A preparation method and application of functionalized nano-silica microspheres

By grafting hyperbranched polymers on the surface of nanosilicon dioxide microspheres, the problem of insufficient dispersion and adsorption performance in aqueous media is solved, the adsorption capacity of metal ions and dyes is significantly improved, and its wastewater Application in processing.

CN118267967BActive Publication Date: 2024-11-19SHANDONG JINWEI NANO TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410655378.9
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-24
Publication Date
2024-11-19
Estimated Expiration
2044-05-24

AI Technical Summary

Technical Problem

Nanosilicon dioxide has poor dispersion in water and poor adsorption performance on metal ions and dye pollutants, which limits its application in wastewater treatment.

Method used

Vinyl nanosilicon dioxide microspheres were prepared by hydrothermal reaction using ethyl orthosilicate, KH570, cetyl trimethylammonium bromide and triethanolamine, and grafted thiol polymerized monomers and olefins on their surfaces. The base polymerization monomer forms a hyperbranched polymer, improving its dispersion and adsorption properties in aqueous media.

Benefits of technology

The adsorption performance of nano-silica on metal ions and dyes was significantly improved, especially the adsorption rates of Pb2+ and Cd2+ reached 93.5-99.3% and 92.1-99.0%, and the adsorption rates of methylene blue reached 82.4-92.2%, enhancing its Application prospects in wastewater treatment with metal and dyes.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
  • Figure SMS_5
    Figure SMS_5
Patent Text Reader

Abstract

The invention relates to the technical field of wastewater treatment, and discloses a preparation method of functionalized nano-silica microspheres and an application thereof. The invention uses tetraethyl orthosilicate as a silicon source, KH570 as a modifier, hexadecyltrimethylammonium bromide and the like as a surfactant, and triethanolamine as a pH regulator, and obtains vinyl nano-silica microspheres containing alkenyl groups on the surface through hydrothermal reaction, and then carries out a mercapto-ene click polymerization reaction with a mercapto polymerization monomer and the alkenyl polymerization monomer, so that a hyperbranched polymer containing a hydrophilic carboxyl group, an imino group and a thiocarbamate chelating group is grafted on the surface of the nano-silica, and Pb is treated. 2+ 、Cd 2+ It shows good adsorption effect on metal ions such as chlorinated bicarbonate and dyes such as methylene blue, which makes nano-silicon dioxide have broad application prospects in the treatment of wastewater containing metal ions and dyes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of wastewater treatment, in particular to a preparation method of functionalized nano silicon dioxide microspheres and application thereof. Background Art

[0002] The preparation method of nano silicon dioxide is simple, the specific surface area is large, it is non-toxic and pollution-free, and it is easy to modify the surface. Organic functional groups or grafted polymer molecular chains can be introduced on its surface, so that nano silicon dioxide can be used as a toughening agent, adsorbent material, etc., and has good practical applications in the fields of polymer materials, wastewater treatment, etc. As a new functional material, hyperbranched polymers have many branching points, molecular chains are not easy to entangle, and the main chain and the end contain a large number of functional groups. They have broad application prospects in the fields of metal nanoparticle stabilizers, adsorbents, and drug carriers. China CN115193421B discloses a preparation method of a wastewater treatment adsorbent, which uses mesoporous nano silicon dioxide, 3-aminopropyl triethoxysilane, 4-vinylbenzaldehyde, cysteine ​​aminobutyric acid monomer, triethanolamine, etc. as dosage, and grafts mercapto hyperbranched polyester to the surface of silicon dioxide, which has strong coordination chelation and adsorption properties for metal ions such as lead, copper, and cadmium. However, the preparation process of the wastewater treatment adsorbent is relatively complicated, and it has no adsorption effect on dye pollutants such as methylene blue, which is not conducive to the practical application of nano-silica in dye-containing and printing and dyeing wastewater. Summary of the invention

[0003] The invention solves the problems of poor dispersibility of silicon dioxide in water and poor adsorption performance for metal ions and dye pollutants.

