A multi-layer resin composite electric heating lightweight floor and preparation method thereof

By using a composite material of modified boron nitride and three-dimensional carbon skeleton graphene in the electric heating floor to form an efficient electrical and thermal conduction network, and using silicon oxide and aluminum oxide in the heat insulation layer, the low heat transfer efficiency and insufficient heat generation are solved. Uniform problem, achieving safe and efficient electric heating effect.

CN118181902BActive Publication Date: 2024-10-15HEBEI MAIDONG PLASTIC FLOORING CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410280536.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-12
Publication Date
2024-10-15
Estimated Expiration
2044-03-12

AI Technical Summary

Technical Problem

Existing electric heating floors have low heat transfer efficiency and uneven heating, which can easily lead to excessive local temperatures and fire risks. In addition, the agglomeration of graphene in the polymer causes the electrical and thermal conductive network to be blocked and the heat transfer efficiency to decrease.

Method used

A multi-layer resin composite electrically heated lightweight floor is used. Modified boron nitride is added to the wear-resistant layer and pressure-resistant layer, and graphene with a three-dimensional carbon skeleton structure is used to form an efficient and connected electrical and thermal conductive network, and is used in heat insulation. Silicon oxide and aluminum oxide are used in the layers to prevent heat loss.

Benefits of technology

It improves the thermal conductivity efficiency and heating uniformity of the floor, enhances the electric-heat conversion efficiency, reduces heat loss, and ensures safety and efficient heating performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118181902B_ABST
    Figure CN118181902B_ABST
Patent Text Reader

Abstract

The present invention discloses a multi-layer resin composite electric heating lightweight floor and a preparation method thereof in the technical field of composite flooring. The composite electric heating lightweight flooring comprises the following parts from top to bottom: a wear-resistant layer, a pressure-resistant layer, an electric heating film, and a heat-insulating layer. The present invention forms a lightweight composite flooring by compounding multiple functional materials to improve the comprehensive performance of the composite flooring, adds modified boron nitride to the wear-resistant layer and the pressure-resistant layer to improve the thermal conductivity, forms a highly efficient and interconnected conductive and thermal network in a polymer matrix with a graphene composite material supported by a three-dimensional carbon skeleton structure, and uses silicon dioxide and aluminum oxide as heat-insulating materials to prevent heat from being lost to the ground.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of composite floors, and specifically refers to a multi-layer resin composite electric heating lightweight floor and a preparation method thereof. Background Art

[0002] Compared with other heating facilities such as radiant heating, floor radiant heating facilities are environmentally friendly, clean, highly thermally efficient, and space-saving. Under many specific conditions, floor radiant heating is also more flexible and can adapt to a variety of environments, such as tents, subways, high-speed railways and other mobile locations; the assembled electric heating floor is simple to process and has a high thermal energy utilization rate. Common electric heating floors often add a layer of resistance wire with heating function between the layers of the composite floor to convert electrical energy into thermal energy, but this method is less safe and can easily cause the temperature in some local areas to be too high and the heat to be uneven, which may even cause Fire; Composite floor panels are made of wood materials with low thermal conductivity and slow floor heating rate; In the prior art, graphene is usually used as the heating material for electric heating floors. Graphene is a two-dimensional nanomaterial composed of hybrid carbon atoms with high electrical conductivity and high thermal conductivity, which exceeds that of carbon nanotubes and diamonds of the same carbon material. Graphene often forms thermally conductive composite materials with polymers. The flat layer structure of graphene can provide multi-channel phonon transmission, but graphene is easy to agglomerate in polymers due to its small particle size, resulting in the blocking of the conductive and thermal network, reduced heat transfer efficiency and uneven heating. Summary of the invention

[0003] In view of the above situation, in order to overcome the defects of the prior art, the present invention provides a multi-layer resin composite electric heating lightweight floor and a preparation method thereof. In order to solve the problems of reduced heat transfer efficiency and uneven heating, a multi-layer functional material is composited to form a lightweight floor to improve the comprehensive performance of the composite floor. Modified boron nitride is added to the wear-resistant layer and the pressure-resistant layer to improve the thermal conductivity. A graphene composite material supported by a three-dimensional carbon skeleton structure is used to form an efficient and interconnected conductive and thermal conductive network in the polymer matrix. Silica and alumina are used as thermal insulation materials to prevent heat from dissipating to the ground.

[0004] In order to achieve the above-mentioned purpose, the technical solution adopted by the present invention is as follows: The present invention proposes a multi-layer resin composite electric heating lightweight floor, the composite electric heating lightweight floor comprises the following parts from top to bottom: a wear-resistant layer, a pressure-resistant layer, an electric heating film, and a heat insulation layer;

[0005] Preferably, the wear-resistant layer has a thickness of 0.2-0.5 mm; the pressure-resistant layer has a thickness of 1-2 mm; the electric heating film has a thickness of 0.5-1 mm; and the heat-insulating layer has a thickness of 3-5 mm.

[0006] Preferably, the wear-resistant layer comprises the following components in parts by weight: 90-120 parts of polyphenylene sulfide resin, 20-30 parts of polytetrafluoroethylene resin, 10-20 parts of polyvinylidene fluoride resin, 20-30 parts of modified boron nitride, 10-20 parts of glass fiber, 10-20 parts of wear-resistant filler, and 0.1-0.5 parts of 1076 antioxidant;

[0007] Preferably, the method for preparing the wear-resistant layer specifically comprises the following steps:

[0008] ① Place boron nitride nanosheets in deionized water to obtain a boron nitride nanosheet dispersion, adjust the pH to 9.0-9.5, add octadecyltrimethylammonium bromide, and reflux at 80-90° C. for 5-7 hours, filter, wash the solid with deionized water, and vacuum dry at 70-80° C. for 20-30 hours to obtain modified boron nitride;

[0009] ② Activate titanium diboride in a sodium hydroxide solution at an activation temperature of 100-120°C for 2-3 hours, filter, transfer the solid to a perfluorodecyltriethoxysilane solution, perform ultrasonic treatment at 400-500W for 1-2 hours, add zirconium oxide grinding balls for grinding, wash the grinding balls with anhydrous ethanol after 1-2 hours, remove excess solvent, and dry to obtain a wear-resistant filler;

[0010] ③ Evenly mix polyphenylene sulfide resin, polytetrafluoroethylene resin and polyvinylidene fluoride resin, heat to a molten state, stir on a stirrer at a speed of 100-120 rpm for 1 hour, add 1076 antioxidant, and continue stirring for 30-40 minutes to obtain a matrix material;

[0011] ④ Add the modified boron nitride and glass fiber prepared in step ① and the wear-resistant filler prepared in step ② to the base material prepared in step ③, melt-extrude at an extrusion temperature of 250-270°C, and transfer to a blow molding machine for blow molding to obtain a wear-resistant layer.

