A method and product for preparing multi-layer tantalum carbide coating by CVD method
By controlling the airflow ratio and sinusoidal cross-fluctuation inlet reaction gas in real time, multi-layer tantalum carbide coating was prepared by CVD method, which solved the problem of easy cracks in the preparation of tantalum carbide coating by CVD method, and improved the purity and protection effect of the coating , extends the service life of the substrate material.
Patent Information
- Application Number
- CN202410261850.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-07
- Publication Date
- 2024-11-19
- Estimated Expiration
- 2044-03-07
AI Technical Summary
The existing CVD method to prepare tantalum carbide coatings is prone to defects such as cracks, resulting in reduced protective effect of the coating, shortened life of the substrate material, and unstable crystal growth.
By controlling the airflow ratio in real time, the reaction gas flow is allowed to pass through sinusoidal cross-wave form, and a multi-layer tantalum carbide coating is formed on the surface of the base material by using tantalum salt, alkanes and hydrogen as raw materials, and the airflow ratio is controlled from 3.8 to 4.2: 1.9~2.1, forming a multi-layer interlaced structure.
It improves the purity and protection effect of the tantalum carbide coating, prevents cracks from extending to the base material, enhances the bonding with the base material, reduces the chance of cracks, and extends the coating life.
Smart Images

Figure CN118109799B_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of semiconductor technology and relates to the preparation of a semiconductor substrate, and specifically relates to a method and product for preparing a multilayer tantalum carbide coating by a CVD method. Background Art
[0002] The information disclosed in this background technology section is only intended to enhance the understanding of the overall background of the invention, and should not necessarily be regarded as an admission or any form of suggestion that the information constitutes the prior art already known to a person skilled in the art.
[0003] Semiconductor materials are an important cornerstone for the production of integrated circuits, optoelectronic devices, sensors and other electronic components. There are many types of semiconductor materials. Compared with the first-generation semiconductor Si materials, the third-generation semiconductor materials have the advantages of higher bandgap width, high breakdown electric field, high electrical conductivity, high thermal conductivity, etc. They are widely used in aerospace, microwave communications, smart grids, new energy vehicles, national defense and military industries, etc. The single crystal growth temperature of the third-generation semiconductor is as high as 2000℃, and the reaction atmosphere is complex under high temperature environment. Only graphite and C / C composite materials can be used as thermal field components for growth. They are eroded by the reaction atmosphere during the long-term growth process, resulting in increasing losses, thereby reducing their service life and increasing production costs. At the same time, during the loss process, due to changes in the thermal field, the instability and non-repeatability of crystal growth will also occur, and the corrosive atmosphere will enter the crystal lattice, affecting the crystal quality. Tantalum carbide ceramic materials have a high melting point (3880℃) and a small thermal expansion coefficient (6.6×10 -6 K -1 ), strong bending resistance (340-400MPa), high hardness (Mohs hardness 9-10) and excellent chemical stability, it has become an emerging ceramic material in recent years. Forming a tantalum carbide film on the substrate material can effectively isolate the cavity atmosphere from the substrate material, which can effectively increase the service life of the substrate material and improve the quality of the single crystal.
[0004] The preparation methods of tantalum carbide films mainly include molten salt method, plasma spraying method, slurry sintering method and chemical vapor deposition method, among which chemical vapor deposition (CVD) can obtain high density and high purity that are difficult to obtain by other methods. Chemical vapor deposition is a process in which the reactants undergo a series of physical and chemical changes such as decomposition, diffusion, adsorption, surface migration and growth in a vapor deposition furnace to form a coating on the surface of the substrate material. In the prior art, chemical vapor deposition will cause the coating to grow in a single crystal direction due to its deposition method. Defects in the growth process will extend from the substrate surface along the growth direction to the coating surface, especially crack defects. The corrosive atmosphere can erode the substrate surface and reduce the protective effect of the coating. Summary of the invention
[0005] In order to solve the problem that cracks and other defects are easily generated during the preparation of tantalum carbide coating products by the existing CVD method, the purpose of the present invention is to provide a method and product for preparing a multilayer tantalum carbide coating by the CVD method.
