Alloy ingot, alloy with insulating properties on the surface and preparation method thereof
By adding trace amounts of vanadium and zirconium elements to the iron-chromium-aluminum-ferritic antioxidant alloy, a dense alumina insulating layer is formed, which solves the problems of low surface hardness and poor wear resistance, and achieves high resistance and wear resistance The insulation performance extends the service life of the alloy.
Patent Information
- Application Number
- CN202410607764.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-16
- Publication Date
- 2024-11-26
- Estimated Expiration
- 2044-05-16
AI Technical Summary
There are many types of alloy elements with insulating properties on the existing surface, with low surface hardness and poor wear resistance of the insulating layer, which affects the life of the alloy.
Based on the iron-chromium-aluminum ferrite antioxidant alloy, by adding trace alloy elements such as vanadium and zirconium, a dense alumina insulating layer is formed on the surface of the material through heat treatment, which improves surface hardness and wear resistance .
The formed alumina insulating layer has high resistance and good wear resistance, which is suitable for use environments of -10~200℃, extending the service life of the alloy.
Smart Images

Figure CN118186312B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of alloys, and in particular to an alloy ingot, an alloy with insulating properties on the surface and a preparation method thereof. Background Art
[0002] Alloy workpieces with insulating properties on the surface are widely used in important fields such as the electronics industry, automobile manufacturing, and aerospace. The steps for producing workpieces with insulating properties on the surface are: first, smelting to obtain a master alloy ingot, the master alloy ingot is forged and machined on a lathe to make a workpiece that meets the size specification requirements, and then the workpiece is heat treated to form an oxide film on the surface of the workpiece. The thickness and density of the oxide film on the surface of the workpiece determine the insulation performance and service life of the workpiece.
[0003] Patent CN 102409255 A discloses an alloy with insulating properties on the surface, whose chemical composition by mass percentage is: chromium 10%~35%, aluminum 2%~10%, silicon 0%~0.5%, manganese 0.1%~1.0%, cobalt 0.2%~0.5%, vanadium 0.1%~0.7%, tungsten 0.1%~0.8%, niobium 0.2%~0.8% and nickel 0.1%~1.2%, and the balance is iron and unavoidable impurities. The main application environment of the alloy is -10~100℃. The alloy product has many types of elements and complex composition. At the same time, the thickness of the insulating layer of the product after heat treatment is poor.
[0004] Patent CN 108950415 A discloses an alloy having high-temperature insulation properties on its surface, whose chemical composition by mass percentage is: chromium 10%~35%, aluminum 2%~10%, silicon 0.01%~0.5%, manganese 0.01%~1.0%, zirconium 0.01%~5%, cobalt 0.2%~0.5%, vanadium 0.01%~0.7%, titanium 0.3%~1.2%, tungsten 0.01%~0.8%, niobium 0.01%~0.8%, nickel 0.01%~1.2%, molybdenum 0.02%~3.0%, tantalum 0.01%~1%, yttrium 0.01%~1% and hafnium 0.01%~1%, and the balance is iron and unavoidable impurities. This technical solution adds metal tantalum, metal yttrium, metal zirconium, metal titanium, metal molybdenum and metal hafnium elements on the basis of CN 102409255 A. The addition of the above elements is conducive to improving the high temperature strength of the alloy and forming mixed oxides such as yttrium oxide, so that the alloy has good insulation performance under high temperature environment of 580~645℃, so its application field is mainly in the aerospace field. However, the addition of metal elements further increases the types of components, which in turn increases the complexity of smelting; moreover, the surface hardness is not high, and the wear resistance of the insulation layer is poor, which greatly affects the life of the alloy. Summary of the invention
[0005] In view of the technical problems that the existing alloys with insulating properties on the surface have many types of product elements and low surface hardness, the present invention provides an alloy ingot, an alloy with insulating properties on the surface and a preparation method thereof. On the basis of an iron-chromium-aluminum ferrite antioxidant alloy, trace alloy elements are added. After a heat treatment process, the aluminum in the material can form a dense aluminum oxide insulating layer on the surface of the material during the heat treatment process. The ceramic layer has high resistance, suitable surface hardness and good wear resistance, thereby solving the problem of low surface hardness of existing products.
