A high-strength and high-plasticity magnesium rare earth alloy and its arc additive manufacturing process

By optimizing the ratio and process in rare earth magnesium alloys, combined with cold metal transition arc additive manufacturing and low-temperature solid solution aging treatment, the problem of difficult balance between strength and plasticity in arc additive manufacturing is solved, and high Magnesium alloy products with high strength simplify the process and reduce production costs.

CN118222898BActive Publication Date: 2024-11-08CHONGQING UNIV
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410353308.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-26
Publication Date
2024-11-08
Estimated Expiration
2044-03-26

AI Technical Summary

Technical Problem

The strength and plasticity of existing rare earth magnesium alloys are difficult to balance after arc additive manufacturing, and the plasticity loss is serious during heat treatment and the cost is high, which is not conducive to sustainable production.

Method used

High-strength, high-plastic magnesium rare earth alloy ratio, including Gd 6-12 wt.%, Al 0.5-2 wt.%, Zr 0.2-0.5 wt.%, Zn 0.1-0.3 wt.%, and cold metal transition arc additive manufacturing With the solid solution aging treatment at low temperature and low time, Mg7Gd, Al2Gd and Al-Zr phases are formed to inhibit grain coarseness and improve the strength and plasticity of the alloy.

Benefits of technology

It significantly improves the tensile strength and elongation of magnesium alloys, reduces abnormal grain growth, reduces plastic loss, simplifies the process flow, reduces production costs, and is suitable for large-scale industrial production.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004760494010000081
    Figure BDA0004760494010000081
  • Figure BDA0004760494010000091
    Figure BDA0004760494010000091
  • Figure HDA0004760494020000011
    Figure HDA0004760494020000011
Patent Text Reader

Abstract

The present invention discloses a high-strength and high-plasticity magnesium rare earth alloy and an arc additive manufacturing process thereof. The magnesium rare earth alloy comprises the following raw materials in mass percentage: Gd 6-12wt.%, Al 0.5-2wt.%, Zr 0.2-0.5wt.%, Zn 0.1-0.3wt.%, the remainder being magnesium and unavoidable impurities, and the mass ratio of Gd to Al is 4-10:1. According to the content ratio of each component of the high-strength magnesium alloy, the present invention selects a combination of cold metal transition arc additive manufacturing technology and solution aging treatment process. The low-temperature and low-time solution treatment method can ensure the full dissolution of the eutectic phase and the full diffusion of the elements, and inhibit the coarsening and abnormal growth behavior of the grains during the solid solution, effectively reducing the plastic loss of the material. In the magnesium alloy sample of the present invention, the alloy grain size is small, there is no abnormal growth after heat treatment, and a large number of nano-level strengthening phases are precipitated in the crystal. The present invention solves the problem of serious plastic loss of rare earth magnesium alloy manufactured by arc additive manufacturing after heat treatment.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of magnesium alloy additive manufacturing, and in particular to a high-strength and high-plasticity magnesium rare earth alloy and an arc additive manufacturing method thereof. Background Art

[0002] Magnesium alloy is the lightest metal structural material in engineering applications. Its specific gravity is similar to that of plastics, and its rigidity and strength are no less than aluminum. It has the advantages of strong earthquake resistance, electromagnetic resistance, thermal conductivity, electrical conductivity, full recycling and no pollution. Adding rare earth elements to magnesium alloy can effectively improve the alloy organization and microstructure, improve the room temperature and high temperature mechanical properties of the alloy, and enhance the corrosion resistance and heat resistance of the alloy. Therefore, rare earth magnesium alloy has higher high temperature mechanical properties and corrosion resistance than conventional magnesium alloy, and is increasingly widely used in important equipment in the fields of weapons and equipment, transportation, etc.

[0003] In recent years, the additive manufacturing technology (i.e. 3D printing) widely used in the manufacture of rare earth magnesium alloys is based on digital model files, using rare earth magnesium alloy wire as raw materials, and manufacturing the required parts by printing layer by layer. This technology has great advantages over traditional casting and extrusion in terms of performance and manufacturing efficiency. It can greatly reduce the loss of raw materials, achieve the characteristics of net forming, and is more conducive to reducing production costs. Cold metal transition (CMT) arc additive manufacturing technology is the application of cold metal transition welding technology to the field of additive manufacturing. It adopts a hot-cold-hot method to reduce the welding current during the droplet transition. It has the advantages of low heat input, spatter-free metal transition, extremely stable arc and good formability. It has been widely used in the additive manufacturing of steel and non-ferrous metal materials.