[0012] Preferably, in step ①, the mass concentration of boron nitride nanosheets in the boron nitride nanosheet dispersion is 50-60 g / L;

[0013] Preferably, in step ①, the amount of octadecyltrimethylammonium bromide added is 0.3-0.5% of the mass of the boron nitride nanosheets;

[0014] Preferably, in step ②, the mass fraction of sodium hydroxide in the sodium hydroxide solution is 40-50%;

[0015] Preferably, in step ②, the mass concentration of titanium diboride in the sodium hydroxide solution is 0.1-0.15 g / mL;

[0016] Preferably, in step ②, the perfluorodecyltriethoxysilane solution is a solution of perfluorodecyltriethoxysilane in anhydrous ethanol, and the mass concentration of the perfluorodecyltriethoxysilane solution is 20-30 g / L;

[0017] Preferably, in step ②, the mass ratio of perfluorodecyltriethoxysilane to titanium diboride is 1:10-20;

[0018] Preferably, the pressure-resistant layer comprises the following components in parts by weight: 40-50 parts of polyethylene resin, 20-30 parts of polyurethane elastomer, 20-30 parts of modified boron nitride, 5-8 parts of maleic anhydride grafted polyvinyl acetate, 3-6 parts of oxazoline crosslinking agent, 1-3 parts of 1076 antioxidant, 1-3 parts of calcium stearate, and 0.5-1 parts of antioxidant 264;

[0019] Preferably, the modified boron nitride in the pressure-resistant layer and the modified boron nitride in the wear-resistant layer are prepared by the same method;

[0020] Preferably, the raw materials of the electric heating film specifically include the following components in parts by weight: 50-60 parts of cellulose, 5-10 parts of graphene oxide, 2-3 parts of carbonate, and 45-56 parts of polyvinylidene fluoride;

[0021] Preferably, the carbonate comprises at least one of sodium carbonate, calcium carbonate and sodium bicarbonate;

[0022] Preferably, the method for preparing the electric heating film specifically comprises the following steps:

[0023] S1. Mix and disperse cellulose and carbonate in deionized water, add graphene oxide, perform ultrasonic treatment at 300-450W for 30min, filter, and completely dry the solid under ventilation conditions to obtain a graphene foaming precursor;

[0024] S2, preheating the tube furnace to 300-400° C., transferring the graphene foaming precursor prepared in step S1 to a quartz boat, placing it in the tube furnace, performing a heat treatment for 1-3 min, and repeatedly washing with a 1 mol / L hydrochloric acid solution to remove excess carbonate, thereby obtaining a graphene oxide / cellulose composite;

[0025] S3, pyrolyzing the graphene oxide / cellulose composite prepared in step S2 in a tube furnace, heating at 10°C / min in a nitrogen atmosphere, heating to 600-800°C, keeping the temperature for 1-1.5h, and naturally cooling to room temperature to obtain three-dimensional carbon skeleton graphene;

[0026] S4, dispersing the three-dimensional carbon skeleton graphene prepared in step S3 in DMAC, ultrasonically treating at 400-500W for 1-2h, adding PVDF solution, placing on a magnetic stirrer and stirring at 200-300rpm for 4-6h to obtain an electric heating film precursor solution;

[0027] S5, placing the electric heating film precursor solution prepared in step S4 in an oven, and drying it at 80-100° C. under vacuum conditions, and obtaining an electric heating film after 12-15 hours;

[0028] Preferably, in step S1, the mass fraction of cellulose in deionized water is 5-10%;

[0029] Preferably, in step S4, the mass concentration of the three-dimensional carbon skeleton graphene in DMAC is 10-15 g / L;

[0030] Preferably, in step S4, the PVDF solution is PVDF dissolved in DMAC, and the mass concentration of PVDF in DMAC is 20-30 g / L.

[0031] Preferably, the thermal insulation layer comprises the following components in parts by weight: 10-20 parts of composite thermal insulation filler, 70-80 parts of polytetrafluoroethylene, and 5-10 parts of glass fiber;

[0032] Preferably, the preparation method of the thermal insulation layer specifically includes the following components:

[0033] A. reacting polymethyl hydrogen siloxane and an organic alcohol aluminum compound at a reaction temperature of 250-300° C. for a reaction time of 5-8 hours to obtain a gel precursor;

[0034] B. The gel precursor prepared in step A is subjected to pyrolysis reaction under oxygen conditions at a pyrolysis temperature of 700-800° C. for 2-3 hours. After the reaction system is naturally cooled to room temperature, it is ground through a 100-mesh sieve to obtain a composite thermal insulation filler;

[0035] C. Disperse the composite thermal insulation filler and polytetrafluoroethylene powder prepared in step B in anhydrous ethanol, mix, add glass fiber, stir at 1000-1200 rpm for 2-3 hours in a high-speed stirrer, and dry to obtain a preformed powder;

[0036] D. The preformed powder prepared in step C is placed in a press for compression molding, and after demoulding, is placed in a high-temperature furnace for high-temperature treatment, the temperature is increased to 340-360° C. at 2° C. / min, and the temperature is kept for 2-4 hours, and then naturally cooled to room temperature to obtain a heat insulation layer;

[0037] Preferably, in step A, the mass ratio between the polymethylhydrogensiloxane and the organic alcohol aluminum compound is 5-20:1.

[0038] The present invention also provides a multi-layer resin composite electrically heated lightweight floor, which specifically comprises the following steps: the composite electrically heated lightweight floor is formed by gluing a wear-resistant layer, a pressure-resistant layer, an electric heating film and an insulating layer with high-temperature resistant polyurethane or epoxy structural adhesive.