[0006] In a first aspect, the present invention provides an alloy ingot, the chemical composition composition by mass percentage is: chromium 10%~30%, aluminum 2%~8%, silicon 0.01%~0.5%, manganese 0.01%~0.8%, titanium 0.3%~1.0%, vanadium ≤0.5%, zirconium 0.05%~2.0%, and the remainder is iron and unavoidable impurities. After heat treatment, an aluminum oxide insulating layer can be formed on the surface of the alloy ingot.
[0007] Furthermore, the method for preparing the alloy ingot comprises the following steps:
[0008] (1) Melting: Melt the iron, chromium and aluminum raw materials under vacuum conditions;
[0009] (2) Refining: After the iron, chromium and aluminum raw materials are melted, they are degassed and refined under argon protection;
[0010] (3) Deoxidation: Deoxidizers are added to deoxidize the molten steel. The deoxidizers are metal silicon, metal manganese, metal aluminum and titanium.
[0011] (4) Casting: Add vanadium and zirconium trace element alloy package for alloying, and finally cast under argon protection.
[0012] Furthermore, in step (1), the melting is performed using electromagnetic induction current under vacuum conditions of 0.1-10 Pa, with a frequency of 2950-3050 Hz and a power of 40-100 kW.
[0013] Furthermore, step (2) is performed under the protection of argon partial pressure of 5-50 kPa, and degassing and refining is performed for 10-30 minutes.
[0014] Furthermore, the deoxygenation time in step (3) is 2 to 5 minutes.
[0015] Furthermore, step (4) is cast under the protection of argon partial pressure of 5 to 50 kPa.
[0016] Furthermore, the heat treatment method comprises the following steps:
[0017] In air, keep the alloy ingot at 900-1300°C for 2-8 hours to oxidize the surface of the alloy ingot.
[0018] In a second aspect, the present invention provides a method for preparing an alloy having insulating properties on the surface, comprising at least the following steps:
[0019] In air, the alloy ingot is kept at 900-1300° C. for 2-8 hours to oxidize the surface of the alloy ingot and form an aluminum oxide insulating layer on the surface of the alloy ingot.
[0020] In a third aspect, the present invention also provides an alloy having insulating properties on the surface which is prepared by the above preparation method.
[0021] Furthermore, the alloy having insulating properties on the surface has an operating temperature of -10 to 200°C.
[0022] The beneficial effects of the present invention are:
[0023] The present invention adds trace alloy elements to the iron-chromium-aluminum ferrite anti-oxidation alloy to make an alloy ingot. The aluminum in the material can form a dense aluminum oxide ceramic insulation layer on the surface of the alloy ingot during the heat treatment process. The added trace alloy vanadium and zirconium elements increase the thickness of the aluminum oxide to 38-60 μm. Research has found that appropriate addition of zirconium elements forms zirconium oxide distributed at the grain boundaries, which can promote oxygen to gather toward the zirconium oxide along the grain boundaries, and finally form aluminum oxide near the zirconium oxide.
[0024] The use environment temperature of the alloy with insulating properties on the surface of the present invention is -10~200°C, and the aluminum oxide insulating layer of the alloy has high resistance, suitable surface hardness and good wear resistance in the use environment. Specifically, at room temperature and -10°C, the surface resistance of the alloy with insulating properties on the surface of the present invention can reach 2800~4200 megohms, and the insulation resistance can reach 480~650 megohms; at 200°C, the surface resistance of the alloy with insulating properties on the surface can be maintained at 2000~4000 megohms, and the insulation resistance can reach 400~600 megohms. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.
[0026] Figure 1 This is a cross-sectional SEM photograph of the alloy prepared in Example 1 of the present invention.
[0027] Figure 2 This is a cross-sectional SEM photograph of an alloy prepared by prior art CN 102409255 A.
[0028] Figure 3 It is an XRD comparison diagram of the alloy prepared in Example 1 of the present invention and the alloy prepared in the prior art CN 102409255 A. DETAILED DESCRIPTION
[0029] In order to enable those skilled in the art to better understand the technical solutions in the present invention, the technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the drawings in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present invention.
[0030] Example 1
[0031] An alloy ingot has the following chemical components by mass percentage: 10% chromium, 2% aluminum, 0.01% silicon, 0.01% manganese, 0.3% titanium, 0.1% vanadium, 0.05% zirconium, and the balance is iron and inevitable impurities.