[0006] In order to achieve the above object, the present invention is implemented through the following technical solutions:
[0007] In a first aspect, the present invention provides a method for preparing a multilayer tantalum carbide coating by a CVD method, wherein a tantalum salt and a reaction gas are used as raw materials to prepare a tantalum carbide coating on the surface of a substrate by a CVD method, and the reaction gas flow is introduced in a sinusoidal cross-wave manner by real-time control of the gas flow ratio, thereby forming a multilayer tantalum carbide coating;
[0008] Among them, the reaction gas includes alkane and hydrogen, and the real-time control of the gas flow ratio is to introduce tantalum salt carrier gas, alkane and hydrogen through a circulation control method under the condition that the reaction gas carrier gas flow remains unchanged. A cycle process of the tantalum salt carrier gas control method is: within a set time, the tantalum salt carrier gas flow rate first increases from 45% to 55% of the original flow rate to the original flow rate of the tantalum salt carrier gas, and then decreases to 45% to 55% of the original flow rate of the tantalum salt carrier gas; a cycle process of the alkane gas flow control method is: within a set time, the alkane flow rate first decreases to 45% to 55% of the original flow rate of the alkane, and then increases to the original flow rate of the alkane; a cycle process of the hydrogen gas flow control method is: within a set time, the hydrogen flow rate first decreases to 45% to 55% of the original flow rate of hydrogen, and then increases to the original flow rate of hydrogen; the ratio of the tantalum salt carrier gas, the original flow rate of the alkane to the original flow rate of the hydrogen is 3.8 to 4.2:1.9 to 2.1:1.
[0009] Preferably, the tantalum salt is heated to sublime, and then transported by a tantalum salt carrier gas to react with the reaction gas to achieve chemical vapor deposition. Specifically, the temperature at which the tantalum salt is heated to sublime is 180 to 800° C. Specifically, the flow rate of the tantalum salt carrier gas is 500 to 2000 sccm. Specifically, the tantalum salt carrier gas is argon.
[0010] Preferably, the alkane is at least one of methane, ethane and propane.
[0011] Preferably, the alkane flow rate is 50 to 500 sccm.
[0012] Preferably, the flow rate of hydrogen is 25-250 sccm.
[0013] Preferably, the reaction gas is delivered by a reaction gas carrier gas. Specifically, the flow rate of the reaction gas is 500-2000 sccm.
[0014] Preferably, the ratio of the flow rate of tantalum salt carrier gas, the flow rate of reaction gas carrier gas, the original flow rate of alkane and the original flow rate of hydrogen is 3.8-4.2:3.8-4.2:1.9-2.1:1, specifically 3.8-4.2:3.8-4.2:2:1.
[0015] Preferably, the temperature of CVD deposition is 1000-1800° C. Specifically, the heating rate to the deposition temperature is 5-15° C. / min. Specifically, the deposition time is 10-20 h.
[0016] Preferably, during one cycle of the tantalum salt carrier gas control method, the set time is 1.8 to 2.2 hours.
[0017] Preferably, during one cycle of the tantalum salt carrier gas control method, in the first half of the set time, the tantalum salt carrier gas flow rate increases from 45% to 55% of the original tantalum salt carrier gas flow rate to the original tantalum salt carrier gas flow rate; in the second half of the set time, the tantalum salt carrier gas flow rate decreases from the original tantalum salt carrier gas flow rate to 45% to 55% of the original tantalum salt carrier gas flow rate.
[0018] Preferably, during one cycle of the alkane gas flow control method, the set time is 1.8 to 2.2 hours.
