Electromagnetic shielding film with high folding resistance and preparation method thereof

By using a three-layer sandwich film in the electromagnetic shielding film, combining the heterogeneous interface of modified carbon fiber and liquid metal, the existing electromagnetic shielding film has been solved, and efficient electromagnetic shielding and bending are achieved. Performance, self-healing function.

CN118290795BActive Publication Date: 2024-11-12江西锦荣新材料有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410313800.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-19
Publication Date
2024-11-12
Estimated Expiration
2044-03-19

AI Technical Summary

Technical Problem

The existing electromagnetic shielding film has poor flexibility and is not resistant to folding, and cannot meet the application needs of scenarios such as cable information encryption and electromagnetic radiation protective clothing.

Method used

The scraping mold and scraping mechanism are used to prepare three-layer sandwich structure films, including two upper and lower layers of modified carbon fiber-polyurethane films and intermediate layer of liquid metal-polyurethane films. The electromagnetic wave reflection ability is enhanced through the heterostructure interface between carbon fiber and liquid metal, and Use the flexibility of polyurethane and the fluidity of liquid metal to form a conductive grid to improve shielding efficiency.

Benefits of technology

It obtains extremely high shielding efficiency and fold resistance, solves the problem of electromagnetic wave leakage on the side wall, and maintains good conductivity and electromagnetic shielding performance during bending, and has self-healing function.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004748348190000111
    Figure BDA0004748348190000111
Patent Text Reader

Abstract

The invention discloses an electromagnetic shielding film with high folding resistance, including a three-layer sandwich structure film of upper and lower two layers of modified carbon fiber-polyurethane film prepared by step-by-step scraping by a scraping mold and a scraping machine, and the middle layer is a liquid metal-polyurethane film. A heterogeneous structure interface is formed between the carbon fiber layer and the liquid metal layer, and the impedance mismatch characteristics of the interface enhance the material's reflection ability for electromagnetic waves. Through the design of the membrane layer structure, the surface square resistance of the obtained electromagnetic shielding film is significantly reduced, and the enhancement of conductivity and impedance mismatch significantly improves the shielding effectiveness. Carbon fiber is a conductive filler, and modified polyurethane is a matrix skeleton. Carbon fiber absorbs microwave energy and releases it in the form of heat energy. The heating of polyurethane causes re-entanglement between molecular chains, and the entire sandwich interlayer is driven to produce a self-healing effect, so that the electromagnetic shielding film takes into account the functions of high folding resistance and self-healing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of electromagnetic shielding, and relates to an electromagnetic shielding film with high folding resistance and a preparation method thereof. Background Art

[0002] Electromagnetic shielding film is a new type of electromagnetic shielding material that can block the penetration of electromagnetic waves, prevent electromagnetic radiation, protect electronic information from leakage and resist electromagnetic interference. It can effectively prevent electromagnetic waves from harming the human body, and shield electromagnetic radiation from interfering with electronic equipment to ensure the normal operation of the equipment. At the same time, by blocking the transmission of electromagnetic signals, it can also ensure that electronic information is not leaked or stolen.

[0003] The base materials of electromagnetic shielding materials that have been mass-produced are mainly copper, aluminum, nickel and various alloy materials, and the products are generally in the form of plates or wire mesh. Existing metal electromagnetic shielding materials can generally provide excellent electromagnetic shielding capabilities (>40dB) when the thickness is at the millimeter level, but due to the high density of traditional metal materials, the weight of the materials made from them is difficult to control at a low level; in addition, due to the strong rigidity of traditional metal materials, they cannot be processed into flexible electromagnetic shielding materials to meet the application of cable information encryption, electromagnetic radiation protective clothing and other scenarios. Therefore, it is necessary to improve the structure of the existing shielding film and design a new type of electromagnetic shielding film to meet the needs. Summary of the invention

[0004] The object of the present invention is to provide an electromagnetic shielding film with high folding resistance and a preparation method thereof, so as to solve the problems of poor flexibility and low folding resistance of the electromagnetic shielding film mentioned in the background technology.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] An electromagnetic shielding film with high folding resistance, comprising a three-layer sandwich structure film of upper and lower modified carbon fiber-polyurethane films prepared by step-by-step scraping by a scraping mold and a scraping machine, and a middle layer of liquid metal-polyurethane film;

[0007] The electromagnetic shielding film with high folding resistance is manufactured by the following steps:

[0008] Step A1, mixing the modified polyurethane particles with DMF solvent, heating to 50-55° C. and stirring for 10-15 hours to obtain solution a;

[0009] Step A2: mixing the modified carbon fiber with solution a to obtain solution b;

[0010] Step A3, mixing the liquid metal with solution a to obtain solution c;

[0011] Step A4, scrape solution b through a scraping mold and a scraper to obtain a modified carbon fiber-polyurethane film, scrape solution c on the modified carbon fiber-polyurethane film to obtain a liquid metal-polyurethane film in the middle layer, and then scrape solution b on the liquid metal-polyurethane film to obtain an upper and lower layer of modified carbon fiber-polyurethane film, and a three-layer sandwich structure film with a liquid metal-polyurethane film in the middle layer, which is an electromagnetic shielding film with high folding resistance.

[0012] Furthermore, the mass ratio of the modified polyurethane particles and the DMF solvent in step A1 is 1:4-4.5.

[0013] Furthermore, the mass ratio of the modified carbon fiber in step A2 to the modified polyurethane particles in solution a is 1.5-2:1.

[0014] Furthermore, the mass ratio of the liquid metal in step A3 to the modified polyurethane particles in solution a is 3-4:1.

[0015] The modified polyurethane particles are prepared by the following steps:

[0016] The polyurethane particles are washed with deionized water and anhydrous ethanol for 2-3 times, then dried at 62-65° C. for 2-3 hours, placed in a tris(hydroxymethyl)aminomethane aqueous solution containing dopamine for 20-25 hours, and then dried at 55-60° C. for 3-5 hours to obtain modified polyurethane particles.

[0017] Furthermore, the volume ratio of dopamine to tris(hydroxymethyl)aminomethane in the tris(hydroxymethyl)aminomethane aqueous solution containing dopamine is 1:5-6.

[0018] The modified carbon fiber is prepared by the following steps:

[0019] Step S1, immersing the carbon fiber in an acetone solution for 4-5 hours for degumming, then washing with distilled water, immersing the degummed carbon fiber in a solution mixed with concentrated HNO3 and concentrated H2SO4 in a ratio of 1:4, etching for 5-6 hours for coarsening, then neutralizing the obtained solution with a sodium hydroxide solution, centrifuging and washing in sequence, immersing the coarsened carbon fiber in a sensitizing solution prepared with 20g / lSnCl2·H2O and 3.5mlHCl for sensitization for 20-30min, centrifuging the obtained solution, then washing with distilled water 2-3 times, immersing the sensitized carbon fiber in a 100ml solution prepared with 0.5g silver nitrate and 1.5ml ammonia water for 30-40min, centrifuging the obtained solution, washing with anhydrous ethanol 2-3 times, and then placing it in a vacuum drying oven at 60°C for 3h to obtain the treated carbon fiber;

[0020] Step S2, put cobalt acetate, nickel acetate and polyvinyl pyrrolidone into a beaker, then add ethylene glycol, magnetically stir for 30-50 minutes, dissolve sodium hydroxide in the mixed solution, and magnetically stir until a uniform solution is obtained. After ultrasonicating the uniform solution at room temperature for 40-60 minutes, transfer it to a stainless steel reactor and add the treated carbon fiber, react at 175-185°C for 10-14 hours, then centrifuge the obtained reaction solution, wash it with anhydrous ethanol for 2-3 times, and place it in a vacuum drying oven for 4-5 hours to obtain modified carbon fiber.

[0021] Furthermore, in step S2, the usage ratio of carbon fiber, cobalt acetate, nickel acetate, polyvinyl pyrrolidone, ethylene glycol and sodium hydroxide is 40-50 mg: 0.2-0.28 g: 0.2-0.25 g: 0.3-0.4 g: 50-60 mL: 0.3-0.35 g.

[0022] Liquid metal is prepared by the following steps:

[0023] Step C1, put metal gallium, indium and tin into a graphite crucible, heat it to 500-600°C under argon protection and keep it for 5-6 hours, scrape off the scum on the surface and set it aside;

[0024] Step C2, adding the metal treated in step C1 into a beaker, adding anhydrous ethanol and 3-mercaptopropionic acid, and ultrasonically treating the mixture in an ice water bath for 1-1.5 hours, ultrasonically treating the suspension in an ultrasonic bath at 20-25° C. for 30-40 minutes, centrifuging the suspension, removing the supernatant, adding ethanol, removing excess 3-mercaptopropionic acid, and storing the product in ethanol for later use to obtain liquid metal.

[0025] Furthermore, the amount ratio of the treated metal, anhydrous ethanol and 3-mercaptopropionic acid in step C2 is 1.7-2 g: 40-50 mL: 5-6 mL.

[0026] The electromagnetic shielding film with high folding resistance is prepared by the following steps:

[0027] Step A1, mixing the modified polyurethane particles with DMF solvent, heating to 50-55° C. and stirring for 10-15 hours to obtain solution a;

[0028] Step A2: mixing the modified carbon fiber with solution a to obtain solution b;

[0029] Step A3, mixing the liquid metal with solution a to obtain solution c;

[0030] Step A4, scrape solution b through a scraping mold and a scraper to obtain a modified carbon fiber-polyurethane film, scrape solution c on the modified carbon fiber-polyurethane film to obtain a liquid metal-polyurethane film in the middle layer, and then scrape solution b on the liquid metal-polyurethane film to obtain an upper and lower layer of modified carbon fiber-polyurethane film, and a three-layer sandwich structure film with a liquid metal-polyurethane film in the middle layer, which is an electromagnetic shielding film with high folding resistance.

[0031] Beneficial effects of the present invention: The electromagnetic shielding film obtained by this technology has extremely high shielding effectiveness, and the product can withstand a certain number of bendings. The electromagnetic shielding film includes two layers of modified carbon fiber-polyurethane film, and the middle layer is a three-layer sandwich structure film of liquid metal-polyurethane film. A heterogeneous structure interface is formed between the carbon fiber layer and the liquid metal layer. The impedance mismatch characteristic of the interface enhances the material's ability to reflect electromagnetic waves. The carbon fiber film is combined with the metal film, and the membrane layer structure is designed to significantly reduce the surface square resistance of the obtained electromagnetic shielding film. The enhancement of conductivity and impedance mismatch significantly improves the shielding effectiveness.

[0032] In addition, during the film scraping process, the shielding film will be significantly stretched in the vertical direction, which will cause the conductivity of the side wall after stretching to decrease, which is easy to cause electromagnetic leakage, and defects are easy to occur at the corners, which will affect the electromagnetic shielding effect. The problem of electromagnetic wave leakage on the side wall can be solved by introducing liquid metal fillers to give the electromagnetic shielding material stretchable and fold-resistant electromagnetic shielding properties. Liquid metal is selected as the conductive filler, and modified polyurethane is used as the matrix skeleton. The liquid metal is ultrasonically treated before dispersion, and the film is formed by scraping. Due to the flexibility of the polyurethane itself and the fluidity of the liquid metal, a conductive grid will be formed in the middle layer under the stretching state, so that the film has good conductivity and electromagnetic shielding properties during the stretching process.

[0033] Carbon fiber is a conductive filler and modified polyurethane is a matrix skeleton. Carbon fiber absorbs microwave energy and releases it in the form of heat energy. The heating of polyurethane causes the molecular chains to re-entangle, and the entire sandwich interlayer will be driven to produce a self-healing effect, making the electromagnetic shielding film have both high folding resistance and self-healing functions.

[0034] Metal absorbers such as gallium, indium, and tin have small particle sizes and dispersed particles, and are easily affected by the adhesion effect in the high-frequency band, thereby reducing the absorption performance of the material. Surface treatment of this type of metal absorber can overcome this disadvantage and greatly enhance the shielding effect of the material. DETAILED DESCRIPTION

[0035] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0036] Example 1

[0037] The modified polyurethane particles are prepared by the following steps:

[0038] The polyurethane particles were washed twice with deionized water and anhydrous ethanol, then dried at 62°C for 2 hours, placed in a tris(hydroxymethylaminomethane) aqueous solution containing dopamine for 20 hours, and then dried at 55°C for 3 hours to obtain modified polyurethane particles, wherein the volume ratio of dopamine to tris(hydroxymethylaminomethane) in the tris(hydroxymethylaminomethane) aqueous solution containing dopamine was 1:5.

[0039] Example 2

[0040] The modified polyurethane particles are prepared by the following steps:

[0041] The polyurethane particles were washed twice with deionized water and anhydrous ethanol, then dried at 64°C for 2 hours, placed in a tris(hydroxymethylaminomethane) aqueous solution containing dopamine for 22 hours, and then dried at 58°C for 4 hours to obtain modified polyurethane particles, wherein the volume ratio of dopamine to tris(hydroxymethylaminomethane) in the tris(hydroxymethylaminomethane) aqueous solution containing dopamine was 1:5.5.

[0042] Example 3

[0043] The modified polyurethane particles are prepared by the following steps:

[0044] The polyurethane particles were washed three times with deionized water and anhydrous ethanol, then dried at 65°C for 3 hours, placed in a tris(hydroxymethylaminomethane) aqueous solution containing dopamine for 25 hours, and then dried at 60°C for 5 hours to obtain modified polyurethane particles, wherein the volume ratio of dopamine to tris(hydroxymethylaminomethane) in the tris(hydroxymethylaminomethane) aqueous solution containing dopamine was 1:6.

[0045] Example 4

[0046] The modified carbon fiber is prepared by the following steps:

[0047] Step S1, immersing the carbon fiber in an acetone solution for 4 hours for degumming, then washing with distilled water, immersing the degummed carbon fiber in a solution mixed with concentrated HNO3 and concentrated H2SO4 in a ratio of 1:4, etching for 5 hours for coarsening, then neutralizing the obtained solution with a sodium hydroxide solution, centrifuging and washing in sequence, immersing the coarsened carbon fiber in a sensitizing solution prepared with 20g / lSnCl2·H2O and 3.5mlHCl for sensitization for 20 minutes, centrifuging the obtained solution, then washing twice with distilled water, immersing the sensitized carbon fiber in a 100ml solution prepared with 0.5g silver nitrate and 1.5ml ammonia water for 30 minutes, centrifuging the obtained solution, washing twice with anhydrous ethanol, and then drying it in a vacuum drying oven at 60°C for 3 hours to obtain the treated carbon fiber;

[0048] Step S2, put 0.2g of cobalt acetate, 0.2g of nickel acetate and 0.3g of polyvinyl pyrrolidone into a beaker, add 50mL of ethylene glycol, stir magnetically for 30min, dissolve 0.3g of sodium hydroxide into the mixed solution, stir magnetically until a uniform solution is obtained, ultrasonicate the uniform solution at room temperature for 40min, transfer it to a stainless steel reactor and add 40mg of treated carbon fiber, react at 175°C for 10h, then centrifuge the obtained reaction solution, wash it twice with anhydrous ethanol, and dry it in a vacuum drying oven for 4h to obtain modified carbon fiber.

[0049] Example 5

[0050] The modified carbon fiber is prepared by the following steps:

[0051] Step S1, immersing the carbon fiber in an acetone solution for 4 hours for degumming, then washing with distilled water, immersing the degummed carbon fiber in a solution mixed with concentrated HNO3 and concentrated H2SO4 in a ratio of 1:4, etching for 5 hours for coarsening, then neutralizing the obtained solution with a sodium hydroxide solution, centrifuging and washing in sequence, immersing the coarsened carbon fiber in a sensitizing solution prepared with 20g / lSnCl2·H2O and 3.5mlHCl for sensitization for 25 minutes, centrifuging the obtained solution, then washing twice with distilled water, immersing the sensitized carbon fiber in a 100ml solution prepared with 0.5g silver nitrate and 1.5ml ammonia water for 35 minutes, centrifuging the obtained solution, washing twice with anhydrous ethanol, and then drying it in a vacuum drying oven at 60°C for 3 hours to obtain the treated carbon fiber;

[0052] Step S2, put 0.24g of cobalt acetate, 0.22g of nickel acetate and 0.35g of polyvinyl pyrrolidone into a beaker, add 55mL of ethylene glycol, stir magnetically for 40min, dissolve 0.32g of sodium hydroxide into the mixed solution, stir magnetically until a uniform solution is obtained, ultrasonicate the uniform solution at room temperature for 50min, transfer it to a stainless steel reactor and add 45mg of treated carbon fiber, react at 180°C for 12h, then centrifuge the obtained reaction solution, wash it twice with anhydrous ethanol, and dry it in a vacuum drying oven for 4h to obtain modified carbon fiber.

[0053] Example 6

[0054] The modified carbon fiber is prepared by the following steps:

[0055] Step S1, immersing the carbon fiber in an acetone solution for 5 hours to degumming, then washing with distilled water, immersing the degummed carbon fiber in a solution mixed with concentrated HNO3 and concentrated H2SO4 in a ratio of 1:4, etching reaction for 6 hours to roughen, then neutralizing the obtained solution with sodium hydroxide solution, centrifuging and washing in sequence, immersing the roughened carbon fiber in a sensitizing solution prepared with 20g / lSnCl2·H2O and 3.5mlHCl for sensitization for 30 minutes, centrifuging the obtained solution, then washing with distilled water 3 times, immersing the sensitized carbon fiber in a 100ml solution prepared with 0.5g silver nitrate and 1.5ml ammonia water for 40 minutes, centrifuging the obtained solution, washing with anhydrous ethanol 3 times, and then drying it in a vacuum drying oven at 60°C for 3 hours to obtain the treated carbon fiber;

[0056] Step S2, put 0.28g of cobalt acetate, 0.25g of nickel acetate and 0.4g of polyvinyl pyrrolidone into a beaker, add 60mL of ethylene glycol, stir magnetically for 50min, dissolve 0.35g of sodium hydroxide into the mixed solution, stir magnetically until a uniform solution is obtained, ultrasonicate the uniform solution at room temperature for 60min, transfer it to a stainless steel reactor and add 50mg of treated carbon fiber, react at 185°C for 14h, then centrifuge the obtained reaction solution, wash it with anhydrous ethanol 3 times, and dry it in a vacuum drying oven for 5h to obtain modified carbon fiber.

[0057] Example 7

[0058] Liquid metal is prepared by the following steps:

[0059] Step C1, placing metal gallium, indium and tin into a graphite crucible, heating to 500° C. and keeping the temperature for 5 hours under argon protection, scraping off the scum on the surface and setting aside;

[0060] Step C2, add 1.7 g of the metal treated in step C1 into a beaker, add 40 mL of anhydrous ethanol and 5 mL of 3-mercaptopropionic acid, and ultrasonically treat in an ice water bath for 1 hour. Ultrasonicate the suspension in an ultrasonic bath at 20° C. for 30 minutes, centrifuge the suspension, remove the supernatant, add ethanol, remove excess 3-mercaptopropionic acid, and store the product in ethanol for later use to obtain liquid metal.

[0061] Example 8

[0062] Liquid metal is prepared by the following steps:

[0063] Step C1, placing metal gallium, indium and tin into a graphite crucible, heating to 550° C. and keeping the temperature for 5 hours under argon protection, scraping off the scum on the surface, and setting aside;

[0064] Step C2, add 1.8 g of the metal treated in step C1 into a beaker, add 45 mL of anhydrous ethanol and 5.5 mL of 3-mercaptopropionic acid, and ultrasonically treat in an ice water bath for 1 hour. Ultrasonicate the suspension in an ultrasonic bath at 22° C. for 35 minutes, centrifuge the suspension, remove the supernatant, add ethanol, remove excess 3-mercaptopropionic acid, and store the product in ethanol for later use to obtain liquid metal.

[0065] Example 9

[0066] Liquid metal is prepared by the following steps:

[0067] Step C1, placing metal gallium, indium and tin into a graphite crucible, heating to 600° C. and keeping the temperature for 6 hours under argon protection, scraping off the scum on the surface and setting aside;

[0068] Step C2, add 2 g of the metal treated in step C1 into a beaker, add 50 mL of anhydrous ethanol and 6 mL of 3-mercaptopropionic acid, and ultrasonically treat in an ice water bath for 1.5 h. Ultrasonicate the suspension in an ultrasonic bath at 25° C. for 40 min. Centrifuge the suspension, remove the supernatant, add ethanol, remove excess 3-mercaptopropionic acid, and store the product in ethanol for later use to obtain liquid metal.

[0069] Example 10

[0070] An electromagnetic shielding film with high folding resistance, comprising a three-layer sandwich structure film of upper and lower modified carbon fiber-polyurethane films prepared by step-by-step scraping by a scraping mold and a scraping machine, and a middle layer of liquid metal-polyurethane film;

[0071] The electromagnetic shielding film with high folding resistance is manufactured by the following steps:

[0072] Step A1, mixing the modified polyurethane particles with DMF solvent, heating to 50° C. and stirring for 10 hours to obtain solution a, wherein the mass ratio of the modified polyurethane particles to the DMF solvent is 1:4;

[0073] Step A2: mixing the modified carbon fiber with solution a to obtain solution b, wherein the mass ratio of the modified carbon fiber to the modified polyurethane particles in solution a is 1.5:1;

[0074] Step A3, mixing the liquid metal with solution a to obtain solution c, wherein the mass ratio of the liquid metal to the modified polyurethane particles in solution a is 3:1;

[0075] Step A4, scrape solution b through a scraping mold and a scraper to obtain a modified carbon fiber-polyurethane film, scrape solution c on the modