A method for reducing internal stress of soft magnetic composite material and annealing device thereof

The magnetic ring is prepared by the hot pressing process and the rotary drive assembly and air intake pipe design is used during the annealing process, which reduces the internal stress of the soft magnetic composite material and improves the magnetic performance of the magnetic ring.

CN118237585BActive Publication Date: 2024-11-15SHANDONG HENGRUI MAGNET TECH CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202410388987.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-01
Publication Date
2024-11-15
Estimated Expiration
2044-04-01

AI Technical Summary

Technical Problem

The internal stress introduced by soft magnetic composites during the preparation process hinders the magnetization process, resulting in a decrease in magnetic permeability and an increase in hysteresis loss, and requires high-temperature annealing to reduce internal stress.

Method used

The magnetic ring is prepared by hot pressing process, and the magnetic ring is rotated and moved up and down in the annular heating chamber by rotating the drive assembly during the annealing process. Combined with the design of the intake pipe and insulation particles, uniform heating and temperature are achieved inside and outside the magnetic ring. Stablize.

Benefits of technology

It improves the annealing effect, reduces the internal stress of soft magnetic composite materials, and improves the magnetic performance of the magnetic ring.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118237585B_ABST
    Figure CN118237585B_ABST
Patent Text Reader

Abstract

The invention discloses a method for reducing the internal stress of a soft magnetic composite material and an annealing device thereof, and relates to the field of annealing technology. The method comprises: 1) mixing a passivator with any one of Fe, SiFe2, FeSiAl or Fe3.5Si4.5Cr magnetic powder, stirring and drying to obtain a passivation powder; 2) loading the passivation powder into a forming mold, and pressing it into a magnetic ring by a hot pressing process, and the hot pressing temperature is 400°C-800°C; 3) opening a sealing cover body and placing the magnetic ring on a support frame, and then closing the sealing cover body and pumping the annular heating chamber to a vacuum state through an air outlet pipe, and the annealing device comprises a hollow tube and a heating mechanism, wherein the hollow tube comprises an outer tube and an inner tube, and one end of the inner tube is sealed. The magnetic ring of the invention can be coaxially placed in the annular heating chamber, and then the inner and outer sides of the magnetic ring are synchronously heated by the inner and outer sides of the first heating component and the second heating component, so that the inner and outer sides of the magnetic ring are heated evenly, the annealing effect is improved, and the effect of removing internal stress is correspondingly improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of annealing, in particular to a method for reducing internal stress of a soft magnetic composite material and an annealing device thereof. Background Art

[0002] A lot of internal stress will be introduced in the preparation process of soft magnetic composite materials, especially in the pressing process. If the magnetic powder is prepared by ball milling, a lot of internal stress will also be generated. The existence of internal stress will hinder the movement of domain walls during magnetization, reduce magnetic permeability, increase hysteresis loss, and be detrimental to the magnetic properties of soft magnetic composite materials. Therefore, high temperature annealing heat treatment is required to reduce internal stress. Summary of the invention

[0003] The object of the present invention is to provide a method for reducing the internal stress of a soft magnetic composite material and an annealing device thereof, so as to solve the problems raised in the above background technology.

[0004] In order to achieve the above-mentioned invention object, the present invention adopts the following technical scheme:

[0005] The present invention provides a method for reducing the internal stress of a soft magnetic composite material, comprising the following steps:

[0006] 1) Mix the passivating agent with any one of Fe, SiFe2, FeSiAl or Fe3.5Si4.5Cr magnetic powder, stir and dry to obtain passivating powder;

[0007] 2) The passivation powder is loaded into a molding die and pressed into a magnetic ring by hot pressing at a temperature of 400°C-800°C;

[0008] 3) Open the sealing cover and place the magnetic ring on the support frame, then close the sealing cover and evacuate the annular heating chamber to a vacuum state through the air outlet pipe;

