Ionic polymer binder and preparation method and application thereof
By enhancing the adhesion and conductivity of the positive electrode of lithium-ion batteries with ionic polymer binders, the problem of active material shedding during cycling of PVDF binders is solved, achieving high specific capacity and long lifespan lithium-ion battery performance.
Patent Information
- Application Number
- CN202410332019.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-03-22
- Publication Date
- 2024-11-22
- Estimated Expiration
- 2044-03-22
AI Technical Summary
The existing PVDF binder for lithium-ion batteries causes active materials to pulverize and detach during cycling due to van der Waals forces and hydrogen bonding, affecting the cycle stability of the battery.
An ionic polymer binder was used to enhance adhesion by leveraging the strong interaction between hexafluorophosphate and the positive electrode active material and the flexibility of polyethylene glycol acrylate. The acrylate was introduced to reduce hydrophilicity, thus preparing a positive electrode sheet for lithium-ion batteries.
It improves the specific capacity, capacity retention and cycle stability of lithium-ion batteries, the electrode sheets are smooth without edge curling or cracking, the active material loading is increased and the conductivity is enhanced.
Smart Images

Figure CN118240508B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of lithium ion batteries, and in particular to an ionic polymer binder and a preparation method and application thereof. Background Art
[0002] With the advancement of the national strategy of "carbon neutrality", the research and development of energy storage technology has become a development focus. As a new type of energy equipment that has been commercialized, lithium-ion batteries have the advantages of high specific energy, long cycle life and high safety performance, and are used in fields such as mobile electronic devices and electric vehicles. Lithium-ion batteries are mainly composed of five parts: positive electrode, diaphragm, negative electrode, electrolyte and battery casing. The bonding strength between the positive and negative electrode materials and the conductive agent and current collector has an important influence on the cycle stability of the battery.
[0003] Currently, commercial positive electrode binders are mainly polyvinylidene fluoride (PVDF), which has good antioxidant ability and chemical reaction inertness. However, the bonding effect of PVDF generally comes from the van der Waals force between molecules and the hydrogen bonds formed by the CF bonds on the main chain and other substances, which will cause the active material to pulverize and fall off the current collector during the cycle, thereby affecting the cycle stability of the battery assembled using the binder. Therefore, how to improve the bonding performance of the binder and the cycle stability of the battery assembled using the binder has become a technical problem that needs to be solved urgently in this field. Summary of the invention
[0004] The purpose of the present invention is to provide an ionic polymer binder and a preparation method and application thereof. The ionic polymer binder provided by the present invention has excellent bonding performance and realizes high loading of positive electrode active materials; the assembled lithium ion battery has high specific capacity, capacity retention rate and cycle stability.
[0005] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:
[0006] The present invention provides an ionic polymer binder having a chemical structure shown in Formula I or Formula II:
[0007]
[0008] In the formula I, R1, R3 and R4 are independently hydrogen or alkyl, and R2 and R5 are independently alkyl;
[0009] In the formula II, R6 is hydrogen or alkyl, R7 is alkylene or aralkylene, R8 and R9 are independently alkyl or aralkyl, R 10 It is an alkyl group.
[0010] Preferably, in the formula I, m=1-3, n=4-40, x+y+z=1, wherein x>0, y>0, z≥0.
[0011] Preferably, in the formula II, q is the degree of polymerization, and q is 20-2000.
[0012] The present invention also provides a method for preparing the ionic polymer binder described in the above technical solution, comprising the following steps:
[0013] (1) mixing a monomer, a first initiator and a first organic solvent to perform a first free radical polymerization reaction to obtain a first polymer solution;
[0014] (2) mixing the first halogenated hydrocarbon, the second solvent and the first polymer solution obtained in step (1) to perform a first quaternization reaction to obtain a second polymer solution;
[0015] (3) mixing the second polymer solution obtained in step (2) with the first fluorophosphate aqueous solution to perform a first ion replacement reaction to obtain an ionic polymer binder;
[0016] When the monomer in step (1) is dialkylamino acrylate, an ionic polymer binder having a chemical structure of formula II is obtained;
[0017] When the monomers in step (1) are dialkylamino acrylate and polyethylene glycol acrylate, an ionic polymer binder with z=0 in the chemical structure of formula I is obtained;
[0018] When the monomers in step (1) are dialkylamino acrylate, polyethylene glycol acrylate and acrylate, an ionic polymer binder with z>0 in the chemical structure of formula I is obtained.
[0019] Preferably, in the step (1), the temperature of the first free radical polymerization reaction is 45 to 80° C., and the time of the first free radical polymerization reaction is 6 to 24 hours.
[0020] Preferably, the temperature of the first quaternization reaction in step (2) is 10 to 45° C., and the time of the first quaternization reaction is 1 to 12 hours.
[0021] Preferably, the temperature of the first ion exchange reaction in step (3) is 10 to 45° C., and the time of the first ion exchange reaction is 1 to 12 hours.
[0022] The present invention also provides a method for preparing the ionic polymer binder described in the above technical solution, comprising the following steps:
[0023] 1) mixing dialkylamino acrylate, water and a second halogenated hydrocarbon, and performing a second quaternization reaction to obtain a trialkylamino acrylate halide aqueous solution;
[0024] 2) mixing the aqueous solution of trialkylamino acrylate halide obtained in step 1) with the aqueous solution of the second fluorophosphate salt, and performing a second ion exchange reaction to obtain trialkylamino acrylate fluorophosphate salt;
[0025] 3) mixing the trialkylamino acrylate fluoride phosphate obtained in step 2), polyethylene glycol acrylate, acrylate, a second initiator and water, and performing a second free radical polymerization reaction to obtain an ionic polymer binder with z>0 in the chemical structure of formula I;
[0026] When the acrylate is omitted in step 3), an ionic polymer binder with z=0 in the chemical structure of formula I is obtained;
[0027] When the polyethylene glycol acrylate and acrylate are omitted in step 3), an ionic polymer binder with a chemical structure of formula II is obtained.
[0028] The present invention also provides the use of the ionic polymer binder described in the above technical solution or the ionic polymer binder prepared by the preparation method described in the above technical solution in a positive electrode sheet of a lithium ion battery.
[0029] Preferably, the method for preparing the positive electrode sheet of a lithium-ion battery comprises the following steps:
[0030] ① mixing the ionic polymer binder and the second organic solvent to obtain a binder solution;
[0031] ② Mixing the active material and the conductive agent to obtain a mixed powder;
[0032] ③ Mixing the binder solution obtained in step ①, the mixed powder obtained in step ② and a third organic solvent to obtain a positive electrode slurry;
[0033] ④ coating the positive electrode slurry obtained in step ③ on the current collector to obtain a positive electrode sheet for a lithium-ion battery;
[0034] There is no order of precedence between step ① and step ②.
[0035] The present invention provides an ionic polymer binder having a chemical structure shown in Formula I or Formula II. The interaction between the hexafluorophosphate in the ionic polymer binder provided by the present invention and the positive electrode active material can enhance the bonding between the materials and the conductivity of lithium ions, and can increase the active material loading of the positive electrode, so that the lithium ion battery assembled using the binder has the advantages of large specific capacity, good cycle stability and long life. The results of the embodiment show that the battery assembled using the ionic polymer binder provided by the present invention can still maintain 137.8 mAhg after 800 cycles at a current density of 0.5C. -1, capacity retention rate 92.11%; after 1000 cycles, it can still maintain 127.1mAhg -1 , capacity retention rate is 85.02%, and the cycle performance is excellent. BRIEF DESCRIPTION OF THE DRAWINGS
[0036] Figure 1 This is the NMR spectrum of the ionic polymer binder prepared in Example 1;
[0037] Figure 2 is the NMR spectrum of trimethylaminoethyl acrylate fluorophosphonate in Example 5;
[0038] Figure 3 This is the NMR spectrum of the ionic polymer binder prepared in Example 9;
[0039] Figure 4 The long cycle charge and discharge curve of the battery assembled with C1 as the positive electrode and lithium metal as the negative electrode at 25°C, a cut-off voltage of 2.5-4.2V and a rate of 0.5C;
[0040] Figure 5 The charge and discharge curves of the battery assembled with C1 as the positive electrode and lithium metal as the negative electrode at 25°C and a cut-off voltage of 2.5-4.2V under different rate conditions such as 0.1C, 0.2C and 0.5C;
[0041] Figure 6 The long cycle charge and discharge curve of a battery assembled with C17 as the positive electrode and lithium metal as the negative electrode at 25°C, a cut-off voltage of 2.5-4.2V and a rate of 0.5C;
[0042] Figure 7 The charge and discharge curves of the battery assembled with C17 as the positive electrode and lithium metal as the negative electrode at 25°C and a cut-off voltage of 2.5-4.2V under different rate conditions such as 0.1C, 0.2C and 0.5C;
[0043] Figure 8 Long cycle charge and discharge curve of lithium iron phosphate / artificial graphite battery assembled with C1 as positive electrode and C22 as negative electrode at 25°C, cut-off voltage of 2.5-4.2V and rate of 0.5C;
[0044] Fig. 9 This is the long cycle charge and discharge curve of the lithium iron phosphate / artificial graphite battery assembled with C17 as the positive electrode and C22 as the negative electrode at 25°C, a cut-off voltage of 2.5-4.2V and a rate of 0.5C. DETAILED DESCRIPTION
[0045] The present invention provides an ionic polymer binder having a chemical structure shown in Formula I or Formula II:
[0046]
[0047] In the formula I, R1, R3 and R4 are independently hydrogen or alkyl, and R2 and R5 are independently alkyl;
[0048] In the formula II, R6 is hydrogen or alkyl, R7 is alkylene or aralkylene, R8 and R9 are independently alkyl or aralkyl, R 10 It is an alkyl group.
[0049] In one technical solution of the present invention, the ionic polymer binder has a chemical structure shown in Formula I:
[0050]
[0051] In the present invention, in the formula I, R1, R3 and R4 are independently hydrogen or alkyl, R2 and R5 are independently alkyl, and the alkyl is preferably methyl or butyl.
[0052] In the present invention, in the formula I, m is preferably 1 to 3, n is preferably 4 to 40, x+y+z is preferably 1, wherein x is preferably >0, y is preferably >0, and z is preferably ≥0.
[0053] In the present invention, the interaction between the hexafluorophosphate in the ionic polymer binder and the positive electrode active material can enhance the bonding between the materials and the conductivity of lithium ions; polyethylene glycol acrylate can improve the flexibility of the binder and soften the pole piece; acrylate is introduced as a hydrophobic segment to reduce the hydrophilicity of the polymer, thereby avoiding the problem of a decrease in battery capacity and cycle performance after the active material absorbs water, thereby making the lithium ion battery assembled using the binder have a higher specific capacity, capacity retention rate and cycle stability.
[0054] In another technical solution of the present invention, the ionic polymer binder has a chemical structure shown in Formula II:
[0055]
[0056] In the present invention, in the formula II, R6 is hydrogen or alkyl, the alkyl is preferably methyl or ethyl; R7 is alkylene or aralkylene, the alkylene is preferably ethylene or propylene, the aralkylene is preferably diphenyl; R8 and R9 are independently alkyl or aralkyl, the alkyl is preferably methyl, the aralkyl is preferably benzyl; R 10 is an alkyl group, and the alkyl group is preferably a methyl group.
[0057] In the present invention, in the formula II, q is the degree of polymerization, and q is preferably 20-2000.
[0058] When the ionic polymer binder provided by the present invention is used to prepare the positive electrode of a lithium ion battery, the interaction between the hexafluorophosphate in the ionic polymer binder and the positive electrode active material can enhance the adhesion between the materials and the conductivity of lithium ions, and can increase the active material loading of the positive electrode; the prepared pole piece is smooth and has no curling or cracking; the lithium ion battery assembled using the binder has the advantages of large specific capacity, good cycle stability and long service life.
[0059] The present invention also provides a method for preparing the ionic polymer binder described in the above technical solution, comprising the following steps:
[0060] (1) mixing a monomer, a first initiator and a first organic solvent to perform a first free radical polymerization reaction to obtain a first polymer solution;
[0061] (2) mixing the first halogenated hydrocarbon, the second solvent and the first polymer solution obtained in step (1) to perform a first quaternization reaction to obtain a second polymer solution;
[0062] (3) mixing the second polymer solution obtained in step (2) with the first fluorophosphate aqueous solution to perform a first ion replacement reaction to obtain an ionic polymer binder;
[0063] When the monomer in step (1) is dialkylamino acrylate, an ionic polymer binder having a chemical structure of formula II is obtained;
[0064] When the monomers in step (1) are dialkylamino acrylate and polyethylene glycol acrylate, an ionic polymer binder with z=0 in the chemical structure of formula I is obtained;
[0065] When the monomers in step (1) are dialkylamino acrylate, polyethylene glycol acrylate and acrylate, an ionic polymer binder with z>0 in the chemical structure of formula I is obtained.
[0066] The present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.
[0067] The present invention mixes a monomer, a first initiator and a first organic solvent, performs a first free radical polymerization reaction, and obtains a first polymer solution.
[0068] In the present invention, the monomer is preferably at least one of dialkylamino acrylate, polyethylene glycol acrylate and acrylate.
[0069] In the present invention, when the monomer is dialkylamino acrylate, an ionic polymer binder with a chemical structure of Formula II is obtained.
[0070] In the present invention, when the monomers are dialkylamino acrylate and polyethylene glycol acrylate, an ionic polymer binder with z=0 in the chemical structure of Formula I is obtained; the molar ratio of the dialkylamino acrylate and polyethylene glycol acrylate is preferably 1:(0.1-1.1), more preferably 1:(0.5-1.0). In the present invention, when the molar ratio of the dialkylamino acrylate and polyethylene glycol acrylate is within the above range, the free radical polymerization reaction can be fully carried out and the binder can have better bonding performance.
[0071] In the present invention, when the monomers are dialkylamino acrylate, polyethylene glycol acrylate and acrylate, an ionic polymer binder with z>0 in the chemical structure of Formula I is obtained; the molar ratio of the dialkylamino acrylate, polyethylene glycol acrylate and acrylate is preferably 1:(0.1-1.1):(0.1-1.1), more preferably 1:(0.5-1.0):(0.5-1.0). In the present invention, when the molar ratio of the dialkylamino acrylate, polyethylene glycol acrylate and acrylate is within the above range, the free radical polymerization reaction can be fully carried out and the binder can have better bonding performance.
[0072] In the present invention, the dialkylamino acrylate is preferably one or more of dimethylaminoethyl acrylate, dimethylaminoethyl methacrylate, 3-(dimethylamino)propyl methacrylate and 4'-[di(4-methylphenyl)amino]biphenyl-4-yl 2-acrylate.
[0073] In the present invention, the polyethylene glycol acrylate is preferably polyethylene glycol monomethyl ether acrylate and / or polyethylene glycol monomethyl ether methacrylate.
[0074] In the present invention, the acrylic acid ester is preferably one or more of butyl acrylate, butyl methacrylate, 2-ethylbutyl acrylate and pentyl acrylate.
[0075] In the present invention, the first initiator is preferably one or more of azobisisobutyronitrile, azobiscyclohexylcarbonitrile, dimethyl azobisisobutyrate and dibenzoyl peroxide, more preferably azobisisobutyronitrile, azobiscyclohexylcarbonitrile or dimethyl azobisisobutyrate. In the present invention, the initiator can initiate free radical polymerization of the monomer.
[0076] In the present invention, the first organic solvent preferably includes one or more of dimethyl carbonate, ethanol, ether, acetonitrile, toluene, acetone, N-methylpyrrolidone, N,N-dimethylformamide, tetrahydrofuran, dichloromethane and chloroform. The present invention uses the above organic solvents to have good compatibility with various raw materials, thereby ensuring that the free radical polymerization reaction is fully carried out.
[0077] In the present invention, the mass of the first initiator is preferably 0.1-2% of the mass of the monomer, and more preferably 0.4-1.5%. In the present invention, controlling the amount of the initiator within the above range can promote the free radical polymerization reaction to proceed fully.
[0078] The present invention has no special limitation on the mass of the first organic solvent, as long as the mass concentration of the monomer is within the range of 10-50%, more preferably within the range of 20-30%. In the present invention, the organic solvent within the above dosage range is more conducive to the full progress of the free radical polymerization reaction.
[0079] The present invention has no special limitation on the operation of mixing the monomer, the first initiator and the first organic solvent. It is sufficient to use a mixing method well known to those skilled in the art to mix the above components uniformly.
[0080] In the present invention, the temperature of the first free radical polymerization reaction is preferably 45 to 80° C., more preferably 60 to 70° C.; the time of the first free radical polymerization reaction is preferably 6 to 24 hours, more preferably 8 to 15 hours. In the present invention, when the temperature and time of the free radical polymerization reaction are within the above ranges, the free radical polymerization reaction can be fully carried out.
[0081] In the present invention, the first free radical polymerization reaction is preferably carried out in an inert atmosphere; the inert atmosphere is preferably nitrogen or argon. In the present invention, the inert atmosphere can prevent the interference of air on the free radical polymerization reaction.
[0082] After obtaining the first polymer solution, the present invention mixes the first halogenated hydrocarbon and the second solvent with the first polymer solution to perform a first quaternization reaction to obtain a second polymer solution.
[0083] In the present invention, the first halogenated hydrocarbon is preferably at least one of methyl iodide, ethyl bromide, propyl bromide and 1-chlorobutane. When the first halogenated hydrocarbon is two or more of the above, the present invention has no special limitation on the ratio between the two or more, and any ratio can be mixed. In the present invention, the halogenated hydrocarbon and the dialkylamino group in the dialkylamino acrylate undergo quaternization reaction, so that the dialkylamino acrylate is converted into a quaternary ammonium salt.
[0084] In the present invention, the second solvent is preferably one or more of dimethyl carbonate, ethanol, ether, acetonitrile, toluene, acetone, N-methylpyrrolidone, N,N-dimethylformamide, tetrahydrofuran, dichloromethane and chloroform.
[0085] In the present invention, the molar ratio of the dialkylamino acrylate to the first halogenated hydrocarbon is preferably (0.5-1):(0.5-1), more preferably (0.5-0.8):(0.5-0.8). The present invention can make each component react fully by controlling the ratio between the two.
[0086] In the present invention, the first halogenated hydrocarbon, the second solvent and the first polymer solution are preferably mixed by mixing the first halogenated hydrocarbon and the second solvent, and then dripping into the first polymer solution. The present invention has no special limitation on the dripping rate, which can be determined according to common sense. The dripping of the present invention can avoid overheating of the reaction.
[0087] The present invention has no special limitation on the amount of the second solvent, as long as the content of the first halogenated hydrocarbon in the mixed solution obtained by mixing the first halogenated hydrocarbon and the second solvent is within the range of 30 to 50 wt %.
[0088] In the present invention, the temperature of the first quaternization reaction is preferably 10 to 45° C., more preferably 25 to 30° C.; the time of the first quaternization reaction is preferably 1 to 12 hours, more preferably 6 to 10 hours.
[0089] The present invention has no particular limitation on the device for the first quaternization reaction, and a reaction device well known to those skilled in the art can be used. In the present invention, the device for the quaternization reaction is preferably a reactor.
[0090] After obtaining the second polymer solution, the present invention mixes the second polymer solution with the first fluorophosphorus salt aqueous solution to perform a first ion exchange reaction to obtain an ionic polymer binder. In the present invention, the halide ions and fluorophosphorus ions of the polymer undergo an ion exchange reaction.
[0091] In the present invention, the first fluorophosphate salt is preferably one or more of ammonium hexafluorophosphate, sodium hexafluorophosphate and potassium hexafluorophosphate; the concentration of the first fluorophosphate salt aqueous solution is preferably 30-45wt%. When the fluorophosphate salt is two or more of the above, the present invention has no special limitation on the ratio between the two or more, and any ratio can be mixed. The present invention has no special limitation on the preparation method of the fluorophosphate salt aqueous solution, and the fluorophosphate salt can be dissolved in water.
[0092] In the present invention, the molar ratio of the first fluorophosphorus salt to the first halogenated hydrocarbon is preferably 1:(0.5-1), more preferably 1:(0.5-0.8). The present invention can make the adhesive have better bonding performance by controlling the ratio between the two.
[0093] The present invention has no special limitation on the operation of mixing the second polymer solution with the first fluorophosphate salt aqueous solution, and the technical scheme for preparing the mixed material well known to those skilled in the art can be adopted.
[0094] In the present invention, the temperature of the first ion exchange reaction is preferably 10 to 45° C., more preferably 25° C.; the time of the first ion exchange reaction is preferably 1 to 12 hours, more preferably 6 to 10 hours. The present invention can avoid the occurrence of side reactions and enable the ion exchange reaction to proceed fully by controlling the temperature and time of the ion exchange reaction.
[0095] The present invention has no special limitation on the device for the ion exchange reaction, and a reaction device well known to those skilled in the art can be used. In the present invention, the device for the ion exchange reaction is preferably a reactor.
[0096] After the first ion exchange reaction is completed, the present invention preferably sequentially extracts and separates the ionic polymer binder oil-water two-phase mixture obtained by the first ion exchange reaction, performs vacuum distillation, cools, filters and dries to obtain the ionic polymer binder.
[0097] The present invention has no special limitation on the extraction and separation operation, and the operation well known to those skilled in the art can be adopted. The present invention adopts extraction and separation to remove the oil phase and obtain the ionic polymer binder aqueous phase dispersion.
[0098] The present invention has no special limitation on the operation of the vacuum distillation, and the operation well known to those skilled in the art can be used to concentrate the solid content to 10 to 45%, preferably 20 to 35%. The present invention can remove water and concentrate by vacuum distillation.
[0099] The present invention has no special limitation on the cooling operation, and the cooling to 5-10° C. is sufficient. In the present invention, the concentrated ionic polymer binder aqueous phase dispersion is cooled to 5-10° C., and the ionic polymer binder is precipitated.
[0100] The present invention has no particular limitation on the filtering operation, and any operation well known to those skilled in the art may be used.
[0101] In the present invention, the drying is preferably vacuum drying; the temperature of the vacuum drying is preferably 30 to 80° C., more preferably 50 to 60° C.; the time of the vacuum drying is preferably 1 to 24 hours, more preferably 12 to 24 hours.
[0102] The present invention also provides a method for preparing the ionic polymer binder described in the above technical solution, comprising the following steps:
[0103] 1) mixing dialkylamino acrylate, water and a second halogenated hydrocarbon, and performing a second quaternization reaction to obtain a trialkylamino acrylate halide aqueous solution;
[0104] 2) mixing the aqueous solution of trialkylamino acrylate halide obtained in step 1) with the aqueous solution of the second fluorophosphate salt, and performing a second ion exchange reaction to obtain trialkylamino acrylate fluorophosphate salt;
[0105] 3) mixing the trialkylamino acrylate fluoride phosphate obtained in step 2), polyethylene glycol acrylate, acrylate, a second initiator and water, and performing a second free radical polymerization reaction to obtain an ionic polymer binder with z>0 in the chemical structure of formula I;
[0106] When the acrylate is omitted in step 3), an ionic polymer binder with z=0 in the chemical structure of formula I is obtained;
[0107] When the polyethylene glycol acrylate and acrylate are omitted in step 3), an ionic polymer binder with a chemical structure of formula II is obtained.
[0108] The present invention has no particular limitation on the sources of the raw materials, and commercially available products known to those skilled in the art may be used.
[0109] The invention mixes dialkylamino acrylate, water and a second halogenated hydrocarbon, and performs a second quaternization reaction to obtain a trialkylamino acrylate halide aqueous solution.
[0110] In the present invention, the dialkylamino acrylate is preferably of the same type as the aforementioned dialkylamino acrylate, which will not be described in detail herein.
[0111] In the present invention, the type of the second halogenated hydrocarbon is preferably the same as the type of the first halogenated hydrocarbon, which will not be described in detail herein.
[0112] In the present invention, the molar ratio of the dialkylamino acrylate to the second halogenated hydrocarbon is preferably (0.5-1):(0.5-1), more preferably (0.5-0.8):(0.5-0.8). The present invention can make each component react fully by controlling the ratio between the two.
[0113] In the present invention, the mixture of the dialkylamino acrylate, water and the second halogenated hydrocarbon is preferably prepared by first mixing the dialkylamino acrylate and water and then adding the second halogenated hydrocarbon dropwise. The present invention has no particular limitation on the rate of the dropwise addition, which can be determined according to common sense. The dropwise addition in the present invention can avoid overheating of the reaction.
[0114] In the present invention, the concentration of dialkylamino acrylate in the mixed solution obtained by mixing dialkylamino acrylate and water is preferably 30 to 45 wt %.
[0115] In the present invention, the temperature and time of the second quaternization reaction are preferably the same as those of the first quaternization reaction, which will not be described in detail herein.
[0116] After obtaining the trialkylamino acrylate halide aqueous solution, the present invention mixes the trialkylamino acrylate halide aqueous solution and the second fluorophosphate salt aqueous solution to perform a second ion replacement reaction to obtain the trialkylamino acrylate fluorophosphate salt.
[0117] In the present invention, the second fluorophosphate salt aqueous solution is preferably the same as the first fluorophosphate salt aqueous solution, which will not be described in detail herein.
[0118] In the present invention, the molar ratio of the dialkylamino acrylate, the second halogenated hydrocarbon and the second fluorophosphonate is preferably (0.5-1): (0.5-1): 1, and more preferably (0.5-0.8): (0.5-0.8): 1. The present invention can fully carry out the reaction by controlling the ratio of the three.
[0119] The present invention has no special limitation on the operation of mixing the aqueous solution of trialkylamino acrylate halide and the aqueous solution of the second fluorophosphate salt, and the well-known technical scheme for preparing the mixed material can be used.
[0120] In the present invention, the temperature and time of the second ion exchange reaction are preferably the same as those of the first ion exchange reaction, which will not be described in detail herein.
[0121] After the second ion exchange reaction is completed, the present invention preferably filters and dries the product obtained by the second ion exchange reaction in sequence to obtain trialkylamino acrylate fluorophosphonium salt.
[0122] The present invention has no particular limitation on the filtering operation, and any operation well known to those skilled in the art may be used.
[0123] In the present invention, the drying is preferably vacuum drying; the temperature of the vacuum drying is preferably 20 to 40° C.; the time of the vacuum drying is preferably 6 to 24 hours, more preferably 12 to 24 hours.
[0124] After obtaining the trialkylamino acrylate fluoride phosphate, the present invention mixes the trialkylamino acrylate fluoride phosphate, polyethylene glycol acrylate, acrylate, a second initiator and water to perform a second free radical polymerization reaction to obtain an ionic polymer binder with z>0 in the chemical structure of formula I.
[0125] In the present invention, the polyethylene glycol acrylate and acrylate are preferably the same as those described above, and will not be described in detail herein.
[0126] In the present invention, the second initiator is preferably ammonium persulfate, potassium persulfate, sodium persulfate, azobisisobutylamidine hydrochloride or azobisisobutylimidazoline hydrochloride.
[0127] In the present invention, the mass of the second initiator is preferably 0.1-2% of the sum of the mass of trialkylamino acrylate fluoride phosphonate, polyethylene glycol acrylate and acrylate, more preferably 0.3-0.5%, and more preferably 0.4%. In the present invention, controlling the amount of the initiator within the above range can promote the free radical polymerization reaction to proceed fully.
[0128] In the present invention, the molar ratio of the trialkylamino acrylate fluorophosphate, polyethylene glycol acrylate and acrylate is preferably 1:(0.1-1.1):(0.1-1.1), more preferably 1:(0.5-1.0):(0.5-1.0).
[0129] The present invention has no particular limitation on the amount of water, as long as the total mass concentration of trialkylamino acrylate fluoride phosphate, polyethylene glycol acrylate and acrylate is maintained within the range of 10 to 50%, more preferably 20 to 30%. In the present invention, water within the above amount range is more conducive to the free radical polymerization reaction to proceed fully.
[0130] The present invention has no special limitation on the operation of mixing trialkylamino acrylate fluorophosphate, polyethylene glycol acrylate, acrylate, the second initiator and water, and the technical scheme for preparing the mixed material well known to those skilled in the art can be adopted.
[0131] In the present invention, the operation of the second free radical polymerization reaction is preferably the same as that of the first free radical polymerization reaction, which will not be described in detail herein.
[0132] After the second free radical polymerization reaction is completed, the present invention preferably sequentially performs reduced pressure distillation, cooling, filtration and drying on the product obtained by the second free radical polymerization reaction to obtain an ionic polymer binder with z>0 in the chemical structure of Formula I.
[0133] The present invention has no special limitation on the operation of the vacuum distillation, and the operation well known to those skilled in the art can be used to concentrate the solid content to 10-50%, preferably 20-35%. The present invention can remove water and concentrate by vacuum distillation.
[0134] The present invention has no special limitation on the cooling operation, and the cooling to 5-10° C. is sufficient. In the present invention, the concentrated ionic polymer binder aqueous phase dispersion is cooled to 5-10° C., and the ionic polymer binder is precipitated.
[0135] The present invention has no particular limitation on the filtering operation, and any operation well known to those skilled in the art may be used.
[0136] In the present invention, the drying is preferably vacuum drying; the temperature of the vacuum drying is preferably 30 to 80° C., more preferably 50 to 60° C.; the time of the vacuum drying is preferably 1 to 24 hours, more preferably 12 to 24 hours.
[0137] In the present invention, when acrylate is omitted, an ionic polymer binder with z=0 in the chemical structure of formula I is obtained; when polyethylene glycol acrylate and acrylate are omitted, an ionic polymer binder with the chemical structure of formula II is obtained.
[0138] The present invention also provides the use of the ionic polymer binder described in the above technical solution or the ionic polymer binder prepared by the preparation method described in the above technical solution in a positive electrode sheet of a lithium ion battery.
[0139] In the present invention, the method for preparing the positive electrode sheet of a lithium ion battery preferably comprises the following steps:
[0140] ① mixing the ionic polymer binder and the second organic solvent to obtain a binder solution;
[0141] ② Mixing the active material and the conductive agent to obtain a mixed powder;
[0142] ③ Mixing the binder solution obtained in step ①, the mixed powder obtained in step ② and a third organic solvent to obtain a positive electrode slurry;
[0143] ④ coating the positive electrode slurry obtained in step ③ on the current collector to obtain a positive electrode sheet for a lithium-ion battery;
[0144] There is no order of precedence between step ① and step ②.
[0145] In the present invention, the ionic polymer binder and the second organic solvent are preferably mixed to obtain a binder solution.
[0146] In the present invention, the second organic solvent is preferably one or more of N-methylpyrrolidone, tetrahydrofuran and acetonitrile. The present invention uses the above organic solvents, which have excellent solubility for ionic polymer binders.
[0147] The present invention has no particular limitation on the amount of the second organic solvent, as long as the viscosity of the binder solution is within the range of 0.1 to 10 Pa·s. In the present invention, when the viscosity of the binder solution is within the above range, the ionic polymer binder can be fully dissolved and the slurry can be controlled at an appropriate viscosity.
[0148] In the present invention, PVDF is preferably added to the binder solution; the mass ratio of the ionic polymer binder to PVDF is preferably 1:(0.1-1).
[0149] The present invention has no special limitation on the operation of mixing the ionic polymer binder and the second organic solvent, and the technical scheme for preparing the mixed material well known to those skilled in the art can be adopted.
[0150] In the present invention, the active material and the conductive agent are preferably mixed to obtain a mixed powder.
[0151] In the present invention, the active material preferably includes lithium iron phosphate (LiFePO4), lithium cobalt oxide (LiCoO2), lithium manganese oxide (LiMn2O4), nickel cobalt manganese (LiNi 0.8 Co 0.1 Mn 0.1 O2) or lithium titanate (Li4Ti5O 12 ). The present invention can make the lithium ion battery have good electrochemical performance by adopting the above-mentioned types of active materials.
[0152] In the present invention, the conductive agent preferably includes one or more of superconducting carbon, carbon nanotubes, acetylene black and Ketjen black. By selecting the conductive agent of the above type, the present invention can make the lithium ion battery have good electrochemical performance.
[0153] In the present invention, the mass ratio of the active material, the conductive agent and the ionic polymer binder is preferably (60-98): (1-20): (1-20), and more preferably (88-96): (2-6): (2-6). The present invention can make the lithium ion battery have good electrochemical performance by controlling the mass ratio of the active material, the conductive agent and the ionic polymer binder within the above range.
[0154] In the present invention, the mixing of the active material and the conductive agent preferably comprises: ball milling the active material and the conductive agent at room temperature at a speed of 600 to 1200 rpm for 1 to 4 hours, more preferably at a speed of 800 to 1000 rpm for 2 to 3 hours. In the present invention, the above method can be used to uniformly mix the active material and the conductive agent.
[0155] After obtaining the binder solution and the mixed powder, the present invention preferably mixes the binder solution, the mixed powder and a third organic solvent to obtain a positive electrode slurry.
[0156] In the present invention, the third organic solvent is preferably N-methylpyrrolidone.
[0157] In the present invention, the total concentration of the mixed powder and the binder in the positive electrode slurry is preferably 40 to 65 wt %, and more preferably 50 to 60 wt %.
[0158] In the present invention, the mixing of the binder solution, the mixed powder and the third organic solvent preferably includes: ball milling the mixed powder and the binder solution at a speed of 600 to 1200 rpm for 1 to 10 hours, then adding the third organic solvent and continuing ball milling for 1 to 4 hours, more preferably ball milling the mixed powder and the binder solution at a speed of 800 to 1000 rpm for 5 to 8 hours, then adding the third organic solvent and continuing ball milling for 2 to 3 hours. The present invention adopts the above mixing operation and controls its parameters within the above range, which is more conducive to fully mixing the raw materials.
[0159] After obtaining the positive electrode slurry, the present invention applies the positive electrode slurry on a current collector to obtain a positive electrode sheet for a lithium ion battery.
[0160] In the present invention, the current collector is preferably an aluminum foil. The present invention has no special limitation on the size of the aluminum foil, which can be adjusted according to actual needs.
[0161] In the present invention, the coating is preferably carried out using a scraper. The present invention has no particular limitation on the type of the scraper, and any equipment well known to those skilled in the art can be used.
[0162] The present invention has no special limitation on the thickness of the positive electrode slurry coating, which can be adjusted according to conventional needs. In the present invention, the coating thickness is preferably 60 to 500 μm.
[0163] After coating, the present invention preferably sequentially dries, rolls and cuts the coated product to obtain a positive electrode sheet for a lithium-ion battery.
[0164] In the present invention, the drying preferably includes atmospheric pressure drying and vacuum drying performed sequentially; the atmospheric pressure drying temperature is preferably 40-60°C; the atmospheric pressure drying time is preferably 6-24h; the vacuum drying temperature is preferably 80°C; the vacuum drying time is preferably 6-24h.
[0165] The present invention has no special limitation on the operations of rolling and cutting, and operations well known to those skilled in the art may be adopted.
[0166] The present invention adopts an ionic polymer binder as a positive electrode binder for a lithium ion battery. The interaction between hexafluorophosphate in the ionic polymer binder and the positive electrode active material can enhance the bonding between the materials and the conductivity of lithium ions. Polyethylene glycol acrylate can improve the flexibility of the binder and soften the pole piece. Since the active material of the positive electrode is relatively sensitive to water, acrylate is introduced as a hydrophobic segment to reduce the hydrophilicity of the polymer, thereby avoiding the problem of a decrease in battery capacity and cycle performance due to water absorption by the active material, thereby enabling the lithium ion battery assembled using the binder to have a higher specific capacity, capacity retention rate and cycle stability.
[0167] The present invention adopts an ionic polymer binder as a positive electrode binder for a lithium ion battery. Since the ionic polymer binder has excellent bonding properties, when the positive electrode of a lithium ion battery prepared by using the ionic polymer binder provided by the present invention is manufactured, the active material loading amount of the positive electrode can be increased, the pole piece is smooth, and there is no curling or cracking phenomenon. Moreover, the lithium ion battery assembled by using the binder has the advantages of large specific capacity, good cycle stability and long service life.
[0168] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0169] Example 1
[0170] Ionic polymer binders have the following chemical structure:
[0171]
[0172] In the corresponding formula I, R1 is hydrogen, R2 is methyl, R3 is hydrogen, x=0.67, y=0.33, z=0, m=2, n=9;
[0173] The molecular weight of the ionic polymer binder is 5.81×10 4 Da;
[0174] The preparation method of the ionic polymer binder is:
[0175] (1) under a nitrogen atmosphere, 1106 g of dimethylaminoethyl acrylate, 1894 g of polyethylene glycol acrylate, 12 g of azobisisobutyronitrile and 7000 g of dimethyl carbonate were mixed in a reaction kettle, and free radical polymerization was carried out at 70° C. for 8 h to obtain a first polymer solution;
[0176] (2) adding 2750 g of a 40 wt % iodomethane dimethyl carbonate solution dropwise to the first polymer solution obtained in step (1), stirring at 25° C. for 6 h to carry out a quaternization reaction to obtain a second polymer solution;
[0177] (3) The second polymer solution obtained in step (2) is added dropwise to 8393 g of a 30 wt% aqueous solution of ammonium hexafluorophosphate, and stirred at 25° C. for 6 h to perform an ion exchange reaction to obtain an oil-water two-phase mixture containing an ionic polymer binder; then, extraction and separation are performed to remove the oil phase to obtain an ionic polymer binder aqueous phase dispersion; thereafter, the aqueous phase dispersion is concentrated by vacuum distillation to a solid content of 35 wt%, and then cooled to 5° C. to precipitate the ionic polymer binder, filtered, and finally dried at 60° C. in a vacuum oven for 12 h to obtain 3898 g of an ionic polymer binder, which is recorded as A1.
[0178] The NMR spectrum of the ionic polymer binder prepared in Example 1 is as follows: Figure 1 shown.
[0179] Example 2
[0180] Ionic polymer binders have the following chemical structure:
[0181]
[0182] In the corresponding formula I, R1 is hydrogen, R2 is methyl, R3 is hydrogen, x=0.60, y=0.40, z=0, m=2, n=9;
[0183] The molecular weight of the ionic polymer binder is 5.51×10 4 Da;
[0184] The preparation method of the ionic polymer binder is as follows:
[0185] (1) under a nitrogen atmosphere, 924 g of dimethylaminoethyl acrylate, 2076 g of polyethylene glycol acrylate, 12 g of azobisisobutyronitrile and 7000 g of dimethyl carbonate were mixed in a reaction kettle, and free radical polymerization was carried out at 70° C. for 8 h to obtain a first polymer solution;
[0186] (2) adding 2277 g of a 40 wt % iodomethane dimethyl carbonate solution dropwise to the first polymer solution obtained in step (1), stirring at 25° C. for 6 h to carry out a quaternization reaction to obtain a second polymer solution;
[0187] (3) The second polymer solution obtained in step (2) is added dropwise to 7020 g of a 30 wt% aqueous solution of ammonium hexafluorophosphate, and stirred at 25° C. for 6 h to perform an ion exchange reaction to obtain an oil-water two-phase mixture containing an ionic polymer binder; then, extraction and separation are performed to remove the oil phase to obtain an ionic polymer binder aqueous phase dispersion; thereafter, the aqueous phase dispersion is concentrated by vacuum distillation to a solid content of 35 wt%, and then cooled to 5° C. to precipitate the ionic polymer binder, filtered, and finally dried in vacuo at 60° C. for 12 h to obtain 3711 g of an ionic polymer binder, which is recorded as A2.
[0188] Example 3
[0189] Ionic polymer binders have the following chemical structure:
[0190]
[0191] In the corresponding formula I, R1 is hydrogen, R2 is methyl, R3 is hydrogen, x=0.72, y=0.28, z=0, m=2, n=9;
[0192] The molecular weight of the ionic polymer binder is 6.06×10 4 Da;
[0193] The preparation method of the ionic polymer binder is as follows:
[0194] (1) under a nitrogen atmosphere, 1278 g of dimethylaminoethyl acrylate, 1722 g of polyethylene glycol acrylate, 12 g of azobisisobutyronitrile and 7000 g of dimethyl carbonate were mixed in a reaction kettle, and free radical polymerization was carried out at 70° C. for 8 h to obtain a first polymer solution;
[0195] (2) adding 3150 g of a 40 wt % iodomethane-dimethyl carbonate solution dropwise to the first polymer solution obtained in step (1), stirring at 25° C. for 6 h to carry out a quaternization reaction to obtain a second polymer solution;
[0196] (3) The second polymer solution obtained in step (2) was added dropwise to 9710 g of a 30 wt% aqueous solution of ammonium hexafluorophosphate, and stirred at 25° C. for 6 h to perform an ion exchange reaction to obtain an oil-water two-phase mixture containing an ionic polymer binder; then, the mixture was extracted and separated to remove the oil phase to obtain an ionic polymer binder aqueous dispersion; the aqueous dispersion was then concentrated by vacuum distillation to a solid content of 35 wt%, and then cooled to 5° C. to precipitate the ionic polymer binder, filtered, and finally dried in vacuo at 60° C. for 12 h to obtain 4076 g of an ionic polymer binder, recorded as A3.
[0197] Example 4
[0198] Ionic polymer binders have the following chemical structure:
[0199]
[0200] In the corresponding formula I, R1 is hydrogen, R2 is methyl, R3 and R4 are hydrogen, R5 is butyl, x=0.66, y=0.17, z=0.17, m=2, n=9;
[0201] The molecular weight of the ionic polymer binder is 6.35×10 4 Da;
[0202] The preparation method of the ionic polymer binder is:
[0203] (1) under a nitrogen atmosphere, 1452 g of dimethylaminoethyl acrylate, 1223 g of polyethylene glycol acrylate, 325 g of butyl acrylate, 12 g of azobisisobutyronitrile and 7000 g of dimethyl carbonate were mixed in a reaction kettle, and free radical polymerization was carried out at 70° C. for 8 h to obtain a first polymer solution;
[0204] (2) adding 3580 g of a 40 wt % iodomethane dimethyl carbonate solution dropwise to the first polymer solution obtained in step (1), stirring at 25° C. for 6 h to carry out a quaternization reaction to obtain a second polymer solution;
[0205] (3) The second polymer solution obtained in step (2) was added dropwise to 11034 g of a 30 wt% aqueous solution of ammonium hexafluorophosphate, and stirred at 25° C. for 6 h to carry out an ion exchange reaction to obtain an oil-water two-phase mixture containing an ionic polymer binder; then, extraction and separation were performed to remove the oil phase to obtain an ionic polymer binder aqueous dispersion; then, the aqueous dispersion was concentrated by vacuum distillation to a solid content of 35 wt%, and then cooled to 5° C. to precipitate the ionic polymer binder, filtered, and finally dried in vacuo at 60° C. for 12 h to obtain 4155 g of an ionic polymer binder, which was recorded as A4.
[0206] Example 5
[0207] Ionic polymer binders have the following chemical structure:
[0208]
[0209] In the above structure, R1 in the corresponding formula I is hydrogen, R2 is methyl, R3 is hydrogen, x=0.60, y=0.40, z=0, m=2, n=9;
[0210] The molecular weight of the ionic polymer binder is 6.74×10 4 Da;
[0211] The preparation method of the ionic polymer binder is:
[0212] In a nitrogen atmosphere, 971 g of trimethylaminoethyl acrylate fluorophosphate, 1029 g of polyethylene glycol acrylate, 8 g of potassium persulfate and 8000 g of water were mixed in a reaction kettle, and free radical polymerization was carried out at 70° C. for 8 h to obtain an ionic polymer binder aqueous dispersion; the aqueous dispersion was then concentrated by vacuum distillation to a solid content of 35%, and then cooled to 5° C. to precipitate the ionic polymer binder, which was then filtered and finally vacuum dried at 60° C. for 12 h to obtain 1863 g of an ionic polymer binder, which was recorded as A5;
[0213] The structural formula of the trimethylaminoethyl acrylate fluorophosphonate is as follows:
[0214]
[0215] The preparation method of the trimethylaminoethyl acrylate fluorophosphonate is:
[0216] (1) 197 g of methyl iodide was added dropwise to 667 g of a 30 wt % aqueous solution of dimethylaminoethyl acrylate, and the mixture was stirred at 25° C. for 6 h to carry out a quaternization reaction to obtain an aqueous solution of trimethylaminoethyl acrylate iodide salt;
[0217] (2) 1014 g of a 45 wt% aqueous solution of ammonium hexafluorophosphate was added dropwise to the aqueous solution of trimethylaminoethyl acrylate iodide salt obtained in step (1), and the mixture was stirred at 25° C. for 8 h to carry out an ion exchange reaction, and a white precipitate was precipitated, which was then filtered. The precipitate was then vacuum dried at 30° C. for 12 h to obtain 401 g of trimethylaminoethyl acrylate iodide salt.
[0218] The NMR spectrum of trimethylaminoethyl acrylate fluorophosphonate in Example 5 is as follows Figure 2 shown.
[0219] Example 6
[0220] Ionic polymer binders have the following chemical structure:
[0221]
[0222] In the above structure, R1 in the corresponding formula I is hydrogen, R2 is methyl, R3 is hydrogen, x=0.67, y=0.33, z=0, m=2, n=9;
[0223] The molecular weight of the ionic polymer binder is 9.01×10 4 Da;
[0224] The preparation method of the ionic polymer binder is:
[0225] Under a nitrogen atmosphere, 1114 g of trimethylaminoethyl acrylate fluorophosphate, 886 g of polyethylene glycol acrylate, 6 g of potassium persulfate and 8000 g of water were mixed in a reactor, and a free radical polymerization reaction was carried out at 70° C. for 8 hours to obtain an ionic polymer binder aqueous dispersion; the aqueous dispersion was then concentrated by reduced pressure distillation to a solid content of 35%, and then cooled to 5° C., the ionic polymer binder was precipitated, filtered, and then vacuum dried at 60° C. for 12 hours to obtain 1879 g of ionic polymer binder, recorded as A6; the preparation method of the trimethylaminoethyl acrylate fluorophosphate is the same as that in Example 5.
[0226] Example 7
[0227] Ionic polymer binders have the following chemical structure:
[0228]
[0229] In the above structure, R1 in the corresponding formula I is hydrogen, R2 is methyl, R3 is hydrogen, x=0.72, y=0.28, z=0, m=2, n=9;
[0230] The molecular weight of the ionic polymer binder is 7.68×10 4 Da;
[0231] The preparation method of the ionic polymer binder is:
[0232] Under a nitrogen atmosphere, 1222 g of trimethylaminoethyl acrylate fluorophosphate, 778 g of polyethylene glycol acrylate, 10 g of potassium persulfate and 8000 g of water were mixed in a reactor, and a free radical polymerization reaction was carried out at 70° C. for 8 hours to obtain an ionic polymer binder aqueous dispersion; the aqueous dispersion was then concentrated by reduced pressure distillation to a solid content of 35%, and then cooled to 5° C., the ionic polymer binder was precipitated, then filtered, and finally vacuum dried at 60° C. for 12 hours to obtain 1895 g of ionic polymer binder, recorded as A7; the preparation method of the trimethylaminoethyl acrylate fluorophosphate is the same as that in Example 5.
[0233] Example 8
[0234] Ionic polymer binders have the following chemical structure:
[0235]
[0236] In the above structure, R1 in the corresponding formula I is hydrogen, R2 is methyl, R3 and R4 are hydrogen, R5 is butyl, x=0.66, y=0.17, z=0.17, m=2, n=9;
[0237] The molecular weight of the ionic polymer binder is 8.98×10 4 Da;
[0238] The preparation method of the ionic polymer binder is:
[0239] Under a nitrogen atmosphere, 1330 g of trimethylaminoethyl acrylate fluorophosphate, 529 g of polyethylene glycol acrylate, 141 g of butyl acrylate, 6 g of potassium persulfate and 8000 g of water were mixed in a reactor, and a free radical polymerization reaction was carried out at 70° C. for 8 hours to obtain an ionic polymer binder aqueous dispersion; the aqueous dispersion was then concentrated by reduced pressure distillation to a solid content of 35%, and then cooled to 5° C., the ionic polymer binder was precipitated, then filtered, and finally vacuum dried at 60° C. for 12 hours to obtain 1831 g of ionic polymer binder, recorded as A8; the preparation method of the trimethylaminoethyl acrylate fluorophosphate is the same as that in Example 5.
[0240] Example 9
[0241] Ionic polymer binders have the following chemical structure:
[0242]
[0243] In the above structure, R6 in formula II is hydrogen, R7 is ethylene, R8, R9, R 10 is methyl, q is 297;
[0244] The molecular weight of the ionic polymer binder is 9.01×10 4 Da;
[0245] The preparation method of the ionic polymer binder comprises the following steps:
[0246] Under a nitrogen atmosphere, 1000 g of trimethylaminoethyl acrylate fluorophosphate, 3 g of potassium persulfate and 4000 g of water were mixed in a reactor, and a free radical polymerization reaction was carried out at 70° C. for 8 hours to obtain an ionic polymer binder aqueous dispersion; the aqueous dispersion was then concentrated by reduced pressure distillation to a solid content of 35 wt %, and then cooled to 5° C., the ionic polymer binder was precipitated, then filtered, and finally vacuum dried at 60° C. for 12 hours to obtain 477 g of ionic polymer binder, recorded as A9; the preparation method of the trimethylaminoethyl acrylate fluorophosphate is the same as that in Example 5.
[0247] The NMR spectrum of the ionic polymer binder prepared in Example 9 is as follows: Figure 3 shown.
[0248] Example 10
[0249] Ionic polymer binders have the following chemical structure:
[0250]
[0251] In the above structure, R6 in formula II is hydrogen, R7 is ethylene, R8, R9, R 10 is methyl, q is 287;
[0252] The molecular weight of the ionic polymer binder is 8.69×10 4 Da;
[0253] The preparation method of the ionic polymer binder comprises the following steps:
[0254] (1) Under a nitrogen atmosphere, 1000 g of dimethylaminoethyl acrylate, 4 g of azobisisobutyronitrile and 4000 g of dimethyl carbonate were mixed in a reaction kettle, and a free radical polymerization reaction was carried out at 70° C. for 8 h to obtain a polydimethylaminoethyl acrylate solution;
[0255] (2) adding 3287 g of a 30 wt % iodomethane dimethyl carbonate solution dropwise to the polydimethylaminoethyl acrylate solution obtained in step (1), stirring at 25° C. for 6 h to carry out a quaternization reaction to obtain a polytrimethylaminoethyl acrylate iodide salt solution;
[0256] (3) The poly(trimethylaminoethyl)acrylate iodide salt solution obtained in step (2) is added dropwise to 7597 g of a 30 wt % aqueous solution of ammonium hexafluorophosphate, and the mixture is stirred at 25° C. for 6 h to perform an ion exchange reaction to obtain an oil-water two-phase mixture containing an ionic polymer binder, and then extracted and separated to remove the oil phase to obtain an ionic polymer binder aqueous phase dispersion; the aqueous phase dispersion is then concentrated by reduced pressure distillation to a solid content of 35 wt %, and then cooled to 5° C. to precipitate the ionic polymer binder, which is then filtered and finally dried in vacuo at 60° C. for 12 h to obtain 1988 g of an ionic polymer binder, which is recorded as A10.
[0257] Embodiment 11
[0258] Ionic polymer binders have the following chemical structure:
[0259]
[0260] In the above structure, R6 in Formula II is methyl, R7 is propylene, R8, R9, R 10 is methyl, q is 205;
[0261] The molecular weight of the ionic polymer binder is 6.76×10 4 Da;
[0262] The preparation method of the ionic polymer binder comprises the following steps:
[0263] In a nitrogen atmosphere, 500 g of 3-(trimethylamino) methyl methacrylate propyl fluoride phosphate, 2 g of potassium persulfate and 2000 g of water were mixed in a reactor, and a free radical polymerization reaction was carried out at 70° C. for 8 h to obtain an ionic polymer binder aqueous dispersion; the aqueous dispersion was then concentrated by vacuum distillation to a solid content of 35 wt %, and then cooled to 5° C. to precipitate the ionic polymer binder, which was then filtered and finally vacuum dried at 60° C. for 12 h to obtain 483 g of an ionic polymer binder, which was recorded as A11;
[0264] The structural formula of the 3-(trimethylamino)propyl methacrylate fluorophosphonate is as follows:
[0265]
[0266] The preparation method of the 3-(trimethylamino)propyl methacrylate fluorophosphonate is as follows:
[0267] (1) 412 g of methyl iodide was added dropwise to 1667 g of a 30 wt% aqueous solution of 3-(dimethylamino)propyl methacrylate, and the mixture was stirred at 25° C. for 6 h to carry out a quaternization reaction to obtain an aqueous solution of iodine salt of 3-(trimethylamino)propyl methacrylate;
[0268] (2) 2117 g of a 45 wt% aqueous solution of ammonium hexafluorophosphate was added dropwise to the aqueous solution of 3-(trimethylamino) methacrylate propyl iodide obtained in step (1), and the mixture was stirred at 25° C. for 8 h to carry out an ion exchange reaction, and a white precipitate was precipitated. The precipitate was vacuum dried at 30° C. for 12 h to obtain 941 g of 3-(trimethylamino) methacrylate propyl fluorophosphate.
[0269] Example 12
[0270] Ionic polymer binders have the following chemical structure:
[0271]
[0272] In the above structure, R6 in formula II is methyl, R7 is ethylene, R8, R9, R 10 is methyl, q is 341;
[0273] The molecular weight of the ionic polymer binder is 1.08×10 5 Da;
[0274] The preparation method of the ionic polymer binder comprises the following steps:
[0275] In a nitrogen atmosphere, 1000 g of trimethylaminoethyl methacrylate fluorophosphate, 2.5 g of potassium persulfate and 4000 g of water were mixed in a reactor, and a free radical polymerization reaction was carried out at 70° C. for 8 h to obtain an ionic polymer binder aqueous dispersion; the aqueous dispersion was then concentrated by vacuum distillation to a solid content of 35 wt %, and then cooled to 5° C. to precipitate the ionic polymer binder, which was then filtered to obtain a solid product, and finally vacuum dried at 60° C. for 12 h to obtain 485 g of an ionic polymer binder, which was recorded as A12;
[0276] The structural formula of the trimethylaminoethyl methacrylate fluorophosphonate is as follows:
[0277]
[0278] The preparation method of the trimethylaminoethyl methacrylate fluorophosphonate is:
[0279] (1) adding 452 g of methyl iodide dropwise to 1667 g of a 30 wt % aqueous solution of dimethylaminoethyl methacrylate, stirring at 25° C. for 6 h to carry out a quaternization reaction to obtain an aqueous solution of trimethylaminoethyl methacrylate iodide salt;
[0280] (2) 2307 g of a 45 wt% ammonium hexafluorophosphate aqueous solution was added dropwise to the aqueous solution of trimethylaminoethyl methacrylate iodine salt obtained in step (1), and the mixture was stirred at 25° C. for 8 h to carry out an ion exchange reaction, and a white precipitate was precipitated. The precipitate was vacuum dried at 30° C. for 12 h to obtain 1002 g of trimethylaminoethyl methacrylate fluorophosphate.
[0281] Comparative Example 1
[0282] 1000 g of PVDF (HSV900) and 9000 g of N-methylpyrrolidone were mixed in a reaction kettle and stirred at 25° C. for 12 h to obtain a binder solution, which was recorded as B1.
[0283] Comparative Example 2
[0284] 400 g of sodium carboxymethyl cellulose powder (MAC500LC, Shenzhen Kejing), 1712 g of styrene-butadiene rubber latex (Shenzhen Kejing, S2919, the mass fraction of the polymer is 35%) and 9000 g of pure water (resistivity greater than 0.1 MΩ·cm) were mixed in a reactor and stirred at 25° C. for 12 h to obtain a binder solution, which was recorded as B2.
[0285] Application Examples 1 to 8
[0286] A1 to A8 prepared in Examples 1 to 8 are respectively used as the ionic polymer binder in step 1) of the following preparation method to prepare positive electrode sheets of lithium ion batteries, which are C1 to C8 in sequence. For example, the positive electrode sheet prepared using the ionic polymer binder A1 in Example 1 is C1, and the same applies to the following;
[0287] The preparation method of the positive electrode sheet of a lithium-ion battery is as follows:
[0288] 1) dissolving 10 g of an ionic polymer binder in 90 g of N-methylpyrrolidone to obtain a binder solution having a viscosity of 102 mPa·s;
[0289] 2) 180 g of lithium iron phosphate and 10 g of superconducting carbon black were ball-milled at a speed of 1008 rpm for 2 h to obtain a mixed powder; wherein the mass ratio of the positive electrode active material, the conductive agent and the ionic polymer binder was 90:5:5;
[0290] 3) ball-milling the binder solution obtained in step 1) and the mixed powder obtained in step 2) at 1008 rpm for 4 h, adding 100 g of N-methylpyrrolidone and continuing ball-milling for 4 h to obtain a positive electrode slurry;
[0291] 4) The positive electrode slurry obtained in step 3) is coated on an aluminum foil with a coating thickness of 250 μm. The aluminum foil coated with the positive electrode slurry is first dried at 60° C. under normal pressure for 12 h, then vacuum dried at 80° C. for 12 h, rolled and cut to obtain a positive electrode sheet for a lithium-ion battery.
[0292] Application Examples 9 to 16
[0293] A1 to A8 prepared in Examples 1 to 8 are respectively used as the ionic polymer in step 1) of the following preparation method, and are dissolved in N-methylpyrrolidone with PVDF (HSV900) at a mass ratio of 7:3 to obtain a binder solution, and the prepared positive electrode sheets of lithium ion batteries are C9 to C16 in sequence, such as: the ionic polymer binder A1 of Example 1 is dissolved in N-methylpyrrolidone with PVDF at a mass ratio of 7:3, and the prepared positive electrode sheet is C9, and the following is deduced in the same manner;
[0294] The preparation method of the positive electrode sheet of a lithium-ion battery is as follows:
[0295] 1) dissolving 7 g of ionic polymer binder and 3 g of PVDF in 90 g of N-methylpyrrolidone to obtain a binder solution having a viscosity of 114 mPa·s;
[0296] 2) 180 g of lithium iron phosphate and 10 g of superconducting carbon black were ball-milled at a speed of 1008 rpm for 2 h to obtain a mixed powder; wherein the mass ratio of the positive electrode active material, the conductive agent and the ionic polymer binder was 90:5:5;
[0297] 3) ball-milling the binder solution obtained in step 1) and the mixed powder obtained in step 2) at 1008 rpm for 4 h, adding 100 g of N-methylpyrrolidone and continuing ball-milling for 4 h to obtain a positive electrode slurry;
[0298] 4) The positive electrode slurry obtained in step 3) is coated on an aluminum foil with a coating thickness of 250 μm. The aluminum foil coated with the positive electrode slurry is first dried at 60° C. under normal pressure for 12 h, then vacuum dried at 80° C. for 12 h, rolled and cut to obtain a positive electrode sheet for a lithium-ion battery.
[0299] Application Examples 17-20
[0300] The ionic polymer binders A9 to A12 prepared in Examples 9 to 12 were respectively used as the ionic polymers in step 1) of the following preparation method, and dissolved in N-methylpyrrolidone with PVDF (HSV900) at a mass ratio of 8:2 to obtain a binder solution, and the positive electrode sheets of the prepared lithium-ion batteries were C17 to C20 in order;
[0301] The preparation method of the positive electrode sheet of a lithium-ion battery is as follows:
[0302] 1) dissolving 8 g of ionic polymer binder and 2 g of PVDF in 90 g of N-methylpyrrolidone to obtain a binder solution;
[0303] 2) 180 g of lithium iron phosphate and 10 g of superconducting carbon black were ball-milled at a speed of 1008 rpm for 2 h to obtain a mixed powder; wherein the mass ratio of the positive electrode active material, the conductive agent and the ionic polymer binder was 90:5:5;
[0304] 3) ball-milling the binder solution obtained in step 1) and the mixed powder obtained in step 2) at 1008 rpm for 4 h, adding 100 g of N-methylpyrrolidone and continuing ball-milling for 4 h to obtain a positive electrode slurry;
[0305] 4) The positive electrode slurry obtained in step 3) is coated on an aluminum foil with a coating thickness of 250 μm. The aluminum foil coated with the positive electrode slurry is first dried at 60° C. under normal pressure for 12 h, then vacuum dried at 80° C. for 12 h, rolled and cut to obtain a positive electrode sheet for a lithium-ion battery.
[0306] Comparative application example 1
[0307] The preparation method of the positive electrode sheet of a lithium-ion battery is as follows:
[0308] 1) Adhesive B1 prepared in Comparative Example 1 was used as the adhesive solution, and 100 g was taken;
[0309] 2) ball milling 180 g of lithium iron phosphate and 10 g of superconducting carbon black at a rotation speed of 1008 rpm for 2 h to obtain a mixed powder;
[0310] 3) ball-milling the binder solution obtained in step 1) and the mixed powder obtained in step 2) at 1008 rpm for 4 h, adding 100 g of N-methylpyrrolidone and continuing ball-milling for 4 h to obtain a positive electrode slurry;
[0311] 4) The positive electrode slurry obtained in step 3) is coated on an aluminum foil with a coating thickness of 250 μm. The aluminum foil coated with the positive electrode slurry is first dried at 60° C. under normal pressure for 12 h, then vacuum dried at 80° C. for 12 h, rolled and cut to obtain a lithium-ion battery positive electrode sheet, numbered C21.
[0312] Comparative Application Example 2
[0313] The preparation method of the negative electrode sheet of a lithium-ion battery is as follows:
[0314] 1) Adhesive B2 prepared in Comparative Example 2 was used as the adhesive solution, and 60 g was taken;
[0315] 2) 188 g of artificial graphite and 6 g of superconducting carbon black were ball-milled at a speed of 1008 rpm for 2 h to obtain a mixed powder;
[0316] 3) ball-milling the binder solution obtained in step 1) and the mixed powder obtained in step 2) at 1008 rpm for 4 h, adding 136 g of pure water (resistivity greater than 0.1 MΩ·cm) and continuing ball-milling for 4 h to obtain a negative electrode slurry;
[0317] 4) The negative electrode slurry obtained in step 3) is coated on the copper foil with a coating thickness of 300 μm. The copper foil coated with the negative electrode slurry is first dried at 60° C. under normal pressure for 12 h, then vacuum dried at 80° C. for 12 h, rolled and cut to obtain a negative electrode sheet for a lithium-ion battery, numbered C22.
[0318] Test Example 1
[0319] The viscosity average molecular weight M of the ionic polymer binders prepared in Examples 1 to 12 is η The thermal decomposition temperature of the ionic polymer binder was measured by a thermogravimetric analyzer (TG209, NETZSCH, Germany) under a nitrogen atmosphere from 25°C to 600°C at a heating rate of 10°C min -1 , the specific results are shown in Table 1:
[0320] Table 1 Performance indicators of ionic polymer binders
[0321] Ionomer Binder <![CDATA[Viscosity-average molecular weight M η (Da)]]> Thermal decomposition temperature (℃) A1 <![CDATA[5.81×10 4 ]]> 326 A2 <![CDATA[5.51×10 4 ]]> 321 A3 <![CDATA[6.06×10 4 ]]> 319 A4 <![CDATA[6.35×10 4 ]]> 323 A5 <![CDATA[6.74×10 4 ]]> 318 A6 <![CDATA[9.01×10 4 ]]> 325 A7 <![CDATA[7.68×10 4 ]]> 317 A8 <![CDATA[8.98×10 4 ]]> 320 A9 <![CDATA[9.01×10 4 ]]> 328 A10 <![CDATA[8.69×10 4 ]]> 321 A11 <![CDATA[6.76×10 4 ]]> 318 A12 <![CDATA[1.08×10 5 ]]> 334
[0322] It can be seen from Table 1 that the molecular weight of the ionic polymer binder is 5.5×10 4 ~1.1×10 5 Da range, which is much lower than the molecular weight of commercial PVDF, such as PVDFHSV900 (molecular weight of 6.0×10 5 Da), it can be expected that under the same conditions, the slurry prepared by the ionic polymer binder of the present invention has a lower viscosity and is easier to coat; the thermal decomposition of the ionic polymer binder is higher than that of PVDF (316°C), so it has good heat resistance and can meet the needs of the battery operating at high temperature.
[0323] Test Example 2
[0324] The surface density of the active material of the positive electrode sheets C1 to C21 of the lithium-ion battery is the mass of lithium iron phosphate per unit area, which is obtained by calculation; the peel strength between the dry slurry coating on the surface of the current collector in the electrode sheet and the current collector is determined according to the GB / T2791-1995 test method; the surface density and peel strength are shown in Table 2.
[0325] The method of assembling a lithium iron phosphate / metal lithium battery using the prepared C1 to C21 as the positive electrode of the battery and lithium metal as the negative electrode of the battery is as follows:
[0326] A lithium iron phosphate / metal lithium battery was obtained by using a commercial lithium hexafluorophosphate electrolyte as the electrolyte with a concentration of 1 mol / L, a molar ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate of 1:1:1, and a polypropylene microporous membrane (Celgard2325) as the separator.
[0327] Battery specific capacity refers to the initial discharge specific capacity and the 500th cycle discharge specific capacity of the assembled lithium iron phosphate / metal lithium battery at a current density of 0.5C. The test instrument is a battery cycle tester (Wuhan Blue Electric, CT3002A), with a cut-off voltage of 2.5-4.2V, a test temperature of 25°C, and a theoretical specific capacity of the active material of 170mAh / g. The results of the surface density, peel strength, initial discharge specific capacity, 500th cycle discharge specific capacity and retention rate (ratio of discharge specific capacity to initial discharge specific capacity) of the lithium iron phosphate pole piece tested are shown in Table 2.
[0328] Table 2 Performance indicators of lithium iron phosphate / metal lithium batteries
[0329]
[0330]
[0331] Figure 4The long cycle charge and discharge curve of the battery assembled with C1 as the positive electrode and lithium metal as the negative electrode at 25°C, a cut-off voltage of 2.5-4.2V and a rate of 0.5C; Figure 5 The charge and discharge curves of the battery assembled with C1 as the positive electrode and lithium metal as the negative electrode at 25°C and a cut-off voltage of 2.5-4.2V under different rate conditions such as 0.1C, 0.2C and 0.5C; Figure 6 The long cycle charge and discharge curve of a battery assembled with C17 as the positive electrode and lithium metal as the negative electrode at 25°C, a cut-off voltage of 2.5-4.2V and a rate of 0.5C; Figure 7 The charge and discharge curves of a battery assembled with C17 as the positive electrode and lithium metal as the negative electrode at 25°C and a cut-off voltage of 2.5-4.2V under different rate conditions such as 0.1C, 0.2C and 0.5C.
[0332] From Table 2 and Figures 4 to 7 It can be seen that under the condition of similar lithium iron phosphate surface density, the lithium iron phosphate positive electrode sheets C9 to C16 prepared by the ionic polymer binder of the present invention and PVDF at a mass ratio of 7:3 and the lithium iron phosphate positive electrode sheets C17 to C20 prepared at a mass ratio of 8:2 have higher peel strength, that is, better bonding strength between the active material and the current collector, than the lithium iron phosphate sheets C1 to C8 prepared by the ionic polymer binder alone and the lithium iron phosphate positive electrode sheet C21 prepared by the PVDF binder alone. The lithium iron phosphate / metal lithium battery assembled with the lithium iron phosphate positive electrode sheets C1 to C8 and C17 to C20 and metallic lithium has a higher initial discharge specific capacity than the battery assembled with the lithium iron phosphate positive electrode sheet C21, and also has a higher discharge specific capacity and capacity retention rate after 500 cycles at a current density of 0.5C, especially the lithium iron phosphate / metal lithium battery assembled with C1 and C17 has the best performance.
[0333] Test Example 3
[0334] The method of assembling a lithium iron phosphate / artificial graphite battery using the prepared C1, C17 or C21 as a lithium iron phosphate positive electrode sheet and C22 as an artificial graphite negative electrode sheet is as follows:
[0335] Using commercial lithium hexafluorophosphate electrolyte as the electrolyte with a concentration of 1 mol / L, the molar ratio of ethylene carbonate, dimethyl carbonate and diethyl carbonate is 1:1:1, and a polypropylene microporous membrane (Celgard2325) as the separator, lithium iron phosphate / artificial graphite batteries were obtained and named D1~D3 respectively.
[0336] The assembled D1-D3 lithium iron phosphate / artificial graphite batteries were subjected to battery cycle testing in a battery cycle tester (Wuhan Blue Electric, CT3002A), wherein the cut-off voltage was 2.5-4.2V, the test temperature was 25°C, the multiple was 0.5C, and the theoretical specific capacity of the active material was 170mAh / g. The results of the initial specific capacity of the battery cycle, the 800th cycle discharge specific capacity, and the capacity retention rate (the ratio of the discharge specific capacity to the initial discharge specific capacity) obtained by the test are shown in Table 3; the results of the initial specific capacity of the battery cycle, the 1000th cycle discharge specific capacity, and the capacity retention rate (the ratio of the discharge specific capacity to the initial discharge specific capacity) obtained by the test are shown in Table 4.
[0337] Table 3 Performance indicators of lithium iron phosphate / artificial graphite batteries
[0338]
[0339] Figure 8 This is the long cycle charge and discharge curve of the lithium iron phosphate / artificial graphite battery assembled with C1 as the positive electrode sheet and C22 as the negative electrode sheet at 25°C, a cut-off voltage of 2.5-4.2V and a rate of 0.5C.
[0340] From Table 3 and Figure 8 It can be seen that the full battery assembled with the lithium iron phosphate positive electrode sheet C1 and the artificial graphite negative electrode sheet C22 prepared with SBR / CMC binder has a higher initial discharge specific capacity than the full battery assembled with the lithium iron phosphate positive electrode sheet C21 prepared with PVDF binder. After 800 cycles at a current density of 0.5C, it can still maintain 137.8mAhg -1 , capacity retention rate is 92.11%, and the cycle performance is excellent.
[0341] Table 4 Performance indicators of lithium iron phosphate / artificial graphite batteries
[0342]
[0343] Fig. 9 This is the long cycle charge and discharge curve of the lithium iron phosphate / artificial graphite battery assembled with C17 as the positive electrode and C22 as the negative electrode at 25°C, a cut-off voltage of 2.5-4.2V and a rate of 0.5C.
[0344] Table 4 and Fig. 9 It can be seen that the lithium iron phosphate / artificial graphite battery assembled with the lithium iron phosphate positive electrode sheet C17 and the artificial graphite negative electrode sheet C22 prepared with SBR / CMC binder has a higher initial discharge specific capacity than the battery assembled with the lithium iron phosphate electrode sheet C21, and also has a higher discharge specific capacity and battery long cycle capacity retention rate after 1000 cycles at a current density of 0.5C.
[0345] It can be seen from the above embodiments that when the ionic polymer binder provided by the present invention is used to prepare the positive electrode of a lithium ion battery, it has excellent adhesion to the active material. This is because the interaction between the hexafluorophosphate in the ionic polymer binder and the positive electrode active material can enhance the adhesion between the materials and the conductivity of lithium ions, thereby increasing the active material loading of the positive electrode; polyethylene glycol acrylate can improve the flexibility of the binder and soften the pole piece; since the active material of the positive electrode is sensitive to water, acrylate is introduced as a hydrophobic segment to reduce the hydrophilicity of the polymer, thereby avoiding the problem of a decrease in battery capacity and cycle performance after the active material absorbs water, thereby making the lithium ion battery assembled using the binder have a higher specific capacity, capacity retention rate and cycle stability; the pole piece is smooth without curling or cracking.
[0346] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. Application of ionic polymer binders in positive electrode sheets of lithium-ion batteries; The ionic polymer binder has a chemical structure shown in Formula I or Formula II: In the formula I, R1, R3 and R4 are independently hydrogen or alkyl, and R2 and R5 are independently alkyl; In the formula II, R6 is hydrogen or alkyl, R7 is alkylene or aralkylene, R8 and R9 are independently alkyl or aralkyl, R 10 is an alkyl group; In the formula I, m=1-3, n=4-40, x+y+z=1, wherein x>0, y>0, z≥0; In the formula II, q is the degree of polymerization, and q is 20-2000.
2. The use according to claim 1, characterized in that: The method for preparing the positive electrode sheet of a lithium-ion battery comprises the following steps: ① mixing the ionic polymer binder and the second organic solvent to obtain a binder solution; ② Mixing the active material and the conductive agent to obtain a mixed powder; ③ Mixing the binder solution obtained in step ①, the mixed powder obtained in step ② and a third organic solvent to obtain a positive electrode slurry; ④ coating the positive electrode slurry obtained in step ③ on the current collector to obtain a positive electrode sheet for a lithium-ion battery; There is no order of precedence between step ① and step ②.