A method for preparing high-purity single-walled carbon nanotubes
By optimizing the injection position and air flow mode in the CVD reactor, the purity and yield of single-walled carbon nanotubes were successfully improved, the problems of high preparation cost and high impurity content in the existing technology were solved, and efficient single-walled carbon nanotubes were achieved. Nanotube preparation.
Patent Information
- Application Number
- CN202410305346.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-18
- Publication Date
- 2024-10-29
- Estimated Expiration
- 2044-03-18
AI Technical Summary
In the existing technology, the CVD preparation method of single-walled carbon nanotubes has problems such as low yield, high cost and high impurity content. Moreover, the catalyst is mixed with the nanotubes, requiring additional purification treatment, which limits its application scope.
By setting the spray gun outlet at 1/5 to 1/2 in the vertical CVD reactor along the direction from the top to the bottom of the reactor, injecting the carbon source, and growing carbon nanotubes at 800~1200°C, using metal particles The catalyst causes carbon atoms to self-assemble into high-purity single-walled carbon nanotubes.
The preparation of high-purity single-walled carbon nanotubes is achieved, the centralized oxidation temperature is at least 803°C, and the non-carbon impurity content is less than 14%, which reduces the preparation cost and simplifies the process flow.
Smart Images

Figure CN118239476B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of carbon nanotube production, and in particular to a method for preparing high-purity single-walled carbon nanotubes. Background Art
[0002] Carbon nanotubes are hollow tubes rolled up from one or more layers of graphene, known as single-walled carbon nanotubes (SWNTs) and multi-walled carbon nanotubes. Carbon nanotubes have extremely broad application prospects in the fields of composite materials, electrochemical electrode materials, flexible electrode materials, field emission devices, and nanoelectronic devices due to their excellent properties such as high Young's modulus and tensile strength, high thermal conductivity and high electron mobility, as well as regular pore structure and huge specific surface area. Carbon nanotubes have a typical one-dimensional tubular structure and both semiconductor and metallic properties. At the same time, due to the sp2 hybridized CC single bond, the electron movement speed is 1 / 300 of the speed of light and the diameter is as high as 20,000 cm 2 / (v·s) of electron mobility, single-walled carbon nanotubes as electrode materials have a more significant effect on enhancing electrochemical performance. Therefore, how to effectively achieve high-quality preparation of single-walled carbon nanotubes is of great significance for the large-scale application of single-walled carbon nanotubes.
[0003] At present, the main methods for growing single-walled carbon nanotubes include arc discharge method, laser evaporation catalytic precipitation technology and chemical vapor deposition (CVD). The first two methods are very complicated to operate. They need to evaporate the solid carbon source into carbon atoms under high temperature conditions above 3000℃, and the preparation conditions are strict. In addition, the carbon nanotubes grown by evaporating carbon atoms will be highly entangled, mixed with other carbon impurities and metal catalysts, and the prepared single-walled carbon nanotubes are uneven and low in purity, and their performance is limited.
[0004] The preparation of carbon nanotubes by chemical vapor deposition (CVD) has very obvious advantages. The equipment for preparing SWNTs by CVD is simple and easy to operate. It is generally carried out under normal pressure. At the same time, the growth temperature of SWNTs is low, and the requirements for the use of instruments and equipment are low. In addition, the process flow is simple and the growth can be effectively controlled, which is beneficial for industrial applications. Despite this, the existing technical solutions for preparing SWNTs with high purity and good uniformity by CVD still have a very broad room for improvement and still need further optimization. There are still major problems in the preparation of SWNTs with high purity and good uniformity by CVD, such as very low SWNTs yield and very high preparation cost.
[0005] In the prior art, a Chinese patent application with publication number CN110694633A discloses a CVD preparation method for single-walled carbon nanotubes, which proposes to optimize the formulation of a Fe-Mo bimetallic catalyst based on MgO support, significantly reduce the content of Mg in the catalyst, and reduce the preparation cost of the catalyst. 4 , H 2 The optimal combination of inert gas flux and the inert gas flux is explored to achieve the macro-quantity preparation of single-walled carbon nanotubes (SWNTs). However, the method proposed in the patent has the following disadvantages: first, it uses a specific catalyst to catalyze the growth of single-walled carbon nanotubes, which has a limited scope of application; second, the product obtained by this method is a mixture of single-walled carbon nanotubes and catalysts, which needs to be purified.
[0006] Therefore, in summary, more methods for preparing high-quality single-walled carbon nanotubes are still needed to meet the needs of the art. Summary of the invention
[0007] In order to solve the technical problem of high-quality single-walled carbon nanotubes, the present invention provides a method for preparing high-purity single-walled carbon nanotubes. The present invention provides a spray gun for spraying a carbon source into a reaction furnace, and sets the spray gun outlet at a position of 1 / 5 to 1 / 2 of the furnace length of the reaction furnace from the top to the bottom of the reaction furnace, and introduces the carbon source from this position, so as to prepare a high-purity single-walled carbon nanotube at 800-1200°C.
[0008] The specific technical scheme of the present invention is:
[0009] The present invention provides a method for preparing high-purity single-walled carbon nanotubes, comprising the following steps:
[0010] S1. Provide a vertical CVD reactor and place a catalyst in the reactor;
[0011] S2. Provide a spray gun for spraying the carbon source into the reactor, and make the outlet of the spray gun be located at 1 / 5 to 1 / 2 of the reactor along the direction from the top to the bottom of the reactor, measured from the height of the reactor;
[0012] S3. Raise the temperature of the reactor to 800-1200°C. After the temperature stabilizes, introduce a carbon source into the reactor through a spray gun and collect black powder, which is the single-walled carbon nanotube.
[0013] The present invention provides a method for preparing single-walled carbon nanotubes using chemical vapor deposition technology. The main process is that a metal particle catalyst floats in a CVD reactor, and a carbon source, a carrier gas and other gases are introduced. Under the action of the airflow, the metal particle catalyst is always at the front end of the airflow, and the carbon nanotubes grow. Under the high temperature environment, the carbon source decomposes on the surface of the metal particles, and carbon atoms are continuously precipitated and repeatedly self-assembled. The carbon nanotubes continue to grow and extend, and finally form carbon nanotubes.
[0014] In the prior art, it is difficult to prepare single-walled carbon nanotubes by chemical vapor deposition, and the obtained product contains a high content of impurities. After many experiments, the researchers of the present invention found that when the growth projection is carried out in a vertical CVD reactor, the carbon source air inlet is set at 1 / 5 to 1 / 2 of the furnace length of the reactor from the top to the bottom of the reactor, and single-walled carbon nanotubes with less impurity content can be grown. Based on the above findings, the inventors of the present invention optimized the air intake method and air intake position for preparing single-walled carbon nanotubes by CVD, and thus proposed the present invention.
[0015] Specifically, the present invention provides a spray gun for spraying a carbon source into a reactor, and sets the outlet of the spray gun at a position of 1 / 5 to 1 / 2 of the length of the reactor from the top to the bottom of the reactor. The carbon source is introduced from this position, and the carbon source is cracked at 800 to 1200°C, and grows along the catalyst to obtain a high-purity single-walled carbon nanotube.
[0016] The spray gun outlet needs to be set at a position of 1 / 5 to 1 / 2 of the furnace length of the reactor, and the carbon source is introduced from this position, so that the single-walled carbon nanotubes obtained are of higher quality. The spray gun outlet is located near the bottom of the reactor, and it is difficult for the carbon source to contact the catalyst evenly. Therefore, there are many amorphous carbon and large agglomerated particles formed by the wrapped catalyst on the surface of the obtained carbon nanotubes, forming more burrs; and when the nozzle is near the top, the air flow speed at the bottom is too slow, and the air flow speed at the air inlet is larger. The air flow difference has a more obvious effect on the growth of carbon nanotubes, making the nanotubes grow unevenly.
[0017] As a preferred embodiment of the above technical solution of the present invention, the cross-section of the spray gun outlet is a trapezoid that is wide at the top and narrow at the bottom, and the number of the spray gun outlets is at least 2.
[0018] In order to prevent the accumulation of carbon atoms when they self-assemble into nanotubes, the number of spray gun outlets is at least 2, and the cross-section of the spray gun outlet needs to be a trapezoid with a wide top and a narrow bottom. The number of spray gun outlets is at least 2, which is convenient for dispersing carbon atoms and avoiding accumulation and growth. However, the self-assembly process of a layer of carbon nanotubes is a relatively fast process, so the cross-section of the spray gun outlet needs to be a trapezoid with a wide top and a narrow bottom, so that the carbon source converges and then sprays into the reactor.
[0019] Preferably, the spray gun outlet is an inverted frustum-conical pipe.
[0020] As a preferred embodiment of the above technical solution of the present invention, a water cooling component is provided on the spray gun to cool the spray gun section in the reaction furnace.
[0021] Since the present invention requires the spray gun to be disposed in a reaction furnace, during the chemical vapor deposition process, the temperature in the furnace is relatively high, and a water cooling assembly needs to be provided for the spray gun to cool the spray gun section in the reaction furnace to prevent the carbon source from decomposing in the spray gun.
[0022] As a preferred embodiment of the above technical solution of the present invention, in step S3, the reaction furnace is heated to 1000-1100°C.
[0023] As a preferred embodiment of the above technical solution of the present invention, the carbon source is methane.
[0024] More preferably, the carbon source intake rate is 5-10 L / h.
[0025] As a preferred embodiment of the above technical solution of the present invention, in step S3, after the temperature is stabilized, hydrogen is introduced into the reaction furnace at a flow rate of 150-300 sccm.
[0026] The introduction of an appropriate amount of hydrogen can help prevent excessive accumulation of carbon atoms, thereby promoting the formation of single-walled carbon nanotubes and avoiding the formation of multi-walled carbon nanotubes.
[0027] As a preferred embodiment of the above technical solution of the present invention, in step S3, an inert gas is used as a carrier gas to introduce the carbon source, and the flow rate of the carrier gas is 600-1000 sccm.
[0028] The carrier gas can facilitate the introduction of the carbon source, and at the same time, as a diluent gas, it can adjust the gas phase concentration in the reaction chamber, thereby optimizing the growth conditions of the single-walled carbon nanotubes.
[0029] As a preferred embodiment of the above technical solution of the present invention, the catalyst is selected from one or more of ferrocene, nickelocene and cobaltocene.
[0030] Compared with the prior art, the present invention has the following technical effects:
[0031] (1) The present invention provides a spray gun for spraying a carbon source into a reaction furnace, and sets the outlet of the spray gun at a position of 1 / 5 to 1 / 2 of the furnace length of the reaction furnace from the top to the bottom of the reaction furnace. The carbon source is introduced from this position, and the carbon source is cracked at 800-1200°C and grows along the catalyst to obtain a high-purity single-walled carbon nanotube with a concentrated oxidation temperature of at least 803°C and a non-carbon impurity content of less than 14%.
[0032] (2) The existing CVD method mainly prepares new catalysts to prepare high-quality single-walled carbon nanotubes. This method is costly and has a limited scope of application. The present invention is based on the optimization of the air intake position and the change of the airflow injection mode by improving the nozzle outlet. The method is easy to use and has a low cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0033] Figure 1 It is a structural schematic diagram of a chemical vapor deposition device of the present invention;
[0034] Figure 2 It is a structural schematic diagram of a spray gun of the present invention;
[0035] Figure 3 It is a schematic cross-sectional structure diagram of a spray gun of the present invention;
[0036] Figure 4 It is a schematic diagram of the cross-sectional structure of the nozzle of the present invention.
[0037] The accompanying drawings are marked as: 1. vertical CVD reactor, 2. spray gun, 21. spray gun outlet, 22. carbon source injection port, 23. carrier gas inlet, 24. nozzle, 25. mounting flange, 26. graphite gasket, 2701. carbon source cooling water inlet, 2702. carbon source cooling water outlet, 2703. cooling water cavity, 2704. fluororubber sealing ring, 2705. fluororubber sealing ring water cooling layer, 2706. fluororubber sealing ring water cooling layer water inlet, 2707. fluororubber sealing ring water cooling layer outlet, 2708. flange cooling water inlet, 2709. flange cooling water outlet, 2710. water cooling layer, 28. carrier gas cavity. DETAILED DESCRIPTION
[0038] The present invention will be further described below in conjunction with embodiments. Those of ordinary skill in the art will be able to implement the present invention based on these descriptions. In addition, the embodiments of the present invention involved in the following description are generally only embodiments of a part of the present invention, rather than all embodiments. Therefore, based on the embodiments in the present invention, all other embodiments obtained by those of ordinary skill in the art without making creative work should belong to the scope of protection of the present invention.
[0039] Generally, the oxidation resistance temperature of single-walled carbon nanotubes is 400-700°C. The characterization technology for evaluating the high quality and high purity of single-walled carbon nanotubes can be thermogravimetric or thermal differential thermal analysis. The highest oxidation resistance temperature refers to the concentrated oxidation temperature of the sample. The concentrated oxidation resistance temperature of the original sample of single-walled carbon nanotubes is greater than 800°C. The non-carbon impurity content refers to the impurity content in the sample other than carbon. In the present invention, it mainly comes from the catalyst. The low content of non-carbon impurities can reflect the high purity performance of single-walled carbon nanotubes.
[0040] Example 1
[0041] Step 1:
[0042] Provide a chemical vapor deposition device①, such as Figure 1 As shown, it includes a vertical CVD reactor and a spray gun arranged on the top of the furnace for spraying a carbon source into the reactor.
[0043] Specifically, the structure of the spray gun is as follows: Figures 2~4 As shown. The spray gun includes a carrier gas cavity, a carbon source injection port, a carrier gas inlet, a nozzle, a spray gun outlet, a mounting flange, a graphite gasket and a water 28 assembly for cooling the spray gun. The nozzle is provided with a thread, which is fixed to the carrier gas cavity by a threaded connection, and the spray gun outlet is provided on the nozzle. The carrier gas cavity is fixed to the mounting flange by molybdenum bolts, and a graphite gasket is added to the contact surface. The carbon source injection port is fixed in the carrier gas cavity, passes through the carrier gas cavity to the spray gun outlet and communicates with the vertical CVD reactor chamber. After the carrier gas inlet and the carbon source injection port meet in the nozzle, they are communicated with the vertical CVD reactor chamber through the spray gun outlet.
[0044] Among them, the water cooling component includes a carbon source cooling water inlet, a carbon source cooling water outlet, a cooling water cavity, a fluororubber sealing ring, a fluororubber sealing ring water cooling layer, a fluororubber sealing ring water cooling layer water inlet, a fluororubber sealing ring water cooling layer outlet, a flange cooling water inlet, a flange cooling water outlet, and a water cooling layer.
[0045] The cooling water cavity is arranged in the carrier gas cavity, and the carbon source injection port is fixed on the cooling water cavity by welding and penetrates the cooling water cavity. The carbon source cooling water inlet and the carbon source cooling water outlet are respectively welded on the bottom and the top of the cooling water cavity, and the carbon source cooling water inlet and the carbon source cooling water outlet are communicated, so as to provide cooling water for the cooling water cavity to enter from the bottom and exit from the top. The cooling water cavity is fixed on the mounting flange by bolts, and a fluororubber sealing ring is added to the contact surface. The water cooling layer is arranged on the mounting flange, and the flange cooling water inlet and the flange cooling water outlet are arranged on the water cooling layer, and the two are communicated, so as to provide cooling water for the water cooling layer, which is used to cool the mounting flange. The fluororubber sealing ring water cooling layer is arranged on the fluororubber sealing ring, and the fluororubber sealing ring water cooling layer water inlet and the fluororubber sealing ring water cooling layer outlet are communicated with the fluororubber sealing ring water cooling layer, so as to provide cooling water for the fluororubber sealing ring water cooling layer, which is used to cool the fluororubber sealing ring. The flange cooling water inlet, the flange cooling water outlet, the mounting flange, the water cooling layer, the carrier gas inlet, the fluororubber sealing ring water cooling layer water inlet, and the fluororubber sealing ring water cooling layer outlet are welded and fixed together.
[0046] like Figure 4, which is a schematic diagram of the cross-sectional structure of the nozzle provided in this embodiment. The number of the spray gun outlets is 3, which are evenly spaced on the nozzle. The spray gun outlet is an inverted truncated cone-shaped pipeline, and its cross section is a trapezoidal shape that is wide at the top and narrow at the bottom. Along the direction from the top to the bottom of the reactor, the end of the spray gun outlet is located at the 7 / 24 position of the reactor in terms of the height of the reactor.
[0047] Step 2:
[0048] Provide a chemical vapor deposition device ②. The difference between the chemical vapor deposition device provided in this step and that provided in step 1 is that: along the direction from the top to the bottom of the reactor, measured by the height of the reactor, the end of the spray gun outlet is located at the 1 / 4 position of the reactor.
[0049] Step 3:
[0050] Provide a chemical vapor deposition device ③. The difference between the chemical vapor deposition device provided in this step and that provided in step 1 is that: along the direction from the top to the bottom of the reactor, measured by the height of the reactor, the end of the spray gun outlet is located at 1 / 3 of the reactor.
[0051] Step 4:
[0052] Provide a chemical vapor deposition device ④. The difference between the chemical vapor deposition device provided in this step and that provided in step 1 is that: along the direction from the top to the bottom of the reactor, measured by the height of the reactor, the end of the spray gun outlet is located at 1 / 5 of the reactor.
[0053] Step 5:
[0054] Provide a chemical vapor deposition device ⑤. The difference between the chemical vapor deposition device provided in this step and that provided in step 1 is that: along the direction from the top to the bottom of the reactor, measured by the height of the reactor, the end of the spray gun outlet is located at the 1 / 2 position of the reactor.
[0055] Step 6:
[0056] Provide a chemical vapor deposition device ⑥. The chemical vapor deposition device provided in this step is different from that provided in step 1 in that: the number of spray gun outlets is 5, which are evenly spaced on the nozzle.
[0057] Step 7:
[0058] Provide a chemical vapor deposition device ⑦. The chemical vapor deposition device provided in this step is different from that provided in step 1 in that: the number of spray gun outlets is 2.
[0059] Example 2
[0060] A single-walled carbon nanotube is provided, which is prepared by using a chemical vapor deposition device① according to the following steps:
[0061] S1. Heat the vertical CVD reactor to 100°C, and introduce ferrocene into the reactor to diffuse in the furnace. The amount of ferrocene introduced is 2% of the mass of the carbon source.
[0062] S2. The temperature of the reactor is raised to 1000°C. After the temperature is stabilized, carbon source methane gas is introduced into the reactor through a spray gun. The specific method of introduction is: argon gas with a flow rate of 750 sccm is used as a carrier gas to introduce methane gas. The intake rate of methane gas is 8 L / h.
[0063] S3. After half an hour, the black powder was collected and observed under a high-power scanning electron microscope. It can be seen that the surface of the carbon nanotubes constituting the fiber is smooth and pure.
[0064] Example 3
[0065] The main difference from Example 2 is that a chemical vapor deposition device ② is used for preparation. The other steps are the same as those in Example 2.
[0066] Example 4
[0067] The main difference from Example 2 is that a chemical vapor deposition device ③ is used for preparation. The other steps are the same as those in Example 2.
[0068] Example 5
[0069] The main difference from Example 2 is that a chemical vapor deposition device ④ is used for preparation. The other steps are the same as those in Example 2.
[0070] Example 6
[0071] The main difference from Example 2 is that a chemical vapor deposition device ⑤ is used for preparation. The other steps are the same as those in Example 2.
[0072] Example 7
[0073] The main difference from Example 2 is that a chemical vapor deposition device ⑥ is used for preparation. The other steps are the same as those in Example 2.
[0074] Example 8
[0075] The main difference from Example 2 is that a chemical vapor deposition device ⑦ is used for preparation. The other steps are the same as those in Example 2.
[0076] Example 9
[0077] The main difference from Example 2 is that in step S2, the temperature is raised to 1100° C. The other steps are the same as those in Example 2.
[0078] Example 10
[0079] The main difference from Example 2 is that in step S2, the temperature is raised to 800° C. The other steps are the same as those in Example 2.
[0080] Embodiment 11
[0081] The main difference from Example 2 is that in step S2, the temperature is raised to 1200° C. The other steps are the same as those in Example 2.
[0082] Example 12
[0083] A single-walled carbon nanotube is provided, which is prepared by using a chemical vapor deposition device① according to the following steps:
[0084] S1. Heat the vertical CVD reactor to 100°C, and introduce ferrocene into the reactor to diffuse in the furnace. The amount of ferrocene introduced is 2% of the mass of the carbon source.
[0085] S2. The temperature of the reactor is raised to 1000°C. After the temperature is stabilized, carbon source methane gas is introduced into the reactor through a spray gun. The specific method of introduction is: argon gas with a flow rate of 600sccm is used as a carrier gas to introduce methane gas. The intake rate of methane gas is 5L / h.
[0086] S3. After half an hour, the black powder was collected to obtain single-walled carbon nanotubes.
[0087] Embodiment 13
[0088] A single-walled carbon nanotube is provided, which is prepared by using a chemical vapor deposition device① according to the following steps:
[0089] S1. Heat the vertical CVD reactor to 100°C, and introduce ferrocene into the reactor to diffuse in the furnace. The amount of ferrocene introduced is 2% of the mass of the carbon source.
[0090] S2. The temperature of the reactor is raised to 1000°C. After the temperature is stabilized, carbon source methane gas is introduced into the reactor through a spray gun. The specific method of introduction is: argon gas with a flow rate of 1000sccm is used as a carrier gas to introduce methane gas. The intake rate of methane gas is 10L / h.
[0091] S3. After half an hour, the black powder was collected to obtain single-walled carbon nanotubes.
[0092] Comparative Example 1
[0093] The main difference from Example 2 is that in the chemical vapor deposition device, the end of the spray gun outlet is located at 3 / 5 of the reactor (measured from the height of the reactor, from the top to the bottom of the reactor). The other steps are the same as in Example 2.
[0094] The carbon nanotubes prepared in this comparative example have many burrs on their surfaces.
[0095] Comparative Example 2
[0096] The main difference from Example 2 is that in the chemical vapor deposition device, the end of the spray gun outlet is located at 1 / 7 of the reactor (measured from the reactor's height, from the top to the bottom). The other steps are the same as in Example 2.
[0097] The carbon nanotubes prepared in this comparative example have many burrs on their surfaces.
[0098] Comparative Example 3
[0099] The main difference from Example 2 is that in the chemical vapor deposition device, the number of the spray gun outlets is 1. The other steps are the same as those in Example 2.
[0100] The carbon nanotubes prepared in this comparative example have some burrs on their surfaces.
[0101] Comparative Example 4
[0102] The main difference from Example 2 is that in the chemical vapor deposition device, the number of spray gun outlets is 7. The other steps are the same as those in Example 2.
[0103] The carbon nanotubes prepared in this comparative example have some burrs on their surfaces.
[0104] Comparative Example 5
[0105] The main difference from Example 2 is that in the chemical vapor deposition device, the spray gun outlet is columnar, and its cross section is a rectangle that is wide at the top and narrow at the bottom. The other steps are the same as in Example 2.
[0106] The carbon nanotubes prepared in this comparative example have many burrs on their surfaces.
[0107] Comparative Example 6
[0108] The main difference from Example 2 is that in the chemical vapor deposition device, the spray gun outlet is columnar, the cross section of which is a rectangle that is wide at the top and narrow at the bottom, and the number is 1. The other steps are the same as in Example 2.
[0109] The carbon nanotubes prepared in this comparative example have many burrs on their surfaces.
[0110] Comparative Example 7
[0111] The main difference from Example 2 is that the intake rate of methane gas is 15 L / h. The other steps are the same as those in Example 2.
[0112] The carbon nanotubes prepared in this comparative example have many burrs on their surfaces.
[0113] Performance Characterization
[0114] The black powders obtained in Examples 2 to 13 and Comparative Examples 1 to 4 were subjected to a centralized antioxidant temperature test using a thermal analyzer, and their non-carbon impurity contents were calculated using thermogravimetric curves. The results are shown in Table 1.
[0115] Table 1
[0116] Central anti-oxidation temperature / ℃ Non-carbon impurity content / % Example 2 846 11.9 Example 3 842 12.3 Example 4 845 12.1 Example 5 829 13.3 Example 6 824 13.8 Example 7 836 12.4 Example 8 839 12.1 Example 9 845 11.8 Example 10 803 13.7 Embodiment 11 810 13.4 Example 12 839 12.3 Embodiment 13 838 12.4 Comparative Example 1 687 17.2 Comparative Example 2 698 16.4 Comparative Example 3 773 14.0 Comparative Example 4 701 15.2 Comparative Example 5 691 17.1 Comparative Example 6 686 17.9 Comparative Example 7 682 17.1
[0117] Data Analysis:
[0118] (1) The present invention provides a spray gun for spraying a carbon source into a reaction furnace, and sets the outlet of the spray gun at a position of 1 / 5 to 1 / 2 of the furnace length of the reaction furnace from the top to the bottom of the reaction furnace. The carbon source is introduced from this position, and the carbon source is cracked at 800-1200°C and grows along the catalyst to obtain a high-purity single-walled carbon nanotube with a concentrated oxidation temperature of at least 803°C and a non-carbon impurity content of less than 14%.
[0119] (2) By comparing and analyzing Comparative Examples 1 and 2 with Example 2, Comparative Examples 1 and 2 respectively locate the end of the spray gun outlet at 3 / 5 and 1 / 7 of the furnace length of the reactor, and the concentrated anti-oxidation temperature becomes lower, the content of non-single-walled nanotubes is relatively large, and the content of non-carbon impurities is still relatively high. The reason for this is that due to incomplete or uneven growth, burrs that wrap the catalyst will be formed, and the non-carbon content is high. The spray gun outlet of Comparative Example 1 is located near the bottom of the reactor, and it is difficult for the carbon source to contact the catalyst evenly. Therefore, there are a lot of amorphous carbon and large agglomerated particles formed by the wrapped catalyst on the surface of the obtained carbon nanotubes, forming more burrs; the nozzle of Comparative Example 2 is located near the top, which will cause the air flow velocity at the bottom to be too slow, and the air flow velocity at the air inlet is relatively large. The air flow difference has a more obvious effect on the growth of carbon nanotubes, making the nanotubes grow unevenly.
[0120] (3) By comparing and analyzing Comparative Examples 3-4 with Example 2, Comparative Examples 3-4 set the number of spray gun outlets to 1 and 7 respectively, and the concentrated antioxidant temperature becomes lower, the content of non-single-walled nanotubes is larger, and the content of non-carbon impurities is higher, and the change in Comparative Example 7 is obvious. Analysis of the reasons shows that the form of dispersing the carbon source through multiple outlets of the spray gun outlet can effectively prevent the accumulation of carbon atoms when they self-assemble into nanotubes. However, the number of spray gun outlets needs to be controlled within a certain range. If the number of outlets is large, since the cross-section of the spray gun outlet is a trapezoid with a wide top and a narrow bottom, it is a converging outlet, which will increase the carbon source flow rate of each spray gun outlet, making the self-assembly accumulation of carbon atoms uneven. If the number of outlets is too small, it cannot play the role of dispersing the airflow.
[0121] (4) By comparing comparative example 5 with example 2, the spray gun outlet of comparative example 5 is columnar, its concentrated anti-oxidation temperature becomes lower, the content of non-single-walled nanotubes is larger, and the content of non-carbon impurities is higher. The reason for this is that the self-assembly process of a layer of carbon nanotubes is a relatively fast process, so it is necessary to make the cross-section of the spray gun outlet into a trapezoid with a wide top and a narrow bottom, so that the carbon source can be converged and then sprayed into the reactor, otherwise the carbon atoms will not have time to accumulate and cannot form continuous single-walled carbon nanotubes, so that the surface of the carbon nanotubes has more defects and a high amorphous carbon content. In addition, comparative example 7 increases the intake rate of the carbon source, but its content of non-single-walled nanotubes is larger, the concentrated anti-oxidation temperature is low, and the content of non-carbon impurities is still high. It can be seen that it is impossible to increase the intake rate of the carbon source to meet the rapid assembly process of single-walled carbon nanotubes. The cross-section of the spray gun outlet is a trapezoid with a wide top and a narrow bottom, so that the carbon source can be converged and then sprayed into the reactor, so as to adapt to the rapid assembly of single-walled carbon nanotubes, which has a great advantage.
[0122] In the process of implementing the present invention, chemical vapor deposition technology is a relatively mature technology, and a vertical CVD reactor can be obtained through existing technology. Before the preparation process of the present invention is implemented, the chemical vapor deposition device has been vacuumed, and then nitrogen is introduced to ensure that the air in the device is completely removed.
[0123] The raw materials and equipment used in the present invention, unless otherwise specified, are all commonly used raw materials and equipment in the art; the methods used in the present invention, unless otherwise specified, are all conventional methods in the art.
[0124] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any way. Any simple modification, change and equivalent transformation made to the above embodiment based on the technical essence of the present invention still falls within the protection scope of the technical solution of the present invention.
Claims
1. A method for preparing high-purity single-walled carbon nanotubes, Features: The following steps are involved: S1. Provide a vertical CVD reactor and place a catalyst in the reactor; S2. Provide a spray gun for spraying the carbon source into the reactor, and make the end of the spray gun outlet be located at 1 / 5 to 1 / 2 of the reactor along the direction from the top to the bottom of the reactor, measured from the height of the reactor; S3, raising the temperature of the reactor to 800-1200°C, and after the temperature stabilizes, introducing a carbon source into the reactor through a spray gun, and collecting black powder, which is single-walled carbon nanotubes; in: The spray gun outlet is an inverted frustum-shaped pipe, and its cross section is a trapezoid that is wide at the top and narrow at the bottom. The number of spray gun outlets is 2~5; The carbon source intake rate is 5~10L / h; In step S3, an inert gas is used as a carrier gas to introduce a carbon source, and the flow rate of the carrier gas is 600-1000 sccm; In step S3, after the temperature is stabilized, hydrogen is introduced into the reaction furnace at a flow rate of 150-300 sccm.
2. A method for preparing high-purity single-walled carbon nanotubes as claimed in claim 1, Features: The spray gun is provided with a water cooling assembly for cooling the spray gun section in the reaction furnace.
3. A method for preparing high-purity single-walled carbon nanotubes as claimed in claim 1, Features: In step S3, the temperature of the reaction furnace is raised to 1000-1100°C.
4. A method for preparing high-purity single-walled carbon nanotubes as claimed in claim 1, Features: The carbon source is methane.
5. A method for preparing high-purity single-walled carbon nanotubes as claimed in claim 1, Features: The catalyst is selected from one or more of ferrocene, nickelocene and cobaltocene.
Citation Information
Patent Citations
CVD preparation method of single-walled carbon nanotube
CN110694633A
Method for manufacturing semiconductive single-walled carbon nanotubes
CN104944412A
Open equipment for continuous growth of carbon nanomaterial and preparation method
CN109336096A
Apparatus for continuously preparing high-quality carbon nanotubes and preparation method of carbon nanotubes
CN110217778A
Preparation method of carbon nanotubes and carbon nanotube fiber
CN110734053A