[0004] The technical solution of the present invention is: a method for preparing functionalized nano-silica microspheres is:

[0005] (1) Add ethanol aqueous solution, surfactant and pH adjuster to the reaction bottle, stir evenly and heat to the reaction temperature, add ethyl orthosilicate and KH570 in a ratio of 1g:(0.1-0.4), stir and react, then pour the solution into a hydrothermal reactor to carry out hydrothermal reaction, cool and centrifuge, wash with water and ethanol in turn, and then dry to obtain vinyl nano-silica microspheres.

[0006] (2) Add N,N-dimethylacetamide, vinyl nano-silica microspheres in a ratio of 1g: (2.2-11): (3-15)g, thiol polymerization monomers, and olefin polymerization monomers into a reaction bottle, stir, add benzoin dimethyl ether, place the reaction bottle under ultraviolet light for reaction, centrifuge, wash with ethanol, and dry to obtain functionalized nano-silica microspheres.

[0007] Wherein, the surfactant is hexadecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide; and the pH regulator is triethanolamine.

[0008] The stirring reaction temperature in (1) is 55-65°C and the time is 3-5h; the hydrothermal reaction temperature is 110-120°C and the time is 36-48h.

[0009] Among them, the irradiation reaction time in (2) is 2-5h; the power of the ultraviolet lamp is 60-150W.

[0010] Among them, the preparation method of the thiol polymerization monomer is as follows: add ethanol, trimesaldehyde and cysteine ​​in a ratio of 1g: (2.3-2.5)g to a reaction bottle, stir to dissolve, then add 99% acetic acid solution by mass, heat to 75-80°C, condense and reflux to react for 6-18h, cool to room temperature, add sodium borohydride, react for 2-3h, remove the solvent by rotary evaporation, and separate by silica gel column chromatography to obtain the thiol polymerization monomer.

[0011] Among them, the preparation method of the thiol polymerization monomer is as follows: add tetrahydrofuran, trimethylolpropane tris(3-mercaptopropionate) and 2-isocyanatoethyl methacrylate in a ratio of 1g: (1.2-1.3)g to a reaction bottle, heat to 40-50°C, react for 6-10h, remove the solvent by rotary evaporation, wash with petroleum ether, and dry to obtain an olefin polymerization monomer.

[0012] Among them, functionalized nano-silica microspheres are used in the treatment of wastewater containing metal ions and dyes.

[0013] The technical effect of the present invention is as follows: the present invention uses tetraethyl orthosilicate as a silicon source, KH570 as a modifier, hexadecyltrimethylammonium bromide and the like as a surfactant, and triethanolamine as a pH regulator, and obtains vinyl nano-silica microspheres having alkenyl groups on the surface through a hydrothermal reaction.

[0014] The invention uses a novel thiol polymerization monomer containing carboxyl and imine groups and a novel olefin polymerization monomer containing thiocarbamate groups, and uses the olefin groups on the surface of vinyl nano-silicon dioxide microspheres as polymerization sites to cause a thiol-olefin click polymerization reaction, thereby grafting a hyperbranched polymer containing hydrophilic carboxyl, imino and thiocarbamate chelating groups on the surface of the nano-silicon dioxide. The hydrophilic carboxyl and imino groups improve the dispersibility of the nano-silicon dioxide in an aqueous medium, reduce the agglomeration of the nano-silicon dioxide, reduce the particle size, and are beneficial to improving the specific surface area and adsorption performance of the nano-silicon dioxide. At the same time, the surface-grafted hyperbranched polymer contains a three-dimensional branched network molecular chain, and the molecular chain is divergent, which can promote the contact between the active adsorption sites in the hyperbranched polymer and the metal ions, further improving the adsorption performance. In addition, the hyperbranched polymer contains a large number of chelating groups such as carboxyl, imino and thiocarbamate, which can bind to Pb 2+ 、Cd 2+ There is a strong coordination chelation between metal ions, which significantly improves the adsorption performance of nano-silicon dioxide for metal ions. 2+ The adsorption rate can reach up to 93.5-99.3% for Cd 2+ The highest adsorption rate reaches 92.1-99.0%, which makes nano-silicon dioxide have broad application prospects in the treatment of metal-containing wastewater.