[0009] 4) Introduce protective gas into the annular heating chamber through the air inlet manifold, and start the heating mechanism. After heating to 400°C at a heating rate of 2°C / min, keep warm for 1 hour, then continue to heat to 770°C at a rate of 5°C / min, and keep warm at 770°C for 3 hours. During the heating period, start the rotary drive assembly to drive the outer tube to rotate forward and reverse, so that the support frame drives the magnetic ring to rotate in the annular heating chamber and continuously move up and down;

[0010] 5) Turn off the heating mechanism and continue to introduce protective gas until the annular heating chamber cools to room temperature;

[0011] 6) The outer tube is driven to rotate by the rotary drive assembly so that the support frame drives the magnetic ring to move up to the top of the annular heating chamber, and then the cover is opened to take out the magnetic ring.

[0012] Furthermore, in step 2), pre-pressing is first performed with a pressure of 60 kN for 30 seconds, and then the pressure is maintained at a pressure of 100 kN for 1 minute.

[0013] Furthermore, before the passivation powder is loaded into the molding die, a lubricant is added into the passivation powder and mixed evenly, wherein the lubricant accounts for 0.5wt% of the mass of the passivation powder.

[0014] An annealing device for reducing the internal stress of a soft magnetic composite material, the annealing device comprising a hollow tube and a heating mechanism, the hollow tube comprising an outer tube and an inner tube, one end of the inner tube is sealed, the edge of the other end of the inner tube is bent outward to extend to form a connecting portion, the outer tube is coaxially arranged with the inner tube, one end of the outer tube is connected to the connecting portion, the other end of the outer tube is provided with a sealing cover body, the outer tube, the inner tube and the sealing cover body are surrounded to form a sealed annular heating chamber;

[0015] The heating mechanism comprises a first heating component arranged on the inner side of the inner tube, and a second heating component arranged on the outer side of the outer tube;

[0016] An air outlet pipe is arranged at the center of the sealing cover body, and an air intake main pipe is also arranged through the center of the first heating component. One end of the air intake main pipe passes through the sealed end of the inner tube and extends into the annular heating cavity. Air intake branch pipes are evenly arranged along the circumferential direction on the outside of the air intake main pipe in the annular heating cavity, and the other end of the air intake branch pipes extends to one end of the annular heating cavity close to the connecting portion.

[0017] Furthermore, the annealing device also includes a shell and a rotation drive assembly, the hollow tube vertically penetrates the shell, and the outer tube and the shell are rotationally connected, the rotation drive assembly is used to drive the outer tube to rotate, and a rotary joint is arranged on the air outlet pipe.

[0018] Furthermore, the air intake branch pipe includes a connecting section connected to the air intake main pipe, and a spiral section connected to the connecting section and spirally wound around the outer side of the inner pipe, and the interior of the air intake branch pipe is filled with thermal insulation particles.

[0019] Furthermore, the connecting portion is connected to the outer tube via a rotating sealing joint, a clamping piece is provided on the connecting portion, and the clamping piece is fixedly connected to the bottom end of the shell via a support rod; a supporting frame is also provided inside the annular heating chamber, the supporting frame comprises a movable ring which is slidably matched with the outer tube and can only slide along the axial direction of the outer tube, and a plurality of supporting rods inclined toward one side of the sealing cover body assembly, the number of the supporting rods is equal to that of the air inlet branch pipe, and the other end of the supporting rod away from the movable ring has a lap portion lapped on the corresponding spiral segment.

[0020] Compared with the prior art, one or more of the above technical solutions have the following beneficial effects:

[0021] 1. The magnetic ring of the present invention can be coaxially placed in an annular heating chamber, and then the inner and outer sides of the magnetic ring are synchronously heated by the first heating component and the second heating component, so that the inner and outer sides of the magnetic ring are heated evenly, the annealing effect is improved, and the effect of removing internal stress is correspondingly improved.