[0019] Preferably, during one cycle of the alkane gas flow control method, in the first half of the set time, the alkane flow rate increases from the original alkane flow rate to 45-55% of the original alkane flow rate; in the second half of the set time, the alkane flow rate increases from 45-55% of the original alkane flow rate to the original alkane flow rate.
[0020] Preferably, during one cycle of the hydrogen gas flow control method, the set time is 1.8 to 2.2 hours.
[0021] Preferably, during one cycle of the hydrogen gas flow control method, in the first half of the set time, the hydrogen flow rate increases from the original hydrogen flow rate to 45-55% of the original hydrogen flow rate; in the second half of the set time, the hydrogen flow rate increases from 45-55% of the original hydrogen flow rate to the original hydrogen flow rate.
[0022] Preferably, the substrate material comprises at least one of graphite, C / C composite material, ceramic and metal.
[0023] The substrate material is pretreated before depositing the tantalum carbide coating. Preferably, the pretreatment process of the substrate material is: using an organic solvent to clean the surface of the substrate material and then removing the organic solvent. Specifically, the organic solvent includes ethanol or acetone.
[0024] Preferably, the steps include:
[0025] S1, placing the pre-treated substrate material in a CVD reaction chamber and evacuating the chamber, introducing argon gas after evacuating the chamber, and heating the reaction chamber to the deposition temperature;
[0026] S2, using argon as a carrier gas to transport the sublimated inorganic tantalum salt into the reaction chamber, and simultaneously using argon as a carrier gas to introduce alkane and hydrogen, controlling the flow rate of the inorganic tantalum salt carrier gas, the flow rate of the reaction gas carrier gas, the original flow rate of the alkane and the original flow rate of the hydrogen to be 3.8-4.2:3.8-4.2:2:1, and depositing a multi-layer tantalum carbide coating on the substrate material by real-time control of the gas flow ratio;
[0027] S3. After the deposition is completed, stop heating and gas supply, cool naturally, take out the product and clean it.
[0028] Chemical vapor deposition is a process involving a variety of chemical and physical reactions. The transport of gas flow in the chamber is controlled by gas flow, temperature and other corresponding means, and a series of reactions such as adsorption, migration, nucleation and growth of the atmosphere on the substrate surface are adjusted. Taking tantalum chloride as an inorganic tantalum salt and methane as an alkane as an example, the following reactions may occur in the reaction chamber:
[0029] CH4→C+2H2;
[0030] TaCl5+H2→Ta+TaCl4+HCl;
[0031] TaCl4+2H2→Ta+4HCl;
[0032] TaCl5+C→TaC+5Cl;
[0033] TaCl4+C→TaC+4Cl;
[0034] Ta+C→TaC;
[0035] Overall reaction formula: TaCl5+CH4+1 / 2H2=TaC+5HCl.
[0036] The chemical vapor deposition equipment includes an inorganic tantalum salt evaporation chamber and a reaction chamber. The carrier gas is passed into the tantalum salt evaporation chamber. Under heating conditions, the Ta source is passed into the reaction chamber in gaseous form together with the carrier gas. The C source is cracked in the reaction chamber and deposited on the substrate surface with the Ta source to form TaC. The residual gas is discharged through the tail gas treatment device along with the carrier gas.
[0037] In a second aspect, the present invention provides a product obtained by the method for preparing a multilayer tantalum carbide coating by the CVD method as described in the first aspect, characterized in that it includes a substrate material and a multilayer tantalum carbide coating deposited on the substrate material.
[0038] Preferably, the thickness of the tantalum carbide coating is 10 to 100 microns.