[0015] The functionalized nano-silica microspheres of the present invention have an adsorption rate of 82.4-92.2% for methylene blue, because the polymer grafted on the surface of the nano-silica contains a large number of carboxyl groups, which can form an electrostatic interaction with methylene blue, thereby enhancing the adsorption performance between the nano-silica and methylene blue, which makes the nano-silica have a broad application prospect in the treatment of dye-containing wastewater. DETAILED DESCRIPTION

[0016] To better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments. It should be understood by those skilled in the art that the specific embodiments described herein are only used to explain the present invention and are not intended to limit the present invention.

[0017] Example 1

[0018] Add 40mL ethanol, 2g trimesaldehyde, and 4.6g cysteine ​​to the reaction flask, stir and dissolve, then drop 1.4mL 99% acetic acid solution, heat to 75°C, condense and reflux for 18h, cool to room temperature, add 90mmol sodium borohydride, react for 3h, remove the solvent by rotary evaporation, perform silica gel column chromatography, use ethyl acetate and petroleum ether solution as eluent, gradient elution, and obtain thiol polymerization monomer with a yield of 2.96g. The reaction formula is as follows:

[0019]

[0020] Example 2

[0021] Add 60 mL of ethanol, 2 g of trimesaldehyde, and 5 g of cysteine ​​to the reaction bottle, stir to dissolve, then add 1 mL of 99% acetic acid solution by mass, heat to 75 ° C, condense and reflux to react for 18 hours, cool to room temperature, add 110 mmol of sodium borohydride, react for 2 hours, remove the solvent by rotary evaporation, and separate by silica gel column chromatography. Use ethyl acetate and petroleum ether solution as eluents and gradient elution to obtain thiol polymerization monomer with a yield of 2.65.

[0022] Example 3

[0023] Add 100 mL of tetrahydrofuran, 5 g of trimethylolpropane tris(3-mercaptopropionate), and 6.5 g of 2-isocyanatoethyl methacrylate to the reaction bottle, heat to 40°C, react for 6 hours, remove the solvent by rotary evaporation, wash with petroleum ether, and dry to obtain an olefin polymerization monomer with a yield of 9.05 g. The reaction formula is as follows:

[0024]

[0025] Example 4

[0026] Add 80 mL of tetrahydrofuran, 5 g of trimethylolpropane tris(3-mercaptopropionate), and 6 g of 2-isocyanatoethyl methacrylate to the reaction bottle, heat to 50°C, react for 10 hours, remove the solvent by rotary evaporation, wash with petroleum ether, and dry to obtain olefin polymerization monomer with a yield of 9.24 g.

[0027] Example 5

[0028] (1) Add 20 mL of 15% ethanol aqueous solution, 0.042 g of surfactant hexadecyltrimethylammonium bromide, and 1.5 g of pH adjuster triethanolamine into a reaction bottle, stir evenly, and heat to 60°C. Add 2 g of tetraethyl orthosilicate and 0.2 g of KH570, stir and react for 5 h. Pour the solution into a hydrothermal reactor, heat to 110°C, and hydrothermally react for 48 h. After cooling, centrifuge, wash with water and ethanol in turn, and then dry to obtain vinyl nano-silica microspheres.

[0029] (2) Add 40 mL of N,N-dimethylacetamide, 1 g of vinyl nano-silica microspheres, 2.2 g of thiol polymerization monomer (prepared according to the method of Example 1), and 3 g of olefin polymerization monomer (prepared according to the method of Example 4) into a reaction bottle, stir, add 0.08 g of benzoin dimethyl ether, place the reaction bottle under a 100 W ultraviolet lamp for reaction for 2 h, centrifuge, wash with ethanol, and dry to obtain functionalized nano-silica microspheres.

[0030] Example 6

[0031] (1) Add 30 mL of 20% ethanol aqueous solution, 0.05 g of surfactant hexadecyltrimethylammonium chloride, and 1.8 g of pH adjuster triethanolamine to a reaction bottle, stir evenly, and heat to 55 °C. Add 2 g of tetraethyl orthosilicate and 0.4 g of KH570, stir and react for 3 h. Pour the solution into a hydrothermal reactor, heat to 115 °C, and hydrothermally react for 48 h. After cooling, centrifuge and wash with water and ethanol in turn, and then dry to obtain vinyl nano-silica microspheres.