[0022] 2. The spiral section of the air inlet branch pipe of the present invention can prolong the time of gas transmission, so that the gas can be fully heated before contacting the magnetic ring, avoiding the contact between cold gas and the magnetic ring to damage the magnetic ring structure. The setting of the thermal insulation particles can absorb heat. When the temperature in the box rises, the heat is collected first. When annealing, the temperature will not drop suddenly, avoiding damage to the internal structure of the magnetic ring and increasing the thermal insulation effect.

[0023] 3. The support bracket of the present invention can automatically position the magnetic ring at the center of the annular heating chamber, and can make the magnetic ring rotate circumferentially in the annular heating chamber and move axially at the same time through the forward and reverse rotation of the outer tube, further, making the magnetic ring heated evenly.

[0024] It is to be understood that the foregoing general description and the following detailed description are exemplary and explanatory only and are not restrictive of the invention. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] The accompanying drawings in the specification, which constitute a part of the present invention, are used to provide a further understanding of the present invention. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute improper limitations on the present invention.

[0026] Figure 1 It is a schematic diagram of the structure of the present invention;

[0027] Figure 2 It is a schematic diagram of the structure of the present invention;

[0028] Figure 3 It is a schematic diagram of the structure of the present invention;

[0029] Figure 4 It is a structural schematic diagram of the present invention.

[0030] In the figure:

[0031] 100, hollow tube; 110, outer tube; 120, inner tube; 121, connecting portion; 130, sealing cover; 140, annular heating chamber; 210, first heating component; 220, second heating component; 310, air outlet pipe; 320, air inlet main pipe; 330, air inlet branch pipe; 331, connecting section; 332, spiral section; 400, shell; 500, support bracket; 510, movable ring; 520, support rod; 521, overlapping portion. DETAILED DESCRIPTION

[0032] In order to enable those skilled in the art to better understand the solution of the present application, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are only part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without creative work should fall within the scope of protection of the present application.

[0033] Embodiment 1, the present invention provides a method for reducing the internal stress of a soft magnetic composite material, comprising the following steps:

[0034] 1) The passivator and Fe are mixed, stirred and dried to obtain a passivation powder, and a lubricant is added to the passivation powder and mixed evenly, wherein the lubricant accounts for 0.5wt% of the passivation powder;

[0035] 2) The passivation powder is loaded into a molding die and pressed into a magnetic ring by a hot pressing process at a temperature of 400°C. In the hot pressing process, a pre-pressing pressure of 60 kN is first used for 30 seconds to remove the air between the particles, and then the pressure is maintained at 100 kN for 1 minute to press into a ring-shaped soft magnetic composite material with an inner diameter of 5.5 mm, an outer diameter of 9.7 mm, and a thickness of 3.3 mm;

[0036] 3) Open the sealing cover 130 and place the magnetic ring on the support frame 500, then close the sealing cover 130 and evacuate the annular heating chamber 140 to a vacuum state through the air outlet pipe 310;

[0037] 4) A protective gas is introduced into the annular heating chamber 140 through the air inlet manifold 320, and the heating mechanism is started. The temperature is raised to 400°C at a heating rate of 2°C / min, and then kept at that temperature for 1 hour. The temperature is then further raised to 770°C at a rate of 5°C / min, and kept at that temperature for 3 hours. During the heating period, the rotation drive assembly is started to drive the outer tube 110 to rotate forward and reverse, so that the support bracket 500 drives the magnetic ring to rotate in the annular heating chamber 140 and continuously move up and down;

[0038] 5) Turn off the heating mechanism and continue to introduce protective gas until the annular heating chamber 140 cools to room temperature;

[0039] 6) After the outer tube 110 is driven to rotate by the rotary drive assembly so that the support bracket 500 drives the magnetic ring to move up to the top of the annular heating chamber 140, the cover is opened to take out the magnetic ring.