[0039] The beneficial effects achieved by one or more technical solutions of the present invention are as follows:
[0040] The present invention controls the gas flow ratio in real time, so that the reaction gas flow is passed into the reaction chamber in a sinusoidal cross wave manner to form a multi-layer staggered tantalum carbide coating structure. The obtained multi-layer tantalum carbide coating has a high purity, and its multi-layer structure can effectively prevent the extension of cracks to the base material, isolate the base material from the reaction chamber atmosphere, and play a better protective role. Compared with the single-layer tantalum carbide coating obtained by traditional CVD, the multi-layer structure is more likely to release the stress caused by the mismatched thermal expansion coefficient of the tantalum carbide coating and the base material, and has better bonding with the base material, reducing the probability of cracks. BRIEF DESCRIPTION OF THE DRAWINGS
[0041] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.
[0042] Figure 1 is a cross-sectional view of the multilayer tantalum carbide coating of Example 1;
[0043] Figure 2 This is a surface morphology image of the multilayer tantalum carbide coating of Example 1;
[0044] Figure 3 This is the surface morphology of the traditional CVD tantalum carbide coating of comparative example 1. DETAILED DESCRIPTION
[0045] In order to enable those skilled in the art to more clearly understand the technical solution of the present invention, the technical solution of the present invention will be described in detail below in combination with specific embodiments and comparative examples.
[0046] The inorganic tantalum salt used in the following examples is tantalum chloride.
[0047] Example 1
[0048] A high-purity graphite sheet was selected as the substrate material, and was placed in anhydrous ethanol for ultrasonic treatment for 5 minutes, then placed in deionized water for ultrasonic treatment for 5 minutes, and then dried by purging with nitrogen.
[0049] Place the pre-treated substrate material in the CVD reaction chamber, turn on the mechanical pump, pump the pressure in the chamber to below 10Pa, and turn on the molecular pump. When the pressure reaches a certain level, introduce argon as a carrier gas, pressurize to 100mbar, and then heat the reaction chamber to 1000℃.
[0050] The inorganic tantalum salt evaporation chamber is heated to 300°C and maintained for 30 minutes. The carrier gas argon flow rate is 1000sccm, and is transported to the reaction chamber. Methane and hydrogen are simultaneously introduced using argon as the carrier gas, wherein the argon flow rate of the inorganic tantalum salt carrier gas is gradually increased from 500sccm to 1000sccm within 1 hour, and then gradually decreased to 500sccm within 1 hour. The argon flow rate of the methane carrier gas is 1000sccm. The ethane flow rate is gradually decreased from 500sccm to 250sccm within 1 hour, and then gradually increased to 500sccm within 1 hour. The synchronous hydrogen flow rate is decreased from 250sccm to 125sccm within 1 hour, and then gradually increased to 250sccm within 1 hour. The process is repeated multiple times. A multi-layer stacked structure can be formed by adjusting the gas flow ratio in the chamber. A multi-layer tantalum carbide coating is obtained by depositing it on a high-purity graphite sheet for 10 hours.
[0051] Turn off the heating power supply and wait for the vapor deposition equipment to cool down; when the temperature drops below 50°C, turn on the vacuum pump to exhaust the gas in the reaction chamber into the tail gas treatment device until the vacuum degree is below 100 Pa, then turn off the vacuum pump and let in argon gas. After the pressure in the reaction chamber rises to normal pressure, open the reaction chamber and take out the prepared graphite sheet with multi-layer tantalum carbide coating.
[0052] The prepared multi-layer tantalum carbide coated graphite material was characterized using a scanning electron microscope. The test results showed that the coating cross section was formed by the dense accumulation of multiple layers of fine particles. Figure 1 and Figure 2 shown.
[0053] Comparative Example 1
[0054] A high-purity graphite sheet was selected as the substrate material, and was placed in anhydrous ethanol for ultrasonic treatment for 5 minutes, then placed in deionized water for ultrasonic treatment for 5 minutes, and then dried by purging with nitrogen.
[0055] Place the pre-treated substrate material in the CVD reaction chamber, turn on the mechanical pump, pump the pressure in the chamber to below 10Pa, and turn on the molecular pump. When the pressure reaches a certain level, introduce argon as a carrier gas, pressurize to 100mbar, and then heat the reaction chamber to 1000℃.