[0039] The beneficial effects achieved by the present invention are as follows:

[0040] The present invention provides a multi-layer resin composite electric heating lightweight floor and a preparation method thereof. The multi-layer functional materials are composited to form a lightweight composite floor, thereby improving the comprehensive performance of the composite floor. In the wear-resistant layer of the composite electric heating lightweight floor of the present invention, the wear-resistant filler is modified by titanium diboride through a silane reagent, thereby increasing the dispersibility of titanium diboride in the wear-resistant layer polymer system, and at the same time, the wear-resistant filler has a high hydrophobic group, thereby increasing the hydrophobicity in the wear-resistant layer polymer system and improving the wear resistance. The wear-resistant layer and the pressure-resistant layer both contain modified boron nitride, and the boron nitride is modified through a surfactant, thereby increasing the dispersibility of boron nitride in the polymer matrix, thereby facilitating the connection of the heat-conducting network, thereby increasing the heat transfer capacity of the wear-resistant layer and the pressure-resistant layer, reducing the heat loss inside the floor, and improving the heating efficiency of the floor. The electric heating layer uses PVDF as a polymer matrix, uses cellulose as a three-dimensional carbon skeleton template, and loads graphene to form a complex conductive and conductive structure. Thermal network, enhances the electric heat conversion efficiency of the electric heating film, after cellulose and sodium carbonate are mixed, graphene oxide is added, because the surface groups of graphene oxide are active, they can form hydrogen bonds with the hydroxyl groups on the cellulose molecular groups, thereby improving the dispersion performance of graphene oxide, after heating, sodium carbonate decomposes to produce H2O and CO2, causing the cellulose to expand to form a three-dimensional structure, and graphene oxide can be evenly loaded on the three-dimensional structure, after high-temperature pyrolysis, the surface groups of graphene oxide decompose and reduce to graphene, and a three-dimensional carbon skeleton of cellulose is formed, which is compounded with PVDF to form an electric heating film with high-efficiency electric heat conversion capability; the multi-layer resin composite electric heating lightweight floor insulation layer of the present invention has a composite insulation filler, polymethyl hydrogen siloxane and organic alcohol aluminum undergo thermal polymerization reaction to form polyaluminum siloxane, and after high-temperature pyrolysis, silicon oxide and aluminum oxide doped insulation fillers are formed, which can prevent heat loss and improve insulation capability. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 This is a schematic diagram of the structure of the multi-layer resin composite electric heating lightweight floor prepared in Example 1;

[0042] Figure 2 This is a SEM electron microscope scanning image of the three-dimensional carbon skeleton graphene prepared in Example 1;

[0043] Figure 3This is a graph showing the surface temperature rise results of the multi-layer resin composite electrically heated lightweight floor prepared in Examples 1-3 and Comparative Examples 1-3;

[0044] Figure 4 This is a graph showing the electric-thermal radiation conversion efficiency of the multi-layer resin composite electrically heated lightweight floor prepared in Examples 1-3 and Comparative Examples 1-3.

[0045] The accompanying drawings are used to provide further understanding of the present invention and constitute a part of the specification. They are used to explain the present invention together with the embodiments of the present invention and do not constitute a limitation of the present invention. DETAILED DESCRIPTION

[0046] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments; based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.

[0047] Unless otherwise defined, all professional and scientific terms used herein have the same meanings as those familiar to those skilled in the art. In addition, any methods and materials similar or equivalent to those described herein may be applied to the present invention. The preferred implementation methods and materials described herein are for demonstration purposes only and are not intended to limit the content of this application.

[0048] The experimental methods in the following examples are conventional methods unless otherwise specified; the experimental materials and test strains used in the following examples are purchased from commercial channels unless otherwise specified.

[0049] Polymethyl hydrogen siloxane (CasNo: 63148-57-2), model: V202-035, purchased from Foshan Huagu Silicone Co., Ltd., hydrogen content 0.33%-0.37%, kinematic viscosity 100-110 (25℃, mm 2 / s).

[0050] Example 1

[0051] This embodiment provides a multi-layer resin composite electric heating lightweight floor, the composite electric heating lightweight floor comprises from top to bottom:

[0052] Wear-resistant layer with a thickness of 0.2mm, pressure-resistant layer with a thickness of 1.5mm, electric heating film with a thickness of 0.5mm, and thermal insulation layer with a thickness of 4mm;

[0053] The structural schematic diagram of the multi-layer resin composite electric heating lightweight floor prepared in this embodiment is as follows: Figure 1As shown, in the figure, 1 is a wear-resistant layer, 2 is a pressure-resistant layer, 3 is an electric heating film, and 4 is a heat-insulating layer.

[0054] The wear-resistant layer includes the following components in parts by weight: 90 parts of polyphenylene sulfide resin, 20 parts of polytetrafluoroethylene resin, 20 parts of polyvinylidene fluoride resin, 20 parts of modified boron nitride, 10 parts of glass fiber, 10 parts of wear-resistant filler, and 0.1 parts of 1076 antioxidant;

[0055] The preparation method of the wear-resistant layer specifically comprises the following steps:

[0056] ① Place 25 g of boron nitride nanosheets in a three-necked flask, add 500 mL of deionized water, stir evenly, adjust the pH to 9.0, add 75 mg of octadecyltrimethylammonium bromide, reflux at 80 ° C for 7 h, remove the filtrate by suction, wash the solid with deionized water, place in a vacuum drying oven, and dry at 70 ° C for 30 h to obtain modified boron nitride;

[0057] ② Prepare a sodium hydroxide solution with a mass fraction of 40%, take 150mL of the sodium hydroxide solution and place it in a flask, add 15g of titanium diboride, and heat the reaction at 100°C for 3h. After the reaction system is naturally cooled to room temperature, filter and remove the filtrate; take 1.5g of perfluorodecyltriethoxysilane and dissolve it in 50mL of deionized water to obtain a perfluorodecyltriethoxysilane solution, transfer the filtered solid to the perfluorodecyltriethoxysilane solution, ultrasonically treat it at 400W for 2h, add 15g of zirconium oxide grinding balls for ball milling, and after 2h, wash the reactants on the grinding balls with anhydrous ethanol, combine the reactants, and dry them to obtain wear-resistant fillers;

[0058] ③ 90 g of polyphenylene sulfide resin, 20 g of polytetrafluoroethylene resin and 20 g of polyvinylidene fluoride resin were mixed evenly, heated to a molten state, stirred on a stirrer at a speed of 100 rpm for 1 hour, 0.1 g of 1076 antioxidant was added, and stirring was continued for 40 minutes to obtain a matrix material;

[0059] ④ Add 20g of modified boron nitride prepared in step ①, 10g of glass fiber and 10g of wear-resistant filler prepared in step ② to the base material prepared in step ③, melt-extrude at an extrusion temperature of 270°C, and then transfer to a blow molding machine for blow molding to obtain a wear-resistant layer.