[0004] Compared with the existing arc additive manufacturing of rare earth magnesium alloy wires, the mechanical properties of the alloys made from rare earth magnesium alloy wires in the past increase with the increase of the rare earth content of the wires, but the excessive rare earth content seriously weakens the plasticity of the material, which increases the risk of wire breakage during the forming of magnesium alloy wires and limits the addition of rare earth elements. Therefore, the strength and plasticity of magnesium alloys are mutually restricted or even contradictory. How to solve the balance between the strength and plasticity of high-performance rare earth magnesium alloys is also an urgent problem to be solved.

[0005] Most cast magnesium alloys can be improved or adjusted through T5 and T6 heat treatment to improve or adjust the mechanical properties and processing properties of the materials. T5 and T6 heat treatments include two stages: high-temperature solid solution and low-temperature aging treatment. Generally, the solid solution temperature is 500-550°C, which needs to be kept warm for more than 10 hours, and the aging temperature is about 200°C, which needs to be kept warm for about 80 hours. At present, arc additive manufacturing of rare earth magnesium alloys in order to obtain the final required mechanical properties adopts a process similar to that of casting rare earth magnesium alloys. For example, the invention patent CN116618792A discloses an arc additive manufacturing method for Mg-Y-Nd-Zr rare earth magnesium alloy structural parts, using wire with Mg-Y-Nd-Zr as the main alloying element as raw material, using CMT arc additive process, and then heat treating the formed components. The solution treatment is: keeping at 520℃~525℃ for 6~8h; the aging treatment is: keeping at 240℃~250℃ for 16h~20h. The result is: the tensile strength is increased by about 12%, the yield strength is increased by about 30%, and the elongation is significantly reduced. For another example, the tensile strength and yield strength of Mg-10Gd-3Y-1Zn-0.5Zr arc additive components before heat treatment are 271MPa, 154MPa, and the elongation is 8.7%, while the tensile strength and yield strength after traditional solution aging heat treatment are 337MPa, 214MPa, and the elongation is only 2.8%. The tensile strength and yield strength of the Mg-6Gd-3Y-0.5Zr arc additive component before heat treatment were 237MPa, 151MPa, and the elongation was 8.9%, while the tensile strength and yield strength after traditional solution aging heat treatment were 345MPa, 218MPa, and the elongation was 5.2%. It can be seen that although the existing heat treatment method can effectively improve the tensile strength and yield strength of arc additive manufacturing rare earth magnesium alloy, the plasticity of the alloy has been significantly sacrificed, and the plasticity has been reduced by more than 40%. The main reasons are: 1) Mg metal itself has a high critical shear stress, and the slip system is difficult to activate, so its plasticity at room temperature is poor. Although the nano-strengthening phase formed after heat treatment of rare earth magnesium alloys hinders slip and improves strength, it further reduces the plasticity of the alloy; 2) The arc manufacturing grains are generally small, and there is uneven distribution of thermal stress in the matrix. In the long-term high-temperature solution treatment, the grains are easy to grow, and the grains in the higher residual thermal stress area will further grow abnormally. Therefore, the grains with uneven size distribution will cause stress concentration and induce early fracture. Therefore, the problem faced by the additive manufacturing of rare earth magnesium alloys is that it is difficult to balance the strength and plasticity of high-performance rare earth magnesium alloys, especially after heat treatment. Although the strength of the alloy is increased, the plasticity loss is serious, which directly affects the life of the finished product. In addition, the solution temperature is high, the time is long, and the cost is high during the heat treatment process, which is not conducive to sustainable production. Summary of the invention

[0006] In view of the above-mentioned deficiencies in the prior art, the technical problem to be solved by the present invention is: to develop a new type of magnesium alloy with synergistically improved stiffness and plasticity; at the same time, to develop a matching new arc additive manufacturing forming process to solve the problems of the difficulty in balancing the strength and plasticity of existing high-performance rare earth magnesium alloys and the serious plasticity loss of arc additively manufactured rare earth magnesium alloys after T5\T6 heat treatment.