[0056] The inorganic tantalum salt evaporation chamber is heated to 300°C and maintained for 30 minutes. The carrier gas argon flow rate is 1000sccm, and it is transported to the reaction chamber. Methane and hydrogen are simultaneously introduced using argon as a carrier gas. The inorganic tantalum salt carrier gas argon flow rate is 1000sccm, the methane carrier gas argon flow rate is 1000sccm, the ethane gas flow rate is 500sccm, and the hydrogen flow rate is 250sccm. The tantalum carbide coating prepared by the traditional CVD method is obtained by depositing it on a high-purity graphite sheet for 10 hours.
[0057] Figure 3This is the surface morphology of the tantalum carbide coating prepared by the traditional CVD method in Comparative Example 1. It can be seen that there are obvious penetrating cracks in the coating, resulting in a relatively low coating life. Figure 1 This is a cross-sectional morphology of the multilayer tantalum carbide coating prepared in Example 1. It can be seen that small cracks appear inside the coating, but the cracks do not penetrate from the coating surface to the substrate material, thus playing an excellent protective role; Figure 2 This is a surface morphology picture of the multilayer tantalum carbide coating prepared in Example 1. It can be seen that the surface morphology of the coating is flat and smooth, no cracks are generated, it is not easy to absorb foreign impurities, and it is not easy to be corroded, thereby ensuring a long life of the coating.
[0058] Example 2
[0059] A high-purity graphite sheet was selected as the substrate material, and was placed in acetone for ultrasonic treatment for 5 minutes, then placed in deionized water for ultrasonic treatment for 5 minutes, and then dried by purging with nitrogen.
[0060] Place the pre-treated substrate material in the CVD reaction chamber, turn on the mechanical pump, pump the pressure in the chamber to below 10Pa, and turn on the molecular pump. When the pressure reaches a certain level, introduce argon as a carrier gas, pressurize to 100mbar, and then heat the reaction chamber to 1000℃.
[0061] The inorganic tantalum salt evaporation chamber is heated to 300°C and maintained for 30 minutes. The carrier gas argon flow rate is 500sccm, and is transported to the reaction chamber. Ethane and hydrogen are simultaneously introduced using argon as the carrier gas, wherein the argon flow rate of the inorganic tantalum salt carrier gas is gradually increased from 250sccm to 500sccm within 1 hour, and then gradually decreased to 250sccm within 1 hour. The argon flow rate of the ethane carrier gas is 500sccm. The ethane flow rate is gradually decreased from 250sccm to 125sccm within 1 hour, and then gradually increased to 250sccm within 1 hour. The synchronous hydrogen flow rate is decreased from 125sccm to 60sccm within 1 hour, and then gradually increased to 125sccm within 1 hour. The process is repeated multiple times. A multilayer stacked structure can be formed by adjusting the gas flow ratio in the chamber. A multilayer tantalum carbide coating is obtained by depositing it on a high-purity graphite sheet for 20 hours.
[0062] Turn off the heating power supply and wait for the vapor deposition equipment to cool down; when the temperature drops below 50°C, turn on the vacuum pump to exhaust the gas in the reaction chamber into the tail gas treatment device until the vacuum degree is below 100 Pa, then turn off the vacuum pump and let in argon gas. After the pressure in the reaction chamber rises to normal pressure, open the reaction chamber and take out the prepared graphite sheet with multi-layer tantalum carbide coating.
[0063] Example 3
[0064] A high-purity graphite sheet was selected as the substrate material, and was placed in acetone for ultrasonic treatment for 5 minutes, then placed in deionized water for ultrasonic treatment for 5 minutes, and then dried by purging with nitrogen.
[0065] Place the pre-treated substrate material in the CVD reaction chamber, turn on the mechanical pump, pump the pressure in the chamber to below 10Pa, and turn on the molecular pump. When the pressure reaches a certain level, introduce argon as a carrier gas, pressurize it to 100mbar, and then heat the reaction chamber to 1800℃.