[0060] The pressure-resistant layer includes the following components in parts by weight: 40 parts of polyethylene resin, 30 parts of polyurethane elastomer, 20 parts of modified boron nitride, 8 parts of maleic anhydride grafted polyvinyl acetate, 6 parts of oxazoline crosslinking agent, 3 parts of 1076 antioxidant, 1 part of calcium stearate, and 0.5 parts of antioxidant 264;

[0061] The method for preparing the pressure-resistant layer specifically comprises the following steps:

[0062] Polyethylene resin, polyurethane elastomer, and oxazoline crosslinking agent are mixed, stirred at 100°C for 5 minutes, modified boron nitride is added, stirred for 30 minutes, maleic anhydride grafted polyvinyl acetate, 1076 antioxidant, calcium stearate, and antioxidant 264 are added, and mixed in a high-speed mixer for 30 minutes at a mixing temperature of 130°C. The extrusion temperature is 170°C and the screw speed is 50rpm. After extrusion, it is calendered into a film to obtain a pressure-resistant layer.

[0063] The raw materials of the electric heating film specifically include the following components in parts by weight: 50 parts of cellulose, 5 parts of graphene oxide, 2 parts of sodium carbonate, and 56 parts of polyvinylidene fluoride;

[0064] The preparation method of the electric heating film specifically comprises the following steps:

[0065] S1. Place 10 g of cellulose and 0.4 g of sodium carbonate in a flask, add 200 mL of deionized water, stir to disperse the system evenly, add 1 g of graphene oxide, place it under 300 W for ultrasonic treatment for 30 min, filter, remove the filtrate, dry the filtered solid under ventilation conditions, and obtain a graphene foaming precursor after complete drying;

[0066] S2, preheating the tube furnace to 300° C., transferring the graphene foaming precursor prepared in step S1 into a quartz boat, placing it in the tube furnace, and performing heat treatment for 3 min. Immediately after the heat treatment, the mixture is repeatedly washed with a 1 mol / L hydrochloric acid solution to remove sodium carbonate, thereby obtaining a graphene oxide / cellulose composite;

[0067] S3, pyrolyzing the graphene oxide / cellulose composite prepared in step S2 in a tube furnace, heating to 600° C. at 10° C. / min in a nitrogen atmosphere, keeping the temperature for 1.5 h, and then naturally cooling to room temperature to obtain a three-dimensional carbon skeleton graphene;

[0068] Figure 2 This is a SEM electron microscope scanning image of the three-dimensional carbon skeleton graphene prepared in this embodiment, with a magnification of 1000 times. From the image, an obvious carbon skeleton structure can be seen, and the joints have obvious graphene structures.

[0069] S4, the three-dimensional carbon skeleton graphene prepared in step S3 was transferred to a flask, 280 mL of DMAC was added, and ultrasonic treatment was performed at 400 W for 2 h. After uniform dispersion, a three-dimensional carbon skeleton graphene dispersion was obtained, 11.2 g of PVDF was placed in 560 mL of DMAC and mixed, and then added to the three-dimensional carbon skeleton graphene dispersion, and placed on a magnetic stirrer, and stirred at 200 rpm for 6 h to obtain an electric heating film precursor solution;

[0070] S5. Transfer the electric heating film precursor solution prepared in step S4 to a mold, dry it in an oven at 80° C. under vacuum conditions, and demold it after 15 hours to obtain an electric heating film.

[0071] The heat insulation layer includes the following components in parts by weight: 20 parts of composite heat insulation filler, 80 parts of polytetrafluoroethylene, and 10 parts of glass fiber;

[0072] The preparation method of the thermal insulation layer specifically comprises the following steps:

[0073] A. Add 20 g of polymethylhydrogensiloxane to 40 mL of tetrahydrofuran for dilution, add 4 g of aluminum isopropoxide and mix, react at 250° C. for 8 h, remove tetrahydrofuran, and obtain a gel precursor;

[0074] B. The gel precursor prepared in step A is subjected to pyrolysis reaction under oxygen conditions at a pyrolysis temperature of 800° C. for 3 h. After the reaction, the system is naturally cooled to room temperature and then ground through a 100-mesh sieve to obtain a composite thermal insulation filler;

[0075] C. Disperse 20 g of the composite thermal insulation filler prepared in step B and 80 g of polytetrafluoroethylene powder in anhydrous ethanol, mix, add 10 g of glass fiber, place in a high-speed stirrer at 1000 rpm for 3 h, and dry to obtain a preformed powder;

[0076] D. The preformed powder prepared in step C is placed in a press to form the powder. After demolding, the powder is placed in a high-temperature furnace and heated to 350° C. at a rate of 2° C. / min. After being kept at this temperature for 3 hours, the powder is naturally cooled to room temperature to obtain a heat-insulating layer.

[0077] The present embodiment also provides a method for preparing a multi-layer resin composite electrically heated lightweight floor, which specifically includes the following steps: the composite electrically heated lightweight floor is glued together with a wear-resistant layer, a pressure-resistant layer, an electric heating film and an insulating layer using high-temperature resistant polyurethane or epoxy structural adhesive, pressed into shape, and cut into the composite electrically heated lightweight floor.

