1.3 mm thick veneers are laid in a longitudinal manner and pre-pressed at a pressure of 6 MPa for 30 min.
[0054] (5) Pressing: Pressing at 120°C for 45 min, hot pressing pressure 4.5 MPa, stacking and cold pressing after demolding, pressing time 3 days;
[0055] Example 3: Using birch wood to press a profile with a thickness of 21 mm
[0056] The preparation method comprises the following steps:
[0057] (1) Pretreatment: The peeled birch veneer was pretreated with a sodium hydroxide solution with a mass concentration of 1‰ at 100°C for 70 min;
[0058] (2) Modification: The veneer was vacuum impregnated with a low molecular weight phenolic resin with a solid content of 15% and a molecular weight of 100-400 for 85 min (vacuuming to -0.10 MPa for 30 min, and then pressurizing at 1.5 MPa for 55 min);
[0059] (3) Gluing: Use a toughened phenolic resin with a molecular weight of 300-800 and a solid content of 55% for surface treatment, and evenly apply it to the modified veneer. The amount used is 0.11g / cm 3 ;
[0060] (4) Paving: 15 sheets of 1.5 mm thick processed birch veneers were fully longitudinally laid and pre-pressed at a pre-pressing pressure of 10 MPa for 60 min;
[0061] (5) Pressing: Pressing at 130°C for 90 min, hot pressing pressure of 7 MPa, and stacking cold pressing after demolding, pressing time of 6 days;
[0062] Comparative Example 1
[0063] The difference between Comparative Example 1 and Example 2 is that no pretreatment is performed in Comparative Example 1.
[0064] Comparative Example 2
[0065] The difference between Comparative Example 2 and Example 2 is that in Comparative Example 2, a small molecular weight phenolic resin with a molecular weight of 200-400 is used in both the modification and sizing steps.
[0066] Comparative Example 3
[0067] The difference between Comparative Example 3 and Example 2 is that in Comparative Example 3, toughening phenolic resin with a molecular weight of 300-800 is used in both the modification and sizing steps.
[0068] Comparative Example 4
[0069] The difference between Comparative Example 4 and Example 2 is that in Comparative Example 4, the modification and sizing steps are combined into one, and the phenolic resins with a high molecular weight of 800-100 and a low molecular weight of 200-400 are directly mixed in a mass ratio of 8:1 for modification, and the mixture is vacuumed to -0.10 MPa for 20 minutes and pressurized to 0.07 MPa for 45 minutes.
[0070] Experimental example
[0071] The thermal conductivity of the plates obtained in Examples 1-3 and Comparative Examples 1-4 was tested in accordance with GB / T 10294-2008. The results are shown in Table 1 below.
[0072] Table 1 Experimental results of various embodiments and comparative examples
[0073]
[0074] From the above results, it can be seen that the low thermal conductivity board obtained by the preparation method defined in the present application has a thermal conductivity of about 0.07W / (m·K), which can maintain the original natural texture and low thermal conductivity of the wood, while also having good stability, strength, mildew resistance and corrosion resistance. The wooden windows produced by it are energy-saving, low-carbon, environmentally friendly and sustainable door and window products, and also have the advantages of good wind pressure resistance, high air tightness and water tightness, etc., and have great market prospects for use as door and window frames.
[0075] The above is only the embodiment of the present application, and the protection scope of the present application is not limited by these specific embodiments, but is determined by the claims of the present application. For those skilled in the art, the present application can have various changes and variations. Any modification, equivalent replacement, improvement, etc. made within the technical ideas and principles of the present application should be included in the protection scope of the present application.
Claims
1. A method for preparing a low thermal conductivity plate, characterized in that: The following steps are involved: (1) Pretreatment: Use alkaline solution to pretreat the wood veneer; (2) Modification: vacuum impregnation of wood veneer with low molecular weight phenolic resin; (3) Gluing: Use high molecular weight phenolic resin for surface treatment and evenly apply the modified wood veneer; (4) Laying: Lay several sheets of glued wood veneer longitudinally and pre-press them; (5) Pressing: Pressing the pre-pressed sheet, and stacking and cold pressing after demolding to obtain the low thermal conductivity sheet; Wherein, the molecular weight of the low molecular weight phenolic resin in step (2) is 100-400, and the treatment time is 1-3h; The molecular weight of the high molecular weight phenolic resin in step (3) is 300-800, and the dosage is 0.07-0.11 g / cm 3 .
2. The preparation method according to claim 1, characterized in that: The mass concentration of the alkaline solution in step (1) is 2-5‰, and the alkaline substance used is one of sodium hydroxide, sodium bicarbonate or sodium carbonate.
3. The preparation method according to claim 1, characterized in that: The material of the wooden veneer in step (1) is poplar, pine or birch; The pretreatment time is 20-60 minutes, and the temperature is 40-100°C.
4. The preparation method according to claim 1, characterized in that: In step (4), the pre-pressing pressure is 5-10 MPa and the time is 30-60 min.
5. The preparation method according to claim 1, characterized in that: In step (5), the pressing temperature is 115-130°C, the pressing time is 30-90 minutes, and the stacking cold pressing time is 3-6 days.
6. The preparation method according to claim 1, characterized in that: In step (5), if the material of the wood veneer is radiata pine, the hot pressing pressure is 4-6 MPa; if the material is birch, the hot pressing pressure is 5-7 MPa.
7. A low thermal conductivity plate, characterized in that: The method is described in any one of claims 1 to 6.
8. An application of the low thermal conductivity plate material as claimed in claim 7, characterized in that: The low thermal conductivity sheet material is used for door and window profiles.
Citation Information
Patent Citations
Preparation method for low-cost insulating phenolic resin laminated board resistant to moisture and heat
CN105773763A
Preparation method of resin impregnated wood powder filled wood-plastic composite material
CN113897071A