[0007] In order to solve the above technical problems, the present invention adopts the following technical solution: a high-strength and high-plasticity magnesium rare earth alloy, which includes the following raw materials in mass percentage: Gd 6-12wt.%, Al 0.5-2wt.%, Zr 0.2-0.5wt.%, Zn 0.1-0.3wt.%, and the remainder is magnesium and unavoidable impurities, and the mass ratio of Gd to Al is 4-10:1.

[0008] In this way, adding Gd element to the rare earth magnesium alloy of the present invention can help the alloy to form Mg7Gd strengthening phase after aging treatment, significantly improve the strength of the alloy, and the diffusion rate of Gd element is low, which can effectively slow down the grain boundary diffusion and hinder the grain coarsening. By adding Al element in an appropriate amount, the critical shear stress difference between the non-basal plane and the basal plane in the magnesium alloy can be effectively reduced, thereby significantly increasing the plasticity of the wire and the alloy, so as to improve the wire processing performance and reduce the risk of wire breakage of magnesium alloy welding wire. Under the extrusion process, the wire can be made into 5kg / disc, and there is no fracture. And Al element has a high growth limiting factor (Q), which can improve the Q value of the alloy as a whole. High Q will cause a large degree of supercooling before the solid-liquid interface, thereby causing equiaxed crystal transformation and grain refinement, which is beneficial to strength and plasticity. At the same time, Al element can form Al2Gd phase with Gd element during solidification, which has extremely high thermal stability, can pin grain boundaries, and inhibit grain growth. The appropriate amount of Zr element can promote grain nucleation, and at the same time, it can form a thermally stable Al-Zr phase with Al element to improve the high temperature performance of the alloy. The addition of an appropriate amount of Zn element can coordinate the plastic deformation ability of the alloy.

[0009] Furthermore, by precisely controlling the mass ratio of Gd to Al between 4 and 10, the formation of brittle phases such as Mg-AL can be effectively avoided, the increase in component brittleness can be avoided, the Al-RE content of thermal stability can be controlled, the loss of excessive Mg-Gd strengthening phase can be avoided, and the strength and plasticity of the component can be balanced.

[0010] Another object of the present invention is to provide an arc additive manufacturing method based on a high-strength and high-plasticity magnesium rare earth alloy, comprising the following steps:

[0011] 1) preparing wire according to the chemical element composition of the above-mentioned high-strength and high-plasticity magnesium rare earth alloy;

[0012] 2) Use computer software to perform three-dimensional modeling of the target magnesium rare earth alloy and set additive parameters, and use cold metal transition arc additive equipment to perform additive manufacturing on the wire obtained in step 1) to obtain an additive manufacturing workpiece; in this way, according to the composition of the prepared wire, cold metal transition arc additive manufacturing is specifically used. Since the equipment has the characteristics of short-circuit retraction, it can greatly reduce heat input, effectively reduce the burning of Mg and Al elements, and ensure the consistency of the composition between the wire and the formed part. At the same time, the reduced heat input can reduce the residual stress of the printing process and reduce the abnormal growth of grains after the later heat treatment. At the same time, due to the high efficiency of cold metal transition arc additive manufacturing, the deposition layer is high, and the temperature gradient is increased, which avoids the easy formation of columnar crystals in the previous deposited magnesium alloy, resulting in anisotropy of the finished product.

[0013] 3) The additive manufacturing workpiece obtained in step 2) is placed in a solution treatment at 400-450°C for 2-4 hours, and after cooling to room temperature with water, it is further placed in an aging treatment at 150-250°C for 2-100 hours to obtain a high-strength and high-plasticity magnesium rare earth alloy. The present invention specifically adopts a low-temperature and low-time solution treatment method to ensure the full dissolution of the eutectic phase and the full diffusion of the elements, and inhibits the coarsening and abnormal growth of the grains during the solution, effectively reducing the plastic loss of the material. In the subsequent aging process, a uniformly distributed and dense Mg7Gd nanophase can be precipitated in the crystal, which can significantly improve the mechanical strength. At the same time, during the manufacturing solidification process, thermally stable Al-Zr and Al-Gd phases are generated in turn. These two precipitation phases can play a role in pinning the grain boundaries, improve the thermal stability and strength of the material, and effectively inhibit grain growth.

[0014] Preferably, in step 1), the wire is prepared by the following method:

[0015] S1: preparing raw materials for smelting and casting to obtain a round ingot;

[0016] S2: homogenizing the round ingot obtained in step S1;

[0017] S3: hot extruding the ingot obtained in step S2 to obtain a wire.

[0018] Preferably, the raw material is industrial pure magnesium, Mg-Gd master alloy, Mg-Al master alloy, Mg-Zn master alloy and Mg-Zr master alloy.

[0019] Preferably, the diameter of the wire is φ1.2 mm.

[0020] Preferably, the temperature of the homogenization treatment is 300° C. and the time is 2 to 4 hours; the temperature during the continuous hot extrusion treatment is 250 to 300° C., the extrusion speed is 10 to 20 mm / s, and the extrusion ratio is 15 to 20.

[0021] Preferably, the additive parameters include the position of the robot arm, the path program, the wire feeding speed, the additive manufacturing speed, and the distance between the welding gun tip and the magnesium alloy substrate. Furthermore, the additive manufacturing speed is 6 to 12 mm / s, and the wire feeding speed is 6 to 12 m / s.

[0022] Preferably, inert gas shielded welding is used in the additive manufacturing process; further, the inert gas is pure argon, CO2 or helium, and the gas flow rate of the inert gas is 10 to 25 L / min.

[0023] Preferably, the temperature of the solution treatment is 450° C. and the time is 2 h; the temperature of the aging treatment is 200° C. and the time is 20 h.

[0024] Compared with the prior art, the present invention has the following beneficial effects:

[0025] 1. The magnesium alloy material of the present invention has carried out precise control on the alloy composition and its ratio. Adding a certain amount of Al element to the alloy with a high rare earth content can effectively promote the activation of non-basal slip system (cone I slip and cone II slip, etc.), thereby significantly increasing the plasticity of the wire material, improving the processing performance, and reducing the risk of wire breakage of the magnesium alloy wire material. At the same time, through the interaction between the elements under a specific process, Al2Gd, Al-Zr and other pinning phases and Mg7Gd nanophases are generated. The pinning phase can play a role in pinning the grain boundary, improve the thermal stability and strength of the material, and effectively inhibit the growth of grains. The nanophase can significantly improve the mechanical strength, and the precise control of the Gd / Al element ratio is conducive to balancing strength and plasticity. The tensile strength of the magnesium alloy material of the present invention reaches more than 350MPa, and the elongation can reach 15%, which is a good high-strength and high-plasticity magnesium alloy.

[0026] 2. The present invention selects a combination of cold metal transition arc additive manufacturing technology and solution aging treatment process according to the content ratio of each component of the high-strength magnesium alloy. Since the alloy of the present invention has a high growth limiting factor, the cold metal transition arc additive manufacturing technology is adopted. On the one hand, the low heat input can effectively reduce the burning loss of elements such as Mg and Al, and reduce the deposition thermal stress; on the other hand, the fast cooling rate leads to the maintenance of the solid solubility in the element matrix, effectively reducing the precipitation of the brittle eutectic phase. Then the printed sample is subjected to a low temperature and low time solution treatment method, which can ensure the full dissolution of the eutectic phase and the full diffusion of the elements, and inhibit the coarsening and abnormal growth behavior of the grains during the solution, effectively reducing the plastic loss of the material. In the subsequent aging process, a uniformly distributed and dense Mg7Gd nanophase can be precipitated in the crystal, which can significantly improve the mechanical strength. Therefore, the alloy grain size in the magnesium alloy sample of the present invention is small, there is no abnormal growth after heat treatment, and a large number of nano-level strengthening phases are precipitated in the crystal. Compared with the comparative example, the present invention can simultaneously improve the room temperature plasticity and tensile strength of magnesium alloy products, and can effectively solve the problem of mutual restriction between strength and plastic toughness of magnesium alloys. At the same time, it also provides a new research direction for the preparation of high-performance magnesium alloys, which is of great significance.

[0027] 2. The preparation process of the present invention is simple, the solid solution temperature is low, the production time is short, the cost is low, and it is conducive to industrial large-scale production. Through the combination of material design and the normal organization of the cold metal transition arc, the problem of serious plasticity loss of rare earth magnesium alloy after T5 and T6 heat treatment in arc additive manufacturing is effectively solved, and it has good application prospects and economic benefits. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a physical picture of the magnesium alloy sample prepared in Example 1.

[0029] Figure 2 This is the microscopic TEM image of the magnesium alloy prepared in Example 1.

[0030] Figure 3 The grain map (AC) and grain size distribution map (BD) of the sample in Example 1 before and after heat treatment; AB is before heat treatment, and CD is after heat treatment. DETAILED DESCRIPTION

[0031] The present invention is further described in detail below in conjunction with the examples. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention. In the following examples, if no specific conditions are specified, the conditions are carried out according to conventional conditions or the conditions recommended by the manufacturer. The raw materials, equipment or instruments used, if the manufacturer is not specified, are all conventional products that can be obtained commercially.

[0032] 1. An arc additive manufacturing method based on high-strength and high-plasticity magnesium rare earth alloy

[0033] Example 1

[0034] 1) A high-strength and high-plasticity magnesium rare earth alloy, comprising the following raw materials in mass percentage: Gd 10wt.%, Al 1wt.%, Zr 0.2wt.%, Zn 0.3wt.%, and the balance being magnesium and inevitable impurities. The raw materials are prepared according to the above ingredients, polished to a metallic luster, and weighed for use. The raw materials used are high-purity Mg, Mg-Gd master alloy, Mg-Al master alloy, Mg-Zn master alloy, and Mg-Zr master alloy.

[0035] 2) The weighed raw materials are melted in a vacuum induction furnace at a melting temperature of 730°C, and heated in a dynamic protective atmosphere of a mixed gas of CO2 and SF6 (ratio 99:1), and kept warm for 15 to 20 minutes to form an alloy melt. The magnesium alloy melt is then stirred for 2 minutes, kept warm at 730°C for 10 minutes, and after removing the slag on the surface of the melt, the alloy melt is poured into a low-carbon steel mold preheated at 250°C, cooled to room temperature, and demolded to obtain a magnesium alloy ingot, which is then processed into a 80mm×120mm cylinder.

[0036] 3) The ingot obtained in step 2) is kept at 300°C for 2 hours, cooled to room temperature, and the round ingot is transferred to an extruder. When the extrusion temperature is 250°C, the extrusion speed is 10-20 mm / s, and the extrusion ratio is 15-20, a wire with a diameter of φ1.2 mm is continuously extruded.

[0037] 4) installing the substrate with the oxide scale removed, and loading the wire obtained in step 3) onto the wire feeding mechanism; using a cold metal transition arc additive manufacturing process, and performing unified parameter input based on the Mne21magdium database, the optimal process parameters predetermined for additive manufacturing are related to the wire composition, wherein the additive manufacturing speed is 8 mm / s, the wire feeding speed is 8 m / s, and inert gas protection is adopted. The inert protective gas is pure argon, and the gas flow rate is 20 L / min. Subsequently, the alloy is additively manufactured, and the Mg-Gd-Al-Zr-Zn wire is melted and deposited on the substrate, and layer-by-layer printing is completed.

[0038] 5) Cut and remove the sample printed in step 4), place it in a resistance furnace, first heat the resistance furnace to 450°C, keep it warm for 2 hours, cool it down by water after solution heat treatment, then heat the resistance furnace to 200°C, keep it warm for 80 hours. After the end, take the Mg-Gd-Al-Zr-Zn magnesium alloy sample out of the furnace and air cool it to room temperature.

[0039] Example 2

[0040] 1) A high-strength and high-plasticity magnesium rare earth alloy, comprising the following raw materials in mass percentage: Gd 6wt.%, Al

[0041] 1.5wt.%, Zr 0.2wt.%, Zn 0.3wt.%, the balance is magnesium and inevitable impurities. Prepare the materials according to the above ingredients and polish the raw materials to obtain metallic luster and weigh them for use. The raw materials used are high-purity Mg, Mg-Gd master alloy, Mg-Al master alloy, Mg-Zn master alloy, and Mg-Zr master alloy.

[0042] 2) The weighed raw materials are melted in a vacuum induction furnace at a melting temperature of 730°C, and heated in a dynamic protective atmosphere of a mixed gas of CO2 and SF6 (ratio 99:1), and kept warm for 15 to 20 minutes to form an alloy melt. The magnesium alloy melt is then stirred for 2 minutes, kept warm at 730°C for 10 minutes, and after removing the slag on the surface of the melt, the alloy melt is poured into a low-carbon steel mold preheated at 250°C, cooled to room temperature, and demolded to obtain a magnesium alloy ingot, which is then processed into a 80mm×120mm cylinder.

[0043] 3) The ingot obtained in step 2) is kept at 300°C for 2 hours, cooled to room temperature, and the round ingot is transferred to an extruder. When the extrusion temperature is 250°C, the extrusion speed is 10-20 mm / s, and the extrusion ratio is 15-20, a wire with a diameter of φ1.2 mm is continuously extruded.

[0044] 4) installing the substrate with the oxide scale removed, and loading the wire obtained in step 3) onto the wire feeding mechanism; using a cold metal transition arc additive manufacturing process, and performing unified parameter input based on the Mne21magdium database, the optimal process parameters predetermined for additive manufacturing are related to the wire composition, wherein the additive manufacturing speed is 9 mm / s, the wire feeding speed is 9 m / s, and inert gas protection is adopted. The inert protective gas is pure argon, and the gas flow rate is 20 L / min. Subsequently, the alloy is additively manufactured, and the Mg-Gd-Al-Zr-Zn wire is melted and deposited on the substrate, and layer-by-layer printing is completed.

[0045] 5) Cut and remove the sample printed in step 4), place it in a resistance furnace, first heat the resistance furnace to 450°C, keep it warm for 2 hours, cool it down by water after solution heat treatment, then heat the resistance furnace to 200°C, keep it warm for 20 hours. After the end, take out the Mg-Gd-Al-Zr-Zn magnesium alloy sample from the furnace and air cool it to room temperature.

[0046] Example 3

[0047] 1) A high-strength and high-plasticity magnesium rare earth alloy, comprising the following raw materials in mass percentage: Gd 12wt.%, Al 2wt.%, Zr 0.5wt.%, Zn 0.3wt.%, and the remainder being magnesium and inevitable impurities. The raw materials are prepared according to the above ingredients and polished to a metallic luster and weighed for use. The raw materials used are high-purity Mg, Mg-Gd master alloy, Mg-Al master alloy, Mg-Zn master alloy, and Mg-Zr master alloy.

[0048] 2) The weighed raw materials are melted in a vacuum induction furnace at a melting temperature of 730°C, and heated in a dynamic protective atmosphere of a mixed gas of CO2 and SF6 (ratio 99:1), and kept warm for 15 to 20 minutes to form an alloy melt. The magnesium alloy melt is then stirred for 2 minutes, kept warm at 730°C for 10 minutes, and after removing the slag on the surface of the melt, the alloy melt is poured into a low-carbon steel mold preheated at 250°C, cooled to room temperature, and demolded to obtain a magnesium alloy ingot, which is then processed into a 80mm×120mm cylinder.

[0049] 3) The ingot obtained in step 2) is kept at 300°C for 2 hours, cooled to room temperature, and the round ingot is transferred to an extruder. When the extrusion temperature is 250°C, the extrusion speed is 10-20 mm / s, and the extrusion ratio is 15-20, a wire with a diameter of φ1.2 mm is continuously extruded.

[0050] 4) installing the substrate with the oxide scale removed, and loading the wire obtained in step 3) onto the wire feeding mechanism; using a cold metal transition arc additive manufacturing process, and performing unified parameter input based on the Mne21magdium database, the optimal process parameters predetermined for additive manufacturing are related to the wire composition, wherein the additive manufacturing speed is 12 mm / s, the wire feeding speed is 12 m / s, and inert gas protection is adopted, the inert protective gas is pure argon, and the gas flow rate is 20 L / min, and then the alloy is additively manufactured, the Mg-Gd-Al-Zr-Zn wire is melted and deposited on the substrate, and layer-by-layer printing is completed.

[0051] 5) Cut and remove the sample printed in step 4), place it in a resistance furnace, heat the resistance furnace to 450°C, keep it warm for 4 hours, cool it down by water after solution heat treatment, then heat the resistance furnace to 175°C, keep it warm for 90 hours. After the end, take out the Mg-Gd-Al-Zr-Zn magnesium alloy sample from the furnace and air cool it to room temperature.

[0052] Comparative Example 1

[0053] No Al element was added to the raw materials, and other raw materials and steps were the same as in Example 1.

[0054] Comparative Example 2

[0055] The arc additive process is replaced by a casting process, and other raw materials and steps are the same as in Example 1.

[0056] Comparative Example 3

[0057] The solution treatment temperature is 500° C., the treatment time is 12 h, and the other raw materials and steps are the same as in Example 1.

[0058] Comparative Example 4

[0059] The alloy composition is Gd 5wt.%, Al 12wt.%, Zr 0.5wt.%, Zn 0.3wt.%, and the balance is magnesium and inevitable impurities. Other steps are the same as Example 1.

[0060] 2. Performance Verification

[0061] 1. The morphology of the magnesium alloy sample after heat treatment in Example 1 was observed under a scanning microscope. The results are as follows: Figure 1 shown.

[0062] It can be seen from the figure that there are a large number of continuous ellipsoidal nano-precipitated phase β′ phase in the crystal of the magnesium alloy sample. This phase is the main strengthening phase in the Mg-Gd alloy, which can effectively hinder dislocation movement and improve mechanical strength.

[0063] 2. Electron backscatter diffraction (EBSD) analysis was performed on the magnesium alloy samples before and after the solution + aging heat treatment in Example 1 under a scanning electron microscope. The results are as follows: Figure 2 shown.

[0064] It can be seen from the figure that the grain size of the magnesium alloy sample before solution + aging heat treatment is about 14.7μm, while after solution + aging heat treatment, the grain length is only about 4μm, and there is no abnormal growth phenomenon. In addition, a large amount of precipitated phases precipitate in the crystal of the magnesium alloy sample after heat treatment. This fully demonstrates that the alloy can fully precipitate the strengthening phase under the designed heat treatment system and greatly avoid excessive grain coarsening and abnormal grain growth.

[0065] 3. The magnesium alloy components prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were subjected to uniaxial tensile tests according to GB / T 228.1 2010 room temperature tensile test needle, and their grain structures were observed and their mechanical properties at room temperature were tested. The test results are shown in Table 1:

[0066] Table 1

[0067]

[0068]

[0069] As can be seen from Table 1, the alloy grain size in the magnesium alloy sample obtained in the embodiment of the present invention is small, there is no abnormal growth, and a large number of nano-level strengthening phases are precipitated in the crystal, which significantly improves its tensile strength without significantly damaging the plasticity of the alloy. However, the grains of the magnesium alloy sample in Comparative Example 1 are relatively large after solidification, and the ductility after heat treatment is low. Compared with before heat treatment, the ductility is lost by 50%, which is due to the lack of effective pinning phases such as Al2Gd and Al-Zr in the alloy. At the same time, the welding wire manufactured in Comparative Example 1 has multiple wire breaks during the forming process, and there are multiple interfaces in one coil of wire. The alloy grains of the magnesium alloy sample in Comparative Example 2 are larger, which is caused by the low solidification rate of the cast alloy, which causes a decrease in room temperature strength and plasticity. After heat treatment, the eutectic phase at the grain boundary fails to dissolve, which will induce fracture at the grain boundary during stretching, which is not conducive to ductility. The alloy grains of the magnesium alloy sample in Comparative Example 3 were significantly coarsened after a high heat treatment, and some abnormally grown grains appeared, which led to stress concentration in the alloy and damaged the plasticity of the alloy. This shows that the solid solution treatment at a lower temperature and for a shorter time in the present invention has indeed improved the plasticity of the alloy. The tensile strength and plasticity of the magnesium alloy in Comparative Example 4 are both low. This is because the addition of excessive Al elements leads to the precipitation of excessive heat-resistant phase Al2Gd, which reduces the plasticity of the component after heat treatment. At the same time, the Al elements that have not been completely consumed react with the Mg elements to form a brittle Mg-Al phase, which loses the strength of the component. This shows that the precise control of the Gd / Al element ratio in the present invention is beneficial to balancing strength and plasticity.