[0040] Embodiment 2, the present invention provides a method for reducing the internal stress of a soft magnetic composite material, comprising the following steps:

[0041] 1) The passivator and SiFe2 are mixed, stirred and dried to obtain a passivation powder, and a lubricant is added to the passivation powder and mixed evenly, wherein the lubricant accounts for 0.5wt% of the passivation powder;

[0042] 2) The passivation powder is loaded into a molding die and pressed into a magnetic ring by a hot pressing process at a temperature of 400°C. In the hot pressing process, a pre-pressing pressure of 60 kN is first used for 30 seconds to remove the air between the particles, and then the pressure is maintained at 100 kN for 1 minute to press into a ring-shaped soft magnetic composite material with an inner diameter of 5.5 mm, an outer diameter of 9.7 mm, and a thickness of 3.3 mm;

[0043] 3) Open the sealing cover 130 and place the magnetic ring on the support bracket 500, then close the sealing cover 130 and evacuate the annular heating chamber 140 to a vacuum state through the air outlet pipe 310;

[0044] 4) A protective gas is introduced into the annular heating chamber 140 through the air inlet manifold 320, and the heating mechanism is started. The temperature is raised to 400°C at a heating rate of 2°C / min, and then kept at this temperature for 1 hour. The temperature is then further raised to 770°C at a rate of 5°C / min, and kept at this temperature for 3 hours. During the heating period, the rotation drive assembly is started to drive the outer tube 110 to rotate forward and reverse, so that the support bracket 500 drives the magnetic ring to rotate in the annular heating chamber 140 and continuously move up and down;

[0045] 5) Turn off the heating mechanism and continue to introduce protective gas until the annular heating chamber 140 cools to room temperature;

[0046] 6) After the outer tube 110 is driven to rotate by the rotary drive assembly so that the support bracket 500 drives the magnetic ring to move up to the top of the annular heating chamber 140, the cover is opened to take out the magnetic ring.

[0047] Embodiment 3, the present invention provides a method for reducing the internal stress of a soft magnetic composite material, comprising the following steps:

[0048] 1) The passivator and FeSiAl are mixed, stirred and dried to obtain a passivation powder, and a lubricant is added to the passivation powder and mixed evenly, wherein the lubricant accounts for 0.5wt% of the passivation powder;

[0049] 2) The passivation powder is loaded into a molding die and pressed into a magnetic ring by a hot pressing process at a temperature of 400°C. In the hot pressing process, a pre-pressing pressure of 60 kN is first used for 30 seconds to remove the air between the particles, and then the pressure is maintained at 100 kN for 1 minute to press into a ring-shaped soft magnetic composite material with an inner diameter of 5.5 mm, an outer diameter of 9.7 mm, and a thickness of 3.3 mm;

[0050] 3) Open the sealing cover 130 and place the magnetic ring on the support bracket 500, then close the sealing cover 130 and evacuate the annular heating chamber 140 to a vacuum state through the air outlet pipe 310;

[0051] 4) A protective gas is introduced into the annular heating chamber 140 through the air inlet manifold 320, and the heating mechanism is started. The temperature is raised to 400°C at a heating rate of 2°C / min, and then kept at this temperature for 1 hour. The temperature is then further raised to 770°C at a rate of 5°C / min, and kept at this temperature for 3 hours. During the heating period, the rotation drive assembly is started to drive the outer tube 110 to rotate forward and reverse, so that the support bracket 500 drives the magnetic ring to rotate in the annular heating chamber 140 and continuously move up and down;

[0052] 5) Turn off the heating mechanism and continue to introduce protective gas until the annular heating chamber 140 cools to room temperature;

[0053] 6) After the outer tube 110 is driven to rotate by the rotary drive assembly so that the support bracket 500 drives the magnetic ring to move up to the top of the annular heating chamber 140, the cover is opened to take out the magnetic ring.

[0054] Embodiment 4, the present invention provides a method for reducing the internal stress of a soft magnetic composite material, comprising the following steps:

[0055] 1) The passivator is mixed with Fe3.5Si4.5Cr, stirred and dried to obtain a passivation powder, and a lubricant is added to the passivation powder and mixed evenly, wherein the lubricant accounts for 0.5wt% of the passivation powder;

[0056] 2) The passivation powder is loaded into a molding die and pressed into a magnetic ring by a hot pressing process at a temperature of 400°C. In the hot pressing process, a pre-pressing pressure of 60 kN is first used for 30 seconds to remove the air between the particles, and then the pressure is maintained at 100 kN for 1 minute to press into a ring-shaped soft magnetic composite material with an inner diameter of 5.5 mm, an outer diameter of 9.7 mm, and a thickness of 3.3 mm;

[0057] 3) Open the sealing cover 130 and place the magnetic ring on the support bracket 500, then close the sealing cover 130 and evacuate the annular heating chamber 140 to a vacuum state through the air outlet pipe 310;

[0058] 4) A protective gas is introduced into the annular heating chamber 140 through the air inlet manifold 320, and the heating mechanism is started. The temperature is raised to 400°C at a heating rate of 2°C / min, and then kept at this temperature for 1 hour. The temperature is then further raised to 770°C at a rate of 5°C / min, and kept at this temperature for 3 hours. During the heating period, the rotation drive assembly is started to drive the outer tube 110 to rotate forward and reverse, so that the support bracket 500 drives the magnetic ring to rotate in the annular heating chamber 140 and continuously move up and down;

[0059] 5) Turn off the heating mechanism and continue to introduce protective gas until the annular heating chamber 140 cools to room temperature;

[0060] 6) After the outer tube 110 is driven to rotate by the rotary drive assembly so that the support bracket 500 drives the magnetic ring to move up to the top of the annular heating chamber 140, the cover is opened to take out the magnetic ring.

[0061] Embodiment 5, the present invention provides a method for reducing the internal stress of a soft magnetic composite material, comprising the following steps:

[0062] 1) The passivator and Fe are mixed, stirred and dried to obtain a passivation powder, and a lubricant is added to the passivation powder and mixed evenly, wherein the lubricant accounts for 0.5wt% of the passivation powder;

[0063] 2) The passivation powder is loaded into a molding die and pressed into a magnetic ring by a hot pressing process at a temperature of 600°C. In the hot pressing process, a pre-pressing pressure of 60 kN is first used for 30 seconds to remove the air between the particles, and then the pressure is maintained at 100 kN for 1 minute to press into a ring-shaped soft magnetic composite material with an inner diameter of 5.5 mm, an outer diameter of 9.7 mm, and a thickness of 3.3 mm;

[0064] 3) Open the sealing cover 130 and place the magnetic ring on the support bracket 500, then close the sealing cover 130 and evacuate the annular heating chamber 140 to a vacuum state through the air outlet pipe 310;

[0065] 4) A protective gas is introduced into the annular heating chamber 140 through the air inlet manifold 320, and the heating mechanism is started. The temperature is raised to 400°C at a heating rate of 2°C / min, and then kept at this temperature for 1 hour. The temperature is then further raised to 770°C at a rate of 5°C / min, and kept at this temperature for 3 hours. During the heating period, the rotation drive assembly is started to drive the outer tube 110 to rotate forward and reverse, so that the support bracket 500 drives the magnetic ring to rotate in the annular heating chamber 140 and continuously move up and down;

[0066] 5) Turn off the heating mechanism and continue to introduce protective gas until the annular heating chamber 140 cools to room temperature;

[0067] 6) After the outer tube 110 is driven to rotate by the rotary drive assembly so that the support bracket 500 drives the magnetic ring to move up to the top of the annular heating chamber 140, the cover is opened to take out the magnetic ring.

[0068] Embodiment 6, the present invention provides a method for reducing the internal stress of a soft magnetic composite material, comprising the following steps:

[0069] 1) The passivator and FeSiAl are mixed, stirred and dried to obtain a passivation powder, and a lubricant is added to the passivation powder and mixed evenly, wherein the lubricant accounts for 0.5wt% of the passivation powder;

[0070] 2) The passivation powder is loaded into a molding die and pressed into a magnetic ring by a hot pressing process at a temperature of 800°C. In the hot pressing process, a pre-pressing pressure of 60 kN is first used for 30 seconds to remove the air between the particles, and then the pressure is maintained at 100 kN for 1 minute to press into a ring-shaped soft magnetic composite material with an inner diameter of 5.5 mm, an outer diameter of 9.7 mm, and a thickness of 3.3 mm;

[0071] 3) Open the sealing cover 130 and place the magnetic ring on the support bracket 500, then close the sealing cover 130 and evacuate the annular heating chamber 140 to a vacuum state through the air outlet pipe 310;

[0072] 4) A protective gas is introduced into the annular heating chamber 140 through the air inlet manifold 320, and the heating mechanism is started. The temperature is raised to 400°C at a heating rate of 2°C / min, and then kept at this temperature for 1 hour. The temperature is then further raised to 770°C at a rate of 5°C / min, and kept at this temperature for 3 hours. During the heating period, the rotation drive assembly is started to drive the outer tube 110 to rotate forward and reverse, so that the support bracket 500 drives the magnetic ring to rotate in the annular heating chamber 140 and continuously move up and down;

[0073] 5) Turn off the heating mechanism and continue to introduce protective gas until the annular heating chamber 140 cools to room temperature;

[0074] 6) After the outer tube 110 is driven to rotate by the rotary drive assembly so that the support bracket 500 drives the magnetic ring to move up to the top of the annular heating chamber 140, the cover is opened to take out the magnetic ring.

[0075] like Figure 1-Figure 4As shown, the present invention also provides an annealing device for the above-mentioned method of reducing the internal stress of the soft magnetic composite material, the annealing device includes a hollow tube 100 and a heating mechanism, the hollow tube 100 includes an outer tube 110 and an inner tube 120, one end of the inner tube 120 is sealed, and the edge of the other end of the inner tube 120 is bent outward and extended to form a connecting portion 121, the outer tube 110 and the inner tube 120 are coaxially arranged, and one end of the outer tube 110 is connected to the connecting portion 121, and the other end of the outer tube 110 is provided with a sealing cover body 130, and the outer tube 110, the inner tube 120 and the sealing cover body 130 are surrounded to form a sealed annular heating chamber 140; the heating The heat mechanism includes a first heating assembly 210 disposed on the inner side of the inner tube 120, and a second heating assembly 220 disposed on the outer side of the outer tube 110; an air outlet pipe 310 is disposed at the center of the sealing cover 130, and an air intake manifold 320 is also penetrated through the center of the first heating assembly 210, one end of the air intake manifold 320 penetrates the sealed end of the inner tube 120 and extends into the annular heating chamber 140, and air intake branch pipes 330 are uniformly disposed along the circumferential direction on the outer side of the air intake manifold 320 located in the annular heating chamber 140, and the other end of the air intake branch pipe 330 extends to one end of the annular heating chamber 140 near the connecting portion 121. When in use, the first heating assembly 210 and the second heating assembly 220 heat the annular heating chamber 140, and since the magnetic ring is coaxially placed in the annular heating chamber 140, the inside and outside of the magnetic ring can be heated evenly, thereby improving the annealing effect and correspondingly improving the effect of removing internal stress. In a specific embodiment of the present invention, the first heating component 210 and the second heating component 220 can be heating tubes and electric heating wires, and the outlet pipe 310 and the air inlet manifold 320 are connected to the air pump and the air supply source respectively, and valves can be provided on the air inlet manifold 320 and the outlet pipe 310, and the opening and closing of the air inlet manifold 320 and the air outlet pipe 310 can be controlled by the valves, so that during the annealing process, a protective gas can be introduced into the annular reinforcement cavity through the air inlet manifold 320. The specific protective gas can be nitrogen. Nitrogen as an insulating gas can prevent the magnetic ring from coming into contact with the air and being oxidized. At the same time, during the process of introducing the protective gas, the first heating component 210 and the second heating component 220 can also preheat the gas flowing in the air inlet branch pipe 330 and the air inlet branch pipe 330 to prevent the cold gas from coming into contact with the magnetic ring and damaging the magnetic ring structure.

[0076] In this specific embodiment, the annealing device further includes a shell 400 and a rotation drive assembly (not shown), the hollow tube 100 vertically penetrates the shell 400, and the outer tube 110 is rotationally connected to the shell 400, the rotation drive assembly is used to drive the outer tube 110 to rotate, and a rotary joint is provided on the outlet pipe 310. Based on the above design, the hollow tube 100 can be driven to rotate by the rotation drive assembly, so that the magnetic ring rotates inside the heating chamber, further making the magnetic ring evenly heated and improving its internal stress relief effect.

[0077] In a specific embodiment of the present invention, the air intake branch pipe 330 includes a connecting section 331 connected to the air intake main pipe 320, and a spiral section 332 connected to the connecting section 331 and spirally wound around the outer side of the inner tube 120, and the interior of the air intake branch pipe 330 is filled with heat-insulating particles. Based on the above design, the spiral section 332 can extend the path during gas transmission, so that the gas can be fully heated before contacting the magnetic ring, avoiding the contact between the cold gas and the magnetic ring to damage the magnetic ring structure, and the setting of the heat-insulating particles can absorb heat. When the temperature in the box rises, the heat is first collected. When annealing, the heat-insulating particles release heat, and the temperature will not drop suddenly through the flow of gas, avoiding damage to the internal structure of the magnetic ring, and increasing the heat-insulating effect.

[0078] In a specific embodiment of the present invention, the connecting portion 121 is connected to the outer tube 110 via a rotary sealing joint, a clamping piece is provided on the connecting portion 121, and the clamping piece is fixedly connected to the bottom end of the shell 400 via a support rod; a support frame 500 is also provided inside the annular heating chamber 140, and the support frame 500 includes a movable ring 510 that slides with the outer tube 110 and can only slide axially along the outer tube 110, and a plurality of supporting rods 520 inclined toward one side of the sealing cover body 130 assembly, the number of the supporting rods 520 is equal to the number of the air inlet branch pipe 330, and the other end of the supporting rod 520 away from the movable ring 510 has a lap portion 521 lapped on the corresponding spiral segment 332. Based on the above design, when the magnetic ring is placed on the supporting rod 520 of the supporting bracket 500, the magnetic ring will slide along the supporting rod 520 and automatically position itself at the center of the annular heating chamber 140, so that the magnetic ring is heated evenly during the heating process, and when the rotating drive assembly drives the outer tube 110 to rotate, the supporting bracket 500 will rotate accordingly, thereby driving the magnetic ring to rotate inside the annular heating chamber 140. During this process, since the supporting rod 520 is positioned by overlapping the spiral section 332 with the overlapping portion 521, when the supporting bracket 500 is rotating, under the action of gravity, the supporting bracket 500 can also move axially in the annular heating chamber 140, that is, through the forward and reverse rotation of the outer tube 110, the magnetic ring can not only rotate circumferentially in the annular heating chamber 140, but also move axially in the annular heating chamber 140 at the same time, further, the magnetic ring is heated evenly.