[0066] The inorganic tantalum salt evaporation chamber is heated to 800°C and maintained for 30 minutes. The carrier gas argon flow rate is 500sccm, and is transported to the reaction chamber. Ethane and hydrogen are simultaneously introduced using argon as the carrier gas, wherein the argon flow rate of the inorganic tantalum salt carrier gas is gradually increased from 250sccm to 500sccm within 1 hour, and then gradually decreased to 250sccm within 1 hour. The argon flow rate of the ethane carrier gas is 500sccm. The ethane flow rate is gradually decreased from 250sccm to 125sccm within 1 hour, and then gradually increased to 250sccm within 1 hour. The synchronous hydrogen flow rate is decreased from 125sccm to 65sccm within 1 hour, and then gradually increased to 125sccm within 1 hour. The process is repeated multiple times. A multilayer stacking structure can be formed by adjusting the gas flow ratio in the chamber, and a multilayer tantalum carbide coating is obtained by depositing it on a high-purity graphite sheet for 10 hours.
[0067] Turn off the heating power supply and wait for the vapor deposition equipment to cool down; when the temperature drops below 50°C, turn on the vacuum pump to exhaust the gas in the reaction chamber into the tail gas treatment device until the vacuum degree is below 100 Pa, then turn off the vacuum pump and let in argon gas. After the pressure in the reaction chamber rises to normal pressure, open the reaction chamber and take out the prepared graphite sheet with multi-layer tantalum carbide coating.
[0068] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.
Claims
1. A method for preparing a multilayer tantalum carbide coating by CVD, characterized in that: In the process of preparing tantalum carbide coating on the surface of substrate material by CVD method using tantalum salt and reaction gas as raw materials, the reaction gas flow is introduced in a sinusoidal cross-wave manner by real-time control of the gas flow ratio, thereby forming a multi-layer tantalum carbide coating; Wherein, the reaction gas includes alkane and hydrogen, and the real-time control of the gas flow ratio is to introduce tantalum salt carrier gas, alkane and hydrogen through a circulation control method under the condition that the reaction gas carrier gas flow remains unchanged. A cycle process of the tantalum salt carrier gas control method is: within a set time, the tantalum salt carrier gas flow rate first increases from 45-55% of the original flow rate to the original flow rate of the tantalum salt carrier gas, and then decreases to 45%-55% of the original flow rate of the tantalum salt carrier gas; a cycle process of the alkane gas flow control method is: within a set time, the alkane flow rate first decreases to 45-55% of the original alkane flow rate, and then increases to the original alkane flow rate; a cycle process of the hydrogen gas flow control method is: within a set time, the hydrogen flow rate first decreases to 45-55% of the original hydrogen flow rate, and then increases to the original hydrogen flow rate; the ratio of the tantalum salt carrier gas, the original alkane flow rate and the original hydrogen flow rate is 3.8-4.2:1.9-2.1:
1.
2. The method for preparing a multilayer tantalum carbide coating by CVD method according to claim 1, characterized in that: The tantalum salt is heated to sublime, and then transported through a tantalum salt carrier gas to react with the reaction gas to achieve chemical vapor deposition; or, the temperature at which the tantalum salt is heated to sublime is 180-800°C; or, the flow rate of the tantalum salt carrier gas is 500-2000 sccm; or, the tantalum salt carrier gas is argon.
3. The method for preparing a multilayer tantalum carbide coating by CVD method according to claim 1, characterized in that: The alkane is at least one of methane, ethane and propane; Or, the flow rate of alkane is 50~500 sccm; Alternatively, the flow rate of hydrogen is 25 to 250 sccm.
4. The method for preparing a multilayer tantalum carbide coating by CVD method according to claim 1, characterized in that: The reaction gas is delivered via a reaction gas carrier gas; Alternatively, the flow rate of the reaction gas is 500~2000 sccm.