[0032] (2) Add 60 mL of N,N-dimethylacetamide, 1 g of vinyl nano-silica microspheres, 5.4 g of thiol polymerization monomer (prepared according to the method of Example 1), and 7 g of olefin polymerization monomer (prepared according to the method of Example 4) into a reaction bottle, stir, add 0.17 g of benzoin dimethyl ether, place the reaction bottle under a 150 W ultraviolet lamp for reaction for 2 h, centrifuge, wash with ethanol, and dry to obtain functionalized nano-silica microspheres.

[0033] Example 7

[0034] (1) Add 25 mL of 20% ethanol aqueous solution, 0.05 g of surfactant hexadecyltrimethylammonium bromide, and 1.6 g of pH adjuster triethanolamine to a reaction bottle, stir evenly, and heat to 55 °C. Add 2 g of tetraethyl orthosilicate and 0.6 g of KH570, stir and react for 5 h. Pour the solution into a hydrothermal reactor, heat to 110 °C, and hydrothermally react for 48 h. After cooling, centrifuge, wash with water and ethanol in turn, and then dry to obtain vinyl nano-silica microspheres.

[0035] (2) Add 90 mL of N,N-dimethylacetamide, 1 g of vinyl nano-silica microspheres, 8.3 g of thiol polymerization monomer (prepared according to the method of Example 1), and 11.5 g of olefin polymerization monomer (prepared according to the method of Example 4) into a reaction bottle, stir, add 0.26 g of benzoin dimethyl ether, place the reaction bottle under a 60 W ultraviolet lamp for reaction for 5 h, centrifuge, wash with ethanol, and dry to obtain functionalized nano-silica microspheres.

[0036] Example 8

[0037] (1) Add 20 mL of 15% ethanol aqueous solution, 0.05 g of surfactant hexadecyltrimethylammonium chloride, and 2 g of pH adjuster triethanolamine to a reaction bottle, stir evenly, and heat to 65 °C. Add 2 g of tetraethyl orthosilicate and 0.8 g of KH570, stir and react for 3 h. Pour the solution into a hydrothermal reactor, heat to 120 °C, and hydrothermally react for 36 h. After cooling, centrifuge, wash with water and ethanol in turn, and then dry to obtain vinyl nano-silica microspheres.

[0038] (2) Add 120 mL of N,N-dimethylacetamide, 1 g of vinyl nano-silica microspheres, 11 g of thiol polymerization monomer (prepared according to the method of Example 1), and 15 g of olefin polymerization monomer (prepared according to the method of Example 4) into a reaction bottle, stir, add 0.35 g of benzoin dimethyl ether, place the reaction bottle under a 100 W ultraviolet lamp for reaction for 3 h, centrifuge, wash with ethanol, and dry to obtain functionalized nano-silica microspheres.

[0039] Comparative Example 1 is vinyl nano-silica microspheres, which are prepared according to the method of Example 5.

[0040] Comparative Example 2

[0041] The difference between this comparative example and Example 5 is that trimethylolpropane tris (3-mercaptopropionate) ( ) instead of mercapto polymerization monomers.

[0042] Add 40 mL of N,N-dimethylacetamide, 1 g of vinyl nano-silica microspheres, 2.2 g of trimethylolpropane tris(3-mercaptopropionate), and 3 g of olefin polymerization monomer into the reaction bottle, stir, add 0.08 g of benzoin dimethyl ether, place the reaction bottle under a 100 W ultraviolet lamp for reaction for 2 h, centrifuge, wash with ethanol, and dry to obtain functionalized nano-silica microspheres.

[0043] Comparative Example 3

[0044] The difference between this comparative example and Example 5 is that trimethylolpropane triacrylate ( ) instead of olefinic polymerization monomers.

[0045] To the reaction bottle, 40 mL of N,N-dimethylacetamide, 1 g of vinyl nano-silica microspheres, 2.2 g of thiol polymerization monomer, and 3 g of olefin polymerization monomer (prepared according to the method of Example 4) were added, and after stirring, 0.08 g of benzoin dimethyl ether was added. The reaction bottle was placed under a 100 W ultraviolet lamp for irradiation and reaction for 2 h, centrifuged, washed with ethanol, and dried to obtain functionalized nano-silica microspheres.