[0032] The method for preparing the alloy ingot comprises the following steps:
[0033] (1) Melting: Iron, chromium and aluminum raw materials are melted under a vacuum of 5 Pa using electromagnetic induction current at a frequency of 3000 Hz and a power of 75 kW;
[0034] (2) Refining: After the iron, chromium and aluminum raw materials are melted, they are degassed and refined for 20 minutes under the protection of argon gas at a partial pressure of 35 kPa;
[0035] (3) Deoxidation: Add deoxidizer to deoxidize the molten steel for 3 minutes. The deoxidizer is silicon, manganese and aluminum alloy;
[0036] (4) Casting: Add vanadium and zirconium trace element alloy package for alloying, and finally cast under the protection of argon partial pressure of 35 kPa.
[0037] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm using a CNC machine. The cylinder obtained by processing the alloy ingot was used as the alloy base material, and heat-treated at 1250°C in air for 6 hours, and then cooled with the furnace to obtain an alloy with an alumina insulating layer on the surface.
[0038] The alloy obtained by heat treatment was observed, and the alloy prepared by prior art CN 102409255 A was used as a control. The results are as follows Figure 1 , Figure 2 shown. Figure 1In the figure, the dark gray area from top to bottom is the insulating layer on the alloy surface, and the light gray area is the alloy base material. It can be seen that the alloy surface obtained by the heat treatment of Example 1 has a thicker insulating layer (more than 50 μm). This is because the zirconium element forms zirconium oxide at the grain boundaries, which promotes the aggregation of oxygen to the zirconium oxide along the grain boundaries, and finally forms aluminum oxide near the zirconium oxide (the top granular area is the formed aluminum oxide). Figure 2 The pure black area on the far right is the inlay material used for SEM testing. The dark gray area that gradually appears to the left represents the surface insulation layer of the alloy from the edge to the inside after heat treatment in the prior art CN 102409255 A. The light gray area to the left is the alloy base material. Since there is no zirconium oxide at the grain boundary of the prior art CN102409255 A, the oxygen atoms cannot expand along the grain boundary during the heat treatment, resulting in a thinner insulation layer (about 30μm). Figure 1 , Figure 2 The difference in the thickness of the insulating layer indicates that the reasonable combination of the alloy elements of the present invention and the technical means of adding a trace amount of zirconium element increase the thickness of the insulating layer.
[0039] The alloy obtained by heat treatment in Example 1 was subjected to XRD test, and the alloy prepared by prior art CN 102409255 A was used as a control. The results are as follows: Figure 3 As shown, by comparison, it can be found that the oxide layer on the surface of the alloy of the present invention contains more Fe(Cr, Al)2O4 and is thicker.
[0040] Example 2
[0041] An alloy ingot has the following chemical components by mass percentage: 20% chromium, 5% aluminum, 0.25% silicon, 0.4% manganese, 0.65% titanium, 0.25% vanadium, 1.0% zirconium, and the balance is iron and inevitable impurities.
[0042] The preparation method of the alloy ingot is the same as that of Example 1.
[0043] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm by a CNC machine. The cylinder obtained by processing the alloy ingot was used as the alloy matrix and heat treated in the same process as in Example 1.
[0044] Example 3
[0045] An alloy ingot has the following chemical components by mass percentage: 30% chromium, 8% aluminum, 0.5% silicon, 0.8% manganese, 1.0% titanium, 0.5% vanadium, 2.0% zirconium, and the balance is iron and inevitable impurities.
[0046] The method for preparing the alloy ingot comprises the following steps:
[0047] (1) Melting: The iron, chromium and aluminum raw materials are melted under a vacuum of 0.5 Pa using electromagnetic induction current at a frequency of 3050 Hz and a power of 100 kW;
[0048] (2) Refining: After the iron, chromium and aluminum raw materials are melted, they are degassed and refined for 10 minutes under the protection of argon gas at a partial pressure of 5 kPa;
[0049] (3) Deoxidation: Add deoxidizer to deoxidize the molten steel for 5 minutes. The deoxidizer is silicon, manganese and aluminum alloy;
[0050] (4) Casting: Add vanadium and zirconium trace element alloy package for alloying, and finally cast under the protection of argon partial pressure of 5 kPa.
[0051] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm using a CNC machine tool.
[0052] The cylinder obtained by processing the alloy ingot is used as the alloy matrix, which is heat treated in air at 1300° C. for 2.5 hours and then cooled in the furnace to obtain an alloy with an aluminum oxide insulating layer on the surface.
[0053] Example 4
[0054] An alloy ingot has the following chemical components by mass percentage: 18% chromium, 6% aluminum, 0.1% silicon, 0.2% manganese, 0.5% titanium, 1.35% zirconium, and the remainder is iron and inevitable impurities.
[0055] The method for preparing the alloy ingot comprises the following steps:
[0056] (1) Melting: The iron, chromium and aluminum raw materials are melted under a vacuum of 10 Pa using electromagnetic induction current with a frequency of 2950 Hz and a power of 40 kW;
[0057] (2) Refining: After the iron, chromium and aluminum raw materials are melted, they are degassed and refined for 30 minutes under the protection of argon gas at a partial pressure of 50 kPa;
[0058] (3) Deoxidation: Add deoxidizer to deoxidize the molten steel for 2 minutes. The deoxidizer is silicon, manganese and aluminum alloy;
[0059] (4) Casting: Add vanadium and zirconium trace element alloy package for alloying, and finally cast under the protection of argon partial pressure of 50 kPa.
[0060] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm using a CNC machine tool.
[0061] The cylinder obtained by processing the alloy ingot is used as the alloy matrix, which is heat treated in air at 900° C. for 8 hours and then cooled in the furnace to obtain an alloy with an aluminum oxide insulating layer on the surface.
[0062] Comparative Example 1
[0063] An alloy ingot has the following chemical components by mass percentage: 20% chromium, 5% aluminum, 0.25% silicon, 0.4% manganese, 0.65% titanium, 0.1% vanadium, 0.04% zirconium, and the balance is iron and inevitable impurities.
[0064] The preparation method of the alloy ingot is the same as that of Example 1.
[0065] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm by a CNC machine. The cylinder obtained by processing the alloy ingot was used as the alloy matrix and heat treated in the same process as in Example 1.
[0066] Comparative Example 2
[0067] An alloy ingot has the following chemical components by mass percentage: 20% chromium, 5% aluminum, 0.25% silicon, 0.4% manganese, 0.2% titanium, 0.05% vanadium, 0.01% zirconium, and the balance is iron and inevitable impurities.
[0068] The preparation method of the alloy ingot is the same as that of Example 1.
[0069] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm by a CNC machine. The cylinder obtained by processing the alloy ingot was used as the alloy matrix and heat treated in the same process as in Example 1.
[0070] Comparative Example 3
[0071] An alloy ingot has the following chemical components by mass percentage: 20% chromium, 5% aluminum, 0.25% silicon, 0.4% manganese, 0.65% titanium, 0.25% vanadium, and the balance is iron and inevitable impurities.
[0072] The preparation method of the alloy ingot is the same as that of Example 1.
[0073] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm by a CNC machine. The cylinder obtained by processing the alloy ingot was used as the alloy matrix and heat treated in the same process as in Example 1.
[0074] Comparative Example 4
[0075] An alloy ingot has the following chemical components by mass percentage: 20% chromium, 5% aluminum, 0.25% silicon, 0.4% manganese, 0.65% titanium, 0.25% vanadium, 3.0% zirconium, and the balance is iron and inevitable impurities.
[0076] The preparation method of the alloy ingot is the same as that of Example 1.
[0077] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm by a CNC machine. The cylinder obtained by processing the alloy ingot was used as the alloy matrix and heat treated in the same process as in Example 1.
[0078] Comparative Example 5
[0079] An alloy ingot has the following chemical components by mass percentage: 20% chromium, 5% aluminum, 0.25% silicon, 0.4% manganese, 1.2% titanium, 0.25% vanadium, 1.0% zirconium, and the balance is iron and inevitable impurities.
[0080] The preparation method of the alloy ingot is the same as that of Example 1.
[0081] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm by a CNC machine. The cylinder obtained by processing the alloy ingot was used as the alloy matrix and heat treated in the same process as in Example 1.
[0082] Comparative Example 6
[0083] An alloy ingot has the following chemical components by mass percentage: 20% chromium, 5% aluminum, 0.25% silicon, 0.4% manganese, 0.65% titanium, 0.7% vanadium, 1.0% zirconium, and the balance is iron and inevitable impurities.
[0084] The preparation method of the alloy ingot is the same as that of Example 1.
[0085] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm by a CNC machine. The cylinder obtained by processing the alloy ingot was used as the alloy matrix and heat treated in the same process as in Example 1.
[0086] According to GB / T 13303-1991 "Determination Method for Antioxidation Performance of Steel", the thickness of the aluminum oxide insulation layer on the surface of the alloys obtained by heat treatment in Examples 1 to 4 and Comparative Examples 1 to 6 was measured using a vernier caliper and an outside micrometer; the surface insulation performance of the alloys obtained by heat treatment in Examples 1 to 4 and Comparative Examples 1 to 6 was tested using an insulation withstand voltage tester (500V AC) and a multimeter. The above tests were performed at five different locations on each sample, and then the average value was taken. The results are shown in Table 1 below.
[0087] Table 1 Surface insulation layer thickness and surface insulation properties of alloys
[0088]
[0089] It can be seen that the alloy ingots with specific chemical composition designed by the present invention have high resistance at room temperature, -10°C and 200°C after heat treatment. In Comparative Examples 1, 2 and 3, as the zirconium content of the alloy ingots gradually decreases, the thickness of the surface insulating layer formed by heat treatment also becomes thinner, and the insulation properties of the resulting alloys at room temperature, -10°C and 200°C are significantly deteriorated. Too much zirconium is added to the alloy ingot of Comparative Example 4. During the heat treatment, the excessive zirconium will preferentially form zirconium oxide, affecting the formation of aluminum oxide, thereby reducing the thickness of the oxide film (i.e., insulating layer) on the surface of the alloy. The alloy ingots of Comparative Examples 5 and 6 contain too much titanium and vanadium, which also affects the formation of the surface insulating layer, and the surface insulation performance is poor.
[0090] The hardness of the surface insulation layer of the alloys obtained by heat treatment in Examples 1 to 4 and Comparative Examples 1 to 6 was tested, and the test method was performed in accordance with GB / T230.1-2018 "Metal Rockwell Hardness Test". The above test was performed at five different locations on each sample, and then the average value was taken. The results are shown in Table 2 below.
[0091] Table 2 Surface insulation layer hardness of alloys (HRC)
[0092]
[0093] By comparison, it can be seen that after heat treatment, the surface insulation layer of the alloy ingot with specific chemical composition designed by the present invention has higher hardness at room temperature, -10°C and 200°C, stronger wear resistance and longer service life under the same environment.
[0094] Comparative Example 7
[0095] An alloy ingot, the chemical composition mass percentage of which is: 20% chromium, 5% aluminum, 0.25% silicon, 0.4% manganese, 0.65% titanium, 0.25% vanadium, 1.0% zirconium, 0.3% cobalt, 0.2% tungsten, 0.5% niobium, 0.8% nickel, 0.15% molybdenum, 0.05% tantalum, 0.02% yttrium, 0.1% hafnium, and the balance is iron and unavoidable impurities.
[0096] The method for preparing the alloy ingot comprises the following steps:
[0097] (1) Melting: The raw materials of iron, chromium, aluminum, cobalt, titanium, tungsten, niobium, nickel and molybdenum are melted by electromagnetic induction current under 5 Pa vacuum conditions, with a current frequency of 3000 Hz and a power of 75 kW;
[0098] (2) Refining: After the raw materials of iron, chromium, aluminum, cobalt, titanium, tungsten, niobium, nickel and molybdenum are melted, they are degassed and refined for 20 minutes under the protection of argon gas at a partial pressure of 35 kPa;
[0099] (3) Deoxidation: Add deoxidizer to deoxidize the molten steel for 3 minutes. The deoxidizer is silicon, manganese and aluminum alloy;
[0100] (4) Casting: Add zirconium, tantalum, yttrium, vanadium, and hafnium trace element alloy packages for alloying, and finally cast under the protection of argon gas partial pressure of 35 kPa.
[0101] The alloy ingot was processed into a round bar with a diameter of 13 mm and a length of 1 m, and then processed into a cylinder with a diameter of 12 mm and a length of 20 mm using a CNC machine tool. The cylinder was used as the alloy base material and heat treated at 1250°C in air for 6 hours, and then cooled in the furnace to obtain an alloy with an alumina insulating layer on the surface.
[0102] The surface insulation performance of the alloy obtained by heat treatment in Example 7 was tested using an insulation withstand voltage tester (500V AC) and a multimeter, and the hardness of the surface insulation layer of the alloy obtained by heat treatment in Example 7 was tested according to the method specified in GB / T230.1-2018 "Metal Rockwell Hardness Test". The above tests were performed at five different locations on each sample, and then the average value was taken. The results are shown in Table 3 below.
[0103] Table 3 Performance comparison of alloys in Example 2 and Comparative Example 7
[0104]
[0105] It can be seen from Table 3 that due to the use of various alloy elements such as tungsten, nickel, niobium, cobalt, tantalum, yttrium, molybdenum and hafnium, the insulation performance of Example 7 is better, but correspondingly, because of the addition of various rare and precious metals, the smelting process of Example 7 is complicated and the manufacturing cost is also high; the insulation performance of the alloy of the present invention can already meet the use requirements of most application scenarios. At the same time, the addition of various alloy elements such as tungsten, nickel, niobium, cobalt, tantalum, yttrium, molybdenum and hafnium is very easy to consume oxygen elements and form oxides during solidification and heat treatment, which is not conducive to the formation of surface oxide film. Therefore, the alloy of Example 7 has low hardness and poor wear resistance. The insulating layer on the surface of the alloy obtained by heat treatment in Example 2 has a higher hardness, which is related to the fact that the present invention controls the content of metal zirconium and adopts a suitable smelting process and heat treatment process. These means jointly promote the precipitation of a thicker oxide film on the surface of the alloy. The thicker the oxide film on the surface of the alloy, the greater the hardness, so the service life of the alloy of the present invention is longer.
[0106] Although the present invention has been described in detail with reference to the accompanying drawings and in combination with the preferred embodiments, the present invention is not limited thereto. Without departing from the spirit and essence of the present invention, a person of ordinary skill in the art may make various equivalent modifications or substitutions to the embodiments of the present invention, and these modifications or substitutions shall be within the scope of the present invention. Any person of ordinary skill in the art may easily think of changes or substitutions within the technical scope disclosed by the present invention, and these shall be within the scope of protection of the present invention.
Claims
1. A method for preparing an alloy having insulating properties on the surface, comprising at least the following steps: In air, the alloy ingot is kept at 900-1300°C for 2-8 hours to oxidize the surface of the alloy ingot and form an aluminum oxide insulating layer on the surface of the alloy ingot. The aluminum oxide insulating layer reaches 38-60 μm. The chemical composition of the alloy ingot is as follows: chromium 18%~30%, aluminum 2%~6%, silicon 0.01%~0.5%, manganese 0.01%~0.8%, titanium 0.3%~1.0%, vanadium ≤0.5%, zirconium 0.05%~1.35%, and the balance is iron and unavoidable impurities; At room temperature and -10°C, the surface resistance of the alloy with insulating properties on the surface reaches 2800~4200 megohms, and the insulation resistance reaches 480~650 megohms; at 200°C, the surface resistance of the alloy with insulating properties on the surface remains at 2000~4000 megohms, and the insulation resistance reaches 400~600 megohms.
2. The preparation method according to claim 1, characterized in that The method for preparing the alloy ingot comprises the following steps: (1) Melting: Melt the iron, chromium and aluminum raw materials under vacuum conditions; (2) Refining: After the iron, chromium and aluminum raw materials are melted, they are degassed and refined under argon protection; (3) Deoxidation: Deoxidizers are added to deoxidize the molten steel. The deoxidizers are metal silicon, metal manganese, metal aluminum and titanium. (4) Casting: Add vanadium and zirconium trace element alloy package for alloying, and finally cast under argon protection.
3. The preparation method according to claim 2, characterized in that: Step (1) uses electromagnetic induction current to melt under vacuum conditions of 0.1-10 Pa, with a frequency of 2950-3050 Hz and a power of 40-100 kW.
4. The preparation method according to claim 2, characterized in that: Step (2) is performed under the protection of argon partial pressure of 5 to 50 kPa, and degassing and refining is performed for 10 to 30 minutes.
5. The preparation method according to claim 2, characterized in that: The deoxygenation time in step (3) is 2 to 5 minutes.
6. The preparation method according to claim 2, characterized in that: Step (4) is casting under the protection of argon partial pressure of 5 to 50 kPa.
7. An alloy having insulating properties on the surface obtained by the preparation method as claimed in claim 1.
8. The alloy having surface insulation properties as claimed in claim 7, characterized in that: The operating temperature of the alloy is -10~200℃.