[0078] Example 2

[0079] This embodiment provides a multi-layer resin composite electric heating lightweight floor, which comprises from top to bottom:

[0080] Wear-resistant layer with a thickness of 0.5mm, pressure-resistant layer with a thickness of 1mm, electric heating film with a thickness of 0.8mm, and thermal insulation layer with a thickness of 3mm;

[0081] The wear-resistant layer includes the following components in parts by weight: 120 parts of polyphenylene sulfide resin, 30 parts of polytetrafluoroethylene resin, 10 parts of polyvinylidene fluoride resin, 30 parts of modified boron nitride, 20 parts of glass fiber, 20 parts of wear-resistant filler, and 0.5 parts of 1076 antioxidant;

[0082] The preparation method of the wear-resistant layer specifically comprises the following steps:

[0083] ① Place 30 g of boron nitride nanosheets in a three-necked flask, add 500 mL of deionized water, stir evenly, adjust the pH to 9.5, add 1.5 g of octadecyltrimethylammonium bromide, reflux at 90 ° C for 5 h, remove the filtrate by suction, wash the solid with deionized water, place in a vacuum drying oven, and dry at 80 ° C for 25 h to obtain modified boron nitride;

[0084] ② Prepare a sodium hydroxide solution with a mass fraction of 50%, take 100 mL of the sodium hydroxide solution and place it in a flask, add 15 g of titanium diboride, and heat the reaction at 120°C for 2 hours. After the reaction system is naturally cooled to room temperature, filter and remove the filtrate; take 1 g of perfluorodecyltriethoxysilane and dissolve it in 50 mL of deionized water to obtain a perfluorodecyltriethoxysilane solution, transfer the filtered solid to the perfluorodecyltriethoxysilane solution, ultrasonically treat it at 500W for 1 hour, add 15 g of zirconium oxide grinding balls for ball milling, and after 1 hour, wash the reactants on the grinding balls with anhydrous ethanol, combine the reactants, and dry them to obtain wear-resistant fillers;

[0085] ③ Evenly mix 120 g of polyphenylene sulfide resin, 30 g of polytetrafluoroethylene resin and 10 g of polyvinylidene fluoride resin, heat to a molten state, stir on a stirrer at 120 rpm for 1 hour, add 0.5 g of 1076 antioxidant, and continue stirring for 30 minutes to obtain a matrix material;

[0086] ④ Add 30 g of modified boron nitride prepared in step ①, 20 g of glass fiber and 20 g of wear-resistant filler prepared in step ② to the base material prepared in step ③, melt-extrude at an extrusion temperature of 260°C, and then transfer to a blow molding machine for blow molding to obtain a wear-resistant layer.

[0087] The pressure-resistant layer includes the following components in parts by weight: 50 parts of polyethylene resin, 20 parts of polyurethane elastomer, 30 parts of modified boron nitride, 5 parts of maleic anhydride grafted polyvinyl acetate, 3 parts of oxazoline crosslinking agent, 1 part of 1076 antioxidant, 3 parts of calcium stearate, and 1 part of antioxidant 264;

[0088] The method for preparing the pressure-resistant layer is the same as that in Example 1.

[0089] The raw materials of the electric heating film specifically include the following components in parts by weight: 60 parts of cellulose, 6 parts of graphene oxide, 3 parts of sodium carbonate, and 45 parts of polyvinylidene fluoride;

[0090] The preparation method of the electric heating film specifically comprises the following steps:

[0091] S1. Place 20 g of cellulose and 1 g of sodium carbonate in a flask, add 200 mL of deionized water, stir to disperse the system evenly, add 2 g of graphene oxide, place under 450 W for ultrasonic treatment for 30 min, filter, remove the filtrate, dry the filtered solid under ventilation conditions, and obtain a graphene foaming precursor after complete drying;

[0092] S2, preheating the tube furnace to 400° C., transferring the graphene foaming precursor prepared in step S1 into a quartz boat, placing it in the tube furnace, and performing heat treatment for 1 min. Immediately after the heat treatment, the mixture is repeatedly washed with a 1 mol / L hydrochloric acid solution to remove sodium carbonate, thereby obtaining a graphene oxide / cellulose composite;

[0093] S3, pyrolyzing the graphene oxide / cellulose composite prepared in step S2 in a tube furnace, heating to 800° C. at 10° C. / min in a nitrogen atmosphere, keeping the temperature for 1 hour, and then naturally cooling to room temperature to obtain a three-dimensional carbon skeleton graphene;

[0094] S4, 3.772 g of the three-dimensional carbon skeleton graphene prepared in step S3 was transferred to a flask, 250 mL of DMAC was added, and ultrasonic treatment was performed at 500 W for 1 h. After uniform dispersion, a three-dimensional carbon skeleton graphene dispersion was obtained, 15 g of PVDF was placed in 500 mL of DMAC and mixed, and then added to the three-dimensional carbon skeleton graphene dispersion, and placed on a magnetic stirrer, and stirred at 300 rpm for 4 h to obtain an electric heating film precursor solution;

[0095] S5. Transfer the electric heating film precursor solution prepared in step S4 to a mold, dry it in an oven under vacuum at 100° C., and demold it after 12 hours to obtain an electric heating film.

[0096] The heat insulation layer comprises the following components in parts by weight: 10 parts of composite heat insulation filler, 70 parts of polytetrafluoroethylene, and 5 parts of glass fiber;

[0097] The preparation method of the thermal insulation layer specifically comprises the following steps:

[0098] A. Add 20 g of polymethylhydrogensiloxane to 40 mL of tetrahydrofuran for dilution, add 1 g of aluminum isopropoxide to mix, react at 300° C. for 5 h, remove tetrahydrofuran, and obtain a gel precursor;

[0099] B. The gel precursor prepared in step A is subjected to pyrolysis reaction under oxygen conditions at a pyrolysis temperature of 700° C. for 2 h. After the reaction, the system is naturally cooled to room temperature and then ground through a 100-mesh sieve to obtain a composite thermal insulation filler;

[0100] C. Disperse 15 g of the composite thermal insulation filler prepared in step B and 105 g of polytetrafluoroethylene powder in anhydrous ethanol, mix, add 7.5 g of glass fiber, place in a high-speed stirrer at 1200 rpm for 2 h, and dry to obtain a preformed powder;

[0101] D. The preformed powder prepared in step C is placed in a press for compaction. After demoulding, it is placed in a high-temperature furnace and heated to 360°C at a rate of 2°C / min. After being kept at this temperature for 4 hours, it is naturally cooled to room temperature to obtain a thermal insulation layer.

[0102] This embodiment also provides a method for preparing a multi-layer resin composite electrically heated lightweight floor, which is the same as the preparation method described in Example 1.