[0046] 200 mg of nano-silica microspheres were added to 100 mL of distilled water and ultrasonically dispersed for 10 min. The particle size of the particles in the nano-silica dispersion system was then tested using a nano-particle size analyzer and a zeta potential analyzer.

[0047] Table 1 Particle size test of silicon dioxide particles

[0048]

[0049] Add lead nitrate to 100 mL of distilled water to prepare Pb 2+ The mass concentration was 50 mg / L, and then 50-100 mg of nano-silica microspheres were added as adsorbents, ultrasonically shaken at 25 ° C for 10 min, and then adsorbed for 3 h. The Pb content in the solution after adsorption was determined by atomic absorption spectrometry. 2+ Calculate the adsorption rate.

[0050] Add cadmium chloride into 100 mL of distilled water to prepare Cd 2+ The mass concentration was 50 mg / L, then 80-160 mg of nano-silica microspheres were added, ultrasonically shaken at 25°C for 10 min, and then adsorbed for 3 h. The Cd content in the adsorbed solution was determined by atomic absorption spectrometry. 2+ Calculate the adsorption rate.

[0051] Adsorption rate Q = (C0-C) / C0×100%. C0 is the concentration of metal ions in the solution before adsorption; C is the concentration of metal ions in the solution after adsorption.

[0052] Table 2 Pb 2+ Adsorption rate test

[0053]

[0054] Table 3 Cd 2+ Adsorption rate test

[0055]

[0056] After testing, the functionalized nano-silica microspheres of Examples 5-8 had a significant effect on Pb 2+ The adsorption rate can reach up to 93.5-99.3% for Cd 2+ The adsorption rate can reach up to 92.1-99.0%. This is because the thiol polymer monomer containing carboxyl and imine groups is combined with the thiocarbamate group ( ) is an olefinic polymerization monomer, and the olefinic groups on the surface of the vinyl nano-silica microspheres are used as polymerization sites to undergo a thiol-olefin click polymerization reaction, thereby grafting a hyperbranched polymer containing hydrophilic carboxyl, imino and thiocarbamate chelating groups on the surface of the nano-silica. The hydrophilic carboxyl and imino groups improve the dispersibility of the nano-silica in the aqueous medium, reduce the agglomeration of the nano-silica, reduce the particle size, and are beneficial to improving the specific surface area and adsorption performance of the nano-silica. At the same time, the surface-grafted hyperbranched polymer contains a three-dimensional branched network molecular chain, and the molecular chain is divergent, which can promote the contact between the active adsorption sites in the hyperbranched polymer and the metal ions, further improving the adsorption performance. In addition, it contains a large number of chelating groups such as carboxyl, imino and thiocarbamate, which can bind to Pb 2+ 、Cd 2+ There is a strong coordination chelation effect between metal ions, which significantly improves the adsorption performance of nano-silica for metal ions.

[0057] Comparative Example 1 is vinyl nano-silica microspheres. The surface of nano-silica is not grafted with hyperbranched polymers, nor does it contain hydrophilic carboxyl groups or imino groups. It has poor dispersibility in water and few active adsorption sites. 2+ 、Cd 2 + The adsorption rate of metal ions is very low.

[0058] Comparative Example 2 uses trimethylolpropane tris(3-mercaptopropionate) to replace the mercapto polymerization monomer. The hyperbranched polymer grafted on the surface of the nano-silica microspheres does not contain hydrophilic carboxyl and imino chelating groups. The nano-silica microspheres have poor dispersibility in the aqueous medium and have fewer chemical adsorption sites, which is not conducive to the adsorption of Pb. 2+ 、Cd 2+ The adsorption rate of metal ions is poor.

[0059] Comparative Example 3 uses trimethylolpropane triacrylate instead of olefinic polymerization monomer. The hyperbranched polymer grafted on the surface of nano-silica microspheres does not contain thiocarbamate chelating groups, which is effective for Pb 2+ 、Cd 2+ The adsorption rate of metal ions is poor.