[0070] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. An arc additive manufacturing method based on high-strength and high-plasticity magnesium rare earth alloy, characterized in that: The magnesium rare earth alloy comprises the following raw materials in mass percentage: Gd 6-12 wt.%, Al 0.5-2 wt.%, Zr 0.2-0.5 wt.%, Zn 0.1-0.3 wt.%, and the balance is magnesium and unavoidable impurities, and the mass ratio of Gd to Al is 4-10:1; The preparation method of the magnesium rare earth alloy comprises the following steps: 1) preparing wire according to the chemical element composition of the high-strength and high-plasticity magnesium rare earth alloy; 2) Using computer software to perform three-dimensional modeling of the target magnesium rare earth alloy and set additive parameters, then loading the wire obtained in step 1) onto a wire feeding mechanism, and using a cold metal transition arc additive device to perform additive manufacturing to obtain an additively manufactured workpiece; 3) The additively manufactured workpiece obtained in step 2) is subjected to solution treatment at 400-450°C for 2-4 h, cooled to room temperature by water, and then subjected to aging treatment at 150-250°C for 20-100 h to obtain a high-strength and high-plasticity magnesium rare earth alloy.

2. The arc additive manufacturing method of high-strength and high-plasticity magnesium rare earth alloy according to claim 1, characterized in that: In step 1), the wire material is prepared by the following method: S1: preparing raw materials for smelting and casting to obtain a round ingot; S2: homogenizing the round ingot obtained in step S1; S3: The ingot obtained in step S2 is subjected to continuous hot extrusion treatment to obtain a wire.

3. The arc additive manufacturing method of high-strength and high-plasticity magnesium rare earth alloy according to claim 2, characterized in that: The raw materials are industrial pure magnesium, Mg-Gd master alloy, Mg-Al master alloy, Mg-Zn master alloy and Mg-Zr master alloy.

4. The arc additive manufacturing method of high-strength and high-plasticity magnesium rare earth alloy according to claim 1, characterized in that: The diameter of the wire is φ1.2 mm.

5. The arc additive manufacturing method of high-strength and high-plasticity magnesium rare earth alloy according to claim 2, characterized in that: The temperature of the homogenization treatment is 300° C. and the time is 2-4 hours; the temperature during the continuous hot extrusion treatment is 250-300° C., the extrusion speed is 10-20 mm / s, and the extrusion ratio is 15-20.

6. The arc additive manufacturing method of high-strength and high-plasticity magnesium rare earth alloy according to claim 1, characterized in that: The additive parameters include a robot arm position, a path program, a wire feeding speed, an additive manufacturing speed, and a distance between a welding gun tip and a magnesium alloy substrate.

7. The arc additive manufacturing method of high-strength and high-plasticity magnesium rare earth alloy according to claim 6, characterized in that: The additive manufacturing speed is 6~12 mm / s, and the wire feeding speed is 6~12 m / s.

8. The arc additive manufacturing method of high-strength and high-plasticity magnesium rare earth alloy according to claim 1, characterized in that: In the additive manufacturing process, inert gas shielded welding is required; the inert gas is argon, CO2 or helium, and the gas flow rate of the inert gas is 10~25 L / min.

9. The arc additive manufacturing method of high-strength and high-plasticity magnesium rare earth alloy according to claim 1, characterized in that: The temperature of the solution treatment is 450°C and the time is 2h; the temperature of the aging treatment is 200°C and the time is 20h.

Citation Information

Patent Citations

  • Electric arc additive manufacturing method of Mg-Y-Nd-Zr rare earth magnesium alloy structural member

    CN116618792A

  • Heatproof magnesium alloy

    CN102994847A

  • High-strength and -toughness rare earth magnesium alloy and preparation method thereof

    CN104651692A

  • High-modulus magnesium alloy and preparation method thereof

    CN109161770A

  • Rare earth magnesium alloy wire suitable for electric arc additive manufacturing and preparation method of rare earth magnesium alloy wire

    CN114717458A