[0103] Example 3

[0104] This embodiment provides a multi-layer resin composite electric heating lightweight floor, which comprises from top to bottom:

[0105] Wear-resistant layer with a thickness of 0.3mm, pressure-resistant layer with a thickness of 2mm, electric heating film with a thickness of 1mm, and thermal insulation layer with a thickness of 5mm;

[0106] The wear-resistant layer includes the following components in parts by weight: 100 parts of polyphenylene sulfide resin, 25 parts of polytetrafluoroethylene resin, 15 parts of polyvinylidene fluoride resin, 15 parts of modified boron nitride, 15 parts of glass fiber, 15 parts of wear-resistant filler, and 0.3 parts of 1076 antioxidant;

[0107] The preparation method of the wear-resistant layer specifically comprises the following steps:

[0108] ① Place 30 g of boron nitride nanosheets in a three-necked flask, add 500 mL of deionized water, stir evenly, adjust the pH to 9.5, add 1.5 g of octadecyltrimethylammonium bromide, reflux at 90 ° C for 5 h, remove the filtrate by suction, wash the solid with deionized water, place in a vacuum drying oven, and dry at 80 ° C for 20 h to obtain modified boron nitride;

[0109] ② Prepare a sodium hydroxide solution with a mass fraction of 50%, take 100 mL of the sodium hydroxide solution and place it in a flask, add 15 g of titanium diboride, and heat the reaction at 120°C for 2 hours. After the reaction system is naturally cooled to room temperature, filter and remove the filtrate; take 1 g of perfluorodecyltriethoxysilane and dissolve it in 50 mL of deionized water to obtain a perfluorodecyltriethoxysilane solution, transfer the filtered solid to the perfluorodecyltriethoxysilane solution, ultrasonically treat it at 500W for 1 hour, add 15 g of zirconium oxide grinding balls for ball milling, and after 1 hour, wash the reactants on the grinding balls with anhydrous ethanol, combine the reactants, and dry them to obtain wear-resistant fillers;

[0110] ③ Evenly mix 100 g of polyphenylene sulfide resin, 25 g of polytetrafluoroethylene resin and 15 g of polyvinylidene fluoride resin, heat to a molten state, stir on a stirrer at 120 rpm for 1 h, add 0.3 g of 1076 antioxidant, and continue stirring for 30 min to obtain a matrix material;

[0111] ④ Add 15g of modified boron nitride prepared in step ①, 15g of glass fiber and 15g of wear-resistant filler prepared in step ② to the base material prepared in step ③, melt-extrude at an extrusion temperature of 250°C, and transfer to a blow molding machine for blow molding to obtain a wear-resistant layer.

[0112] The pressure-resistant layer includes the following components in parts by weight: 50 parts of polyethylene resin, 20 parts of polyurethane elastomer, 30 parts of modified boron nitride, 5 parts of maleic anhydride grafted polyvinyl acetate, 3 parts of oxazoline crosslinking agent, 1 part of 1076 antioxidant, 3 parts of calcium stearate, and 1 part of antioxidant 264;

[0113] The method for preparing the pressure-resistant layer is the same as that in Example 1.

[0114] The raw materials of the electric heating film specifically include the following components in parts by weight: 60 parts of cellulose, 6 parts of graphene oxide, 3 parts of sodium carbonate, and 45 parts of polyvinylidene fluoride;

[0115] The preparation method of the electric heating film specifically comprises the following steps:

[0116] S1. Place 20 g of cellulose and 1 g of sodium carbonate in a flask, add 200 mL of deionized water, stir to disperse the system evenly, add 2 g of graphene oxide, place under 450 W for ultrasonic treatment for 30 min, filter, remove the filtrate, dry the filtered solid under ventilation conditions, and obtain a graphene foaming precursor after complete drying;

[0117] S2, preheating the tube furnace to 400° C., transferring the graphene foaming precursor prepared in step S1 into a quartz boat, placing it in the tube furnace, and performing heat treatment for 1 min. Immediately after the heat treatment, the mixture is repeatedly washed with a 1 mol / L hydrochloric acid solution to remove sodium carbonate, thereby obtaining a graphene oxide / cellulose composite;

[0118] S3, pyrolyzing the graphene oxide / cellulose composite prepared in step S2 in a tube furnace, heating to 800° C. at 10° C. / min in a nitrogen atmosphere, keeping the temperature for 1 hour, and then naturally cooling to room temperature to obtain a three-dimensional carbon skeleton graphene;

[0119] S4, 3.772 g of the three-dimensional carbon skeleton graphene prepared in step S3 was transferred to a flask, 250 mL of DMAC was added, and ultrasonic treatment was performed at 500 W for 1 h. After uniform dispersion, a three-dimensional carbon skeleton graphene dispersion was obtained, 15 g of PVDF was placed in 500 mL of DMAC and mixed, and then added to the three-dimensional carbon skeleton graphene dispersion, and placed on a magnetic stirrer, and stirred at 300 rpm for 4 h to obtain an electric heating film precursor solution;

[0120] S5. Transfer the electric heating film precursor solution prepared in step S4 to a mold, dry it in an oven under vacuum at 100° C., and demold it after 12 hours to obtain an electric heating film.

[0121] The heat insulation layer comprises the following components in parts by weight: 10 parts of composite heat insulation filler, 70 parts of polytetrafluoroethylene, and 5 parts of glass fiber;

[0122] The preparation method of the thermal insulation layer specifically comprises the following steps:

[0123] A. Add 20 g of polymethylhydrogensiloxane to 40 mL of tetrahydrofuran for dilution, add 1 g of aluminum isopropoxide to mix, react at 300° C. for 5 h, remove tetrahydrofuran, and obtain a gel precursor;

[0124] B. The gel precursor prepared in step A is subjected to pyrolysis reaction under oxygen conditions at a pyrolysis temperature of 700° C. for 2 h. After the reaction, the system is naturally cooled to room temperature and then ground through a 100-mesh sieve to obtain a composite thermal insulation filler;

[0125] C. Disperse 15 g of the composite thermal insulation filler prepared in step B and 105 g of polytetrafluoroethylene powder in anhydrous ethanol, mix, add 7.5 g of glass fiber, place in a high-speed stirrer at 1200 rpm for 2 h, and dry to obtain a preformed powder;

[0126] D. The preformed powder prepared in step C is placed in a press for compaction. After demoulding, it is placed in a high-temperature furnace and heated to 360°C at a rate of 2°C / min. After being kept at this temperature for 4 hours, it is naturally cooled to room temperature to obtain a thermal insulation layer.