[0060] Add methylene blue to 100 mL of distilled water to a mass concentration of 100 mg / L, then add 50-200 mg of nano-silica microspheres, ultrasonically vibrate at 25°C for 10 minutes, and then adsorb for 3 hours. Determine the concentration of methylene blue in the solution after adsorption by atomic absorption spectrometry. Calculate the adsorption rate.

[0061] Adsorption rate Q = (C0-C) / C0×100%. C0 is the concentration of methylene blue in the solution before adsorption; C is the concentration of methylene blue in the solution after adsorption.

[0062] Table 4 Methylene blue adsorption rate test

[0063]

[0064] After testing, the adsorption rate of methylene blue by the functionalized nano-silica microspheres of Examples 5-8 reached 82.4-92.2%. This is because the polymer grafted on the surface of the nano-silica contains a large number of carboxyl groups, which can form electrostatic interactions with methylene blue, thereby enhancing the adsorption performance between the nano-silica and methylene blue.

[0065] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A method for preparing functionalized nano-silica microspheres, It is characterized in that The preparation method is: (1) Add ethanol aqueous solution, surfactant and pH adjuster to the reaction bottle, stir evenly and heat to the reaction temperature, add tetraethyl orthosilicate and KH570, stir and react, pour the solution into the hydrothermal reactor, carry out hydrothermal reaction, cool and centrifuge, wash with water and ethanol in turn, and then dry to obtain vinyl nano-silica microspheres; (2) Add N,N-dimethylacetamide, vinyl nano-silica microspheres, thiol polymerization monomers, and olefin polymerization monomers into a reaction bottle, stir, add benzoin dimethyl ether, place the reaction bottle under ultraviolet light for reaction, centrifuge, wash with ethanol, and dry to obtain functionalized nano-silica microspheres; The structural formula of the mercapto polymerizable monomer is ; The structural formula of the olefinic polymerizable monomer is .

2. The method for preparing functionalized nano-silica microspheres according to claim 1, It is characterized in that The surfactant is hexadecyltrimethylammonium chloride or hexadecyltrimethylammonium bromide; the pH regulator is triethanolamine.

3. The method for preparing functionalized nano-silica microspheres according to claim 1, It is characterized in that The ratio of the tetraethyl orthosilicate to KH570 is 1g: (0.1-0.4)g.

4. The method for preparing functionalized nano-silica microspheres according to claim 1, It is characterized in that The stirring reaction temperature in (1) is 55-65°C and the time is 3-5h; the hydrothermal reaction temperature is 110-120°C and the time is 36-48h.

5. The method for preparing functionalized nano-silica microspheres according to claim 1, It is characterized in that In the vinyl nano-silica microspheres of (2), the ratio of the mercapto polymerization monomer to the olefin polymerization monomer is 1 g: (2.2-11) g: (3-15) g.

6. The method for preparing functionalized nano-silica microspheres according to claim 1, It is characterized in that The irradiation reaction time in (2) is 2-5 hours; the power of the ultraviolet lamp is 60-150W.

7. The method for preparing functionalized nano-silica microspheres according to claim 5, It is characterized in that The preparation method of the thiol polymerization monomer is as follows: add ethanol, trimesaldehyde and cysteine ​​in a ratio of 1g: (2.3-2.5)g into a reaction bottle, add acetic acid solution dropwise after stirring to dissolve, heat to 75-80°C, condense and reflux to react for 6-18h, cool to room temperature, add sodium borohydride, react for 2-3h, remove the solvent by rotary evaporation, and separate by silica gel column chromatography to obtain the thiol polymerization monomer.

8. The method for preparing functionalized nano-silica microspheres according to claim 5, It is characterized in that The preparation method of the olefin polymerization monomer is as follows: tetrahydrofuran, trimethylolpropane tris(3-mercaptopropionate) and 2-isocyanatoethyl methacrylate in a ratio of 1 g: (1.2-1.3) g are added into a reaction bottle, the temperature is raised to 40-50° C., the reaction is performed for 6-10 hours, the solvent is removed by rotary evaporation, the mixture is washed with petroleum ether, and the mixture is dried to obtain the olefin polymerization monomer.

9. Use of the functionalized nano-silica microspheres obtained by the preparation method according to any one of claims 1 to 8 in the treatment of wastewater containing metal ions and wastewater containing dyes.