[0079] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. A method for reducing internal stress of a soft magnetic composite material, characterized in that: The steps include: 1) Mix the passivating agent with any one of Fe, SiFe2, FeSiAl or Fe3.5Si4.5Cr magnetic powder, stir and dry to obtain passivating powder; The passivation powder is loaded into a forming mold and pressed into a magnetic ring by a hot pressing process at a temperature of 400°C-800°C; Open the sealing cover and place the magnetic ring on the support frame, then close the sealing cover and evacuate the annular heating chamber to a vacuum state through the air outlet pipe; A protective gas is introduced into the annular heating chamber through the air inlet main pipe, and the heating mechanism is started. After the temperature is raised to 400°C at a heating rate of 2°C / min, the temperature is kept for 1 hour, and then the temperature is further raised to 770°C at a rate of 5°C / min, and the temperature is kept at 770°C for 3 hours. During the heating period, the rotary drive component is started to drive the outer tube to rotate forward and reverse, so that the support frame drives the magnetic ring to rotate in the annular heating chamber and continuously move up and down; Turn off the heating mechanism and continue to introduce protective gas until the annular heating chamber cools to room temperature; The outer tube is driven to rotate by the rotary drive assembly so that the support frame drives the magnetic ring to move up to the top of the annular heating chamber, and then the cover is opened to take out the magnetic ring; The above method for reducing the internal stress of the soft magnetic composite material also includes an annealing device, the annealing device includes a hollow tube and a heating mechanism, the hollow tube includes an outer tube and an inner tube, one end of the inner tube is sealed, the edge of the other end of the inner tube is bent outward to extend to form a connecting portion, the outer tube is coaxially arranged with the inner tube, and one end of the outer tube is connected to the connecting portion, and the other end of the outer tube is provided with a sealing cover body, and the outer tube, the inner tube and the sealing cover body are surrounded to form a sealed annular heating chamber; The heating mechanism comprises a first heating component arranged on the inner side of the inner tube, and a second heating component arranged on the outer side of the outer tube; An air outlet pipe is arranged at the center of the sealing cover body, and an air intake main pipe is also arranged through the center of the first heating assembly, one end of the air intake main pipe passes through the sealed end of the inner tube and extends into the annular heating chamber, and air intake branch pipes are evenly arranged along the circumferential direction on the outer side of the air intake main pipe in the annular heating chamber, and the other end of the air intake branch pipes extends to one end of the annular heating chamber close to the connecting portion; The annealing device further comprises a shell and a rotation drive assembly, the hollow tube vertically penetrates the shell, and the outer tube is rotationally connected to the shell, the rotation drive assembly is used to drive the outer tube to rotate, and a rotary joint is arranged on the air outlet pipe; The connecting part is connected to the outer tube via a rotating sealing joint, a clamping piece is provided on the connecting part, and the clamping piece is fixedly connected to the bottom end of the shell via a support rod; a supporting frame is also provided inside the annular heating chamber, and the supporting frame includes a movable ring which is slidably matched with the outer tube and can only slide along the axial direction of the outer tube, and a plurality of supporting rods inclined toward one side of the sealing cover body assembly, the number of the supporting rods is equal to that of the air inlet branch pipe, and the other end of the supporting rod away from the movable ring has a lap portion lapped on the corresponding spiral segment.

2. The method for reducing internal stress of a soft magnetic composite material according to claim 1, characterized in that: In step 2), pre-press with a pressure of 60 kN for 30 seconds, and then maintain the pressure at a pressure of 100 kN for 1 minute.

3. The method for reducing internal stress of a soft magnetic composite material according to claim 1, characterized in that: Before the passivation powder is loaded into the molding die, a lubricant is added into the passivation powder and mixed evenly, wherein the lubricant accounts for 0.5wt% of the passivation powder.

4. The method for reducing internal stress of a soft magnetic composite material according to claim 1, characterized in that: The air intake branch pipe comprises a connecting section connected to the air intake main pipe, and a spiral section connected to the connecting section and spirally wound around the outer side of the inner pipe. The interior of the air intake branch pipe is filled with thermal insulation particles.

Citation Information

Patent Citations

  • Thermal deformation interface diffusion preparation method of soft magnetic composite material

    CN108538568A

  • Homogenizing isothermal annealing device for sintered neodymium-iron-boron magnet

    CN219490070U

  • Magnetic field heat treatment furnace and magnetic field heat treatment system

    CN219637271U

  • Coaxial type vacuum heating device

    JP2000087237A