[0127] This embodiment also provides a method for preparing a multi-layer resin composite electrically heated lightweight floor, which is the same as the preparation method described in Example 1.

[0128] Comparative Example 1

[0129] This comparative example provides an electric heating composite floor and a preparation method thereof, which is different from Example 1 only in that the wear-resistant layer and the pressure-resistant layer among all components do not include modified boron nitride, and the remaining components and component contents are the same as those in Example 1.

[0130] Comparative Example 2

[0131] This comparative example provides an electric heating composite floor and a preparation method thereof, which differs from Example 1 only in that the raw materials in the electric heating layer among all components only include 10 parts of graphene and 40 parts of polyvinylidene fluoride, and the preparation method of the electric heating layer only includes S3 and S4, and the remaining components and component contents are the same as those in Example 1.

[0132] Comparative Example 3

[0133] This comparative example provides an electric heating composite floor and a preparation method thereof, which differs from Example 1 only in that the composite thermal insulation filler in the thermal insulation layer of all components is replaced with nano-silicon dioxide of the same mass fraction, and the remaining components and component contents are the same as those in Example 1.

[0134] Experimental Example 1

[0135] In this experimental example, the electric heating performance of the multi-layer resin composite electric heating lightweight floor prepared by Examples 1-3 and Comparative Examples 1-3 was measured. The composite electric heating lightweight floor test specimens were connected to the electric heating experimental platform, the output voltage was set to 220V, and infrared temperature was used to record the temperature change after power was turned on.

[0136] Figure 3 The temperature rise results of the multi-layer resin composite electric heating lightweight floor prepared by Examples 1-3 and Comparative Examples 1-3 are shown in the figure. As shown in the figure, the surface temperature of the composite electric heating lightweight floor prepared by Examples 1-3 reaches 30°C after 20-30 minutes and can be maintained at 30-35°C within 80 minutes. In the floor prepared by Comparative Example 1, the wear-resistant layer and the pressure-resistant layer lack modified boron nitride. The modified boron nitride has good thermal conductivity. Due to the reduced thermal conductivity of the wear-resistant layer and the pressure-resistant layer, the temperature rise rate of the floor surface is relatively fast. Slow; in the floor prepared in Comparative Example 2, the electric heating layer is made of a composite of graphene and PVDF, the dispersion performance of graphene in PVDF is poor, the electrical conductivity and thermal conductivity are limited, the surface temperature of the floor is low, and the heating rate is slow; in the floor prepared in Comparative Example 3, the composite insulation material of the insulation layer is replaced by ordinary nano-silicon dioxide, resulting in the heat of the floor being lost from the floor stratum, and the floor surface heating rate is fast, but due to the heat loss, the surface temperature first rises to 29.3°C and then drops to 26.7°C, and the temperature is unstable.

[0137] Experimental Example 2

[0138] In this experimental example, the floor prepared by Examples 1-3 and Comparative Examples 1-3 was subjected to an electric-thermal radiation test. According to the heat measurement method in GB / T7287-2008 and the standard definition of electric-thermal radiation conversion efficiency, the electric-thermal radiation conversion efficiency was calculated. The calculation formula is as follows:

[0139] η= ×100%;

[0140] Where: η is the electric-thermal radiation conversion efficiency, unit is %; S is the area of ​​the radiation surface, unit is square meter 2 ;P e is the measured electric power, in W; T r is the mean radiation temperature, in K; T o —ambient temperature, in K; σ is Stepan-Boltzmann constant, 5.67×10 -8 W / (m 2 ·K 4 ).

[0141] Figure 4 This is a graph showing the electric-thermal radiation conversion efficiency of the multi-layer resin composite electric heating lightweight floor prepared by Examples 1-3 and Comparative Examples 1-3. As shown in the figure, the electric-thermal radiation conversion efficiency of the multi-layer resin composite electric heating lightweight floor prepared by Examples 1-3 is 61.1-63.8%, Comparative Example 1 is 43.7%, Comparative Example 2 is 38.1%, and Comparative Example 3 is 45.3%; the wear-resistant layer and the pressure-resistant layer in Comparative Example 1 lack modified boron nitride, which leads to a decrease in heat conduction efficiency and further reduces the electric-thermal radiation conversion efficiency; the graphene material of the electric heating film in Comparative Example 2 is unevenly dispersed in PVDF; the thermal insulation performance of the thermal insulation layer in Comparative Example 3 is poor, and heat is lost faster.

[0142] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.

[0143] The present invention and its implementation methods are described above, which is not restrictive. The drawings are only one of the implementation methods of the present invention, and the actual application is not limited thereto. In short, if ordinary technicians in the field are inspired by it and design methods and embodiments similar to the technical solution without creativity without departing from the purpose of the invention, they should all fall within the protection scope of the present invention.

Claims

1. A method for preparing a multi-layer resin composite electrically heated lightweight floor, characterized in that: The composite electrically heated lightweight floor is formed by gluing a wear-resistant layer, a pressure-resistant layer, an electric heating film and a heat-insulating layer with high-temperature-resistant polyurethane or epoxy structural adhesive and pressing; The wear-resistant layer comprises the following components in parts by weight: 90-120 parts of polyphenylene sulfide resin, 20-30 parts of polytetrafluoroethylene resin, 10-20 parts of polyvinylidene fluoride resin, 20-30 parts of modified boron nitride, 10-20 parts of glass fiber, 10-20 parts of wear-resistant filler, and 0.1-0.5 parts of 1076 antioxidant; The preparation method of the wear-resistant layer specifically comprises the following steps: ① Place boron nitride nanosheets in deionized water to obtain a boron nitride nanosheet dispersion, adjust the pH to 9.0-9.5, add octadecyltrimethylammonium bromide, and reflux at 80-90° C. for 5-7 hours, filter, wash the solid with deionized water, and vacuum dry at 70-80° C. for 20-30 hours to obtain modified boron nitride; ② Activate titanium diboride in a sodium hydroxide solution at an activation temperature of 100-120°C for 2-3 hours, filter, transfer the solid to a perfluorodecyltriethoxysilane solution, perform ultrasonic treatment at 400-500W for 1-2 hours, add zirconium oxide grinding balls for grinding, wash the grinding balls with anhydrous ethanol after 1-2 hours, remove excess solvent, and dry to obtain a wear-resistant filler; ③ Evenly mix polyphenylene sulfide resin, polytetrafluoroethylene resin and polyvinylidene fluoride resin, heat to a molten state, stir on a stirrer at a speed of 100-120 rpm for 1 hour, add 1076 antioxidant, and continue stirring for 30-40 minutes to obtain a matrix material; ④ Add the modified boron nitride, glass fiber and wear-resistant filler prepared in step ① to the base material prepared in step ③, melt extrude at an extrusion temperature of 250-270° C., and transfer to a blow molding machine for blow molding to obtain a wear-resistant layer; The pressure-resistant layer comprises the following components in parts by weight: 40-50 parts of polyethylene resin, 20-30 parts of polyurethane elastomer, 20-30 parts of modified boron nitride, 5-8 parts of maleic anhydride grafted polyvinyl acetate, 3-6 parts of oxazoline crosslinking agent, 1-3 parts of 1076 antioxidant, 1-3 parts of calcium stearate, and 0.5-1 parts of antioxidant 264; The raw materials of the electric heating film specifically include the following components in parts by weight: 50-60 parts of cellulose, 5-10 parts of graphene oxide, 2-3 parts of carbonate, and 45-56 parts of polyvinylidene fluoride; The heat insulation layer comprises the following components in parts by weight: 10-20 parts of composite heat insulation filler, 70-80 parts of polytetrafluoroethylene, and 5-10 parts of glass fiber; The preparation method of the thermal insulation layer specifically comprises the following components: A. reacting polydimethylsiloxane with an organic alcohol aluminum compound at a reaction temperature of 250-300° C. for a reaction time of 5-8 hours to obtain a gel precursor; B. The gel precursor prepared in step A is subjected to pyrolysis reaction under oxygen conditions at a pyrolysis temperature of 700-800° C. for 2-3 hours. After the reaction system is naturally cooled to room temperature, it is ground through a 100-mesh sieve to obtain a composite thermal insulation filler; C. Disperse the composite thermal insulation filler and polytetrafluoroethylene powder prepared in step B in anhydrous ethanol, mix, add glass fiber, stir at 1000-1200 rpm for 2-3 hours in a high-speed stirrer, and dry to obtain a preformed powder; D. The preformed powder prepared in step C is placed in a press to be pressed into shape. After demolding, it is placed in a high-temperature furnace for high-temperature treatment, the temperature is increased to 340-360°C at 2°C / min, and after keeping the temperature for 2-4 hours, it is naturally cooled to room temperature to obtain a thermal insulation layer.

2. The method for preparing the multi-layer resin composite electrically heated lightweight floor according to claim 1, characterized in that: In step ①, in the boron nitride nanosheet dispersion, the mass concentration of the boron nitride nanosheets is 50-60 g / L; and the amount of octadecyltrimethylammonium bromide added is 0.3-0.5% of the mass of the boron nitride nanosheets.

3. The method for preparing the multi-layer resin composite electrically heated lightweight floor according to claim 2, characterized in that: In step ②, the mass fraction of sodium hydroxide in the sodium hydroxide solution is 40-50%; the mass concentration of titanium diboride in the sodium hydroxide solution is 0.1-0.15 g / mL; the perfluorodecyltriethoxysilane solution is a solution of perfluorodecyltriethoxysilane in anhydrous ethanol, and the mass concentration of the perfluorodecyltriethoxysilane solution is 20-30 g / L; the mass ratio of perfluorodecyltriethoxysilane to titanium diboride is 1:10-20.

4. The method for preparing the multi-layer resin composite electrically heated lightweight floor according to claim 1, characterized in that: The preparation method of the electric heating film specifically comprises the following steps: S1. Mix and disperse cellulose and carbonate in deionized water, add graphene oxide, perform ultrasonic treatment at 300-450W for 30min, filter, and completely dry the solid under ventilation conditions to obtain a graphene foaming precursor; S2, preheating the tube furnace to 300-400° C., transferring the graphene foaming precursor prepared in step S1 to a quartz boat, placing it in the tube furnace, performing a heat treatment for 1-3 min, and repeatedly washing with a 1 mol / L hydrochloric acid solution to remove excess carbonate, thereby obtaining a graphene oxide / cellulose composite; S3, pyrolyzing the graphene oxide / cellulose composite prepared in step S2 in a tube furnace, heating at 10°C / min in a nitrogen atmosphere, heating to 600-800°C, keeping the temperature for 1-1.5h, and naturally cooling to room temperature to obtain three-dimensional carbon skeleton graphene; S4, dispersing the three-dimensional carbon skeleton graphene prepared in step S3 in DMAC, ultrasonically treating at 400-500W for 1-2h, adding PVDF solution, placing on a magnetic stirrer and stirring at 200-300rpm for 4-6h to obtain an electric heating film precursor solution; S5. Place the electric heating film precursor solution prepared in step S4 in an oven and dry it at 80-100° C. under vacuum conditions. After 12-15 hours, an electric heating film is obtained.

5. The method for preparing the multi-layer resin composite electrically heated lightweight floor according to claim 4, characterized in that: In step S1, the mass fraction of cellulose in deionized water is 5-10%.

6. The method for preparing the multi-layer resin composite electrically heated lightweight floor according to claim 5, characterized in that: In step S4, the mass concentration of the three-dimensional carbon skeleton graphene in DMAC is 10-15 g / L; the PVDF solution is PVDF dissolved in DMAC, and the mass concentration of PVDF in DMAC is 20-30 g / L.

7. The method for preparing the multi-layer resin composite electrically heated lightweight floor according to claim 1, characterized in that: In step A, the mass ratio between the polydimethylsiloxane and the organic alcohol aluminum compound is 5-20:

1.

8. A multi-layer resin composite electric heating lightweight floor made according to the preparation method according to any one of claims 1 to 7, characterized in that: The wear-resistant layer has a thickness of 0.2-0.5 mm; the pressure-resistant layer has a thickness of 1-2 mm; the electric heating film has a thickness of 0.5-1 mm; and the heat-insulating layer has a thickness of 3-5 mm.