5. The method for preparing a multilayer tantalum carbide coating by CVD method according to claim 1, characterized in that: The ratio of the flow rate of the tantalum salt carrier gas, the flow rate of the reaction gas carrier gas, the original flow rate of the alkane and the original flow rate of the hydrogen is 3.8~4.2:3.8~4.2:1.9~2.1:1, or 3.8~4.2:3.8~4.2:2:
1.
6. The method for preparing a multilayer tantalum carbide coating by CVD method according to claim 1, characterized in that: The CVD deposition temperature is 1000~1800 ℃; or, the heating rate to the deposition temperature is 5~15 ℃ / min; or, the deposition time is 10~20 h.
7. The method for preparing a multilayer tantalum carbide coating by CVD method according to claim 1, characterized in that: During one cycle of the alkane gas flow control mode, the set time is 1.8 to 2.2 hours; Or, in one cycle of the alkane gas flow control mode, in the first half of the set time, the alkane flow rate increases from the original alkane flow rate to 45-55% of the original alkane flow rate; in the second half of the set time, the alkane flow rate increases from 45-55% of the original alkane flow rate to the original alkane flow rate; Or, in one cycle of the tantalum salt carrier gas control method, the set time is 1.8 to 2.2 hours; Or, in one cycle of the tantalum salt carrier gas control mode, in the first half of the set time, the tantalum salt carrier gas flow rate increases from 45% to 55% of the original tantalum salt carrier gas flow rate to the original tantalum salt carrier gas flow rate; in the second half of the set time, the tantalum salt carrier gas flow rate decreases from the original tantalum salt carrier gas flow rate to 45% to 55% of the original tantalum salt carrier gas flow rate; Or, in one cycle of the hydrogen gas flow control method, the set time is 1.8 to 2.2 hours; Alternatively, during one cycle of the hydrogen gas flow control method, in the first half of the set time, the hydrogen flow rate increases from the original hydrogen flow rate to 45-55% of the original hydrogen flow rate; in the second half of the set time, the hydrogen flow rate increases from 45-55% of the original hydrogen flow rate to the original hydrogen flow rate.
8. The method for preparing a multilayer tantalum carbide coating by CVD method according to claim 1, characterized in that: The following steps are involved: S1, placing the pre-treated substrate material in a CVD reaction chamber and evacuating the chamber, introducing argon gas after evacuating the chamber, and heating the reaction chamber to the deposition temperature; S2, using argon as a carrier gas to transport the sublimated inorganic tantalum salt into the reaction chamber, and simultaneously using argon as a carrier gas to introduce alkane and hydrogen, controlling the flow rate of the inorganic tantalum salt carrier gas, the flow rate of the reaction gas carrier gas, the original flow rate of the alkane and the original flow rate of the hydrogen to be 3.8-4.2:3.8-4.2:2:1, and depositing a multi-layer tantalum carbide coating on the substrate material by real-time control of the gas flow ratio; S3. After the deposition is completed, stop heating and gas supply, cool naturally, take out the product and clean it.
9. A product obtained by the method for preparing a multilayer tantalum carbide coating by a CVD method according to any one of claims 1 to 8, comprising a substrate material and a multilayer tantalum carbide coating deposited on the substrate material.
10. The product according to claim 9, characterized in that The thickness of tantalum carbide coating is 10~100 microns.
Citation Information
Patent Citations
Anti-ablation ZrC / SiC multilayer alternate coating and preparation method thereof
CN113106416A
Graphite plate with TaC composite coating and preparation method thereof
CN115725960A
Method for preparing tantalum carbide coating by CVD (chemical vapor deposition) and product thereof
CN115786876A
Method for preparing tantalum carbide coating by CVD (chemical vapor deposition) method
CN115948721A
Light-emitting diode epitaxial wafer, preparation method thereof and light-emitting diode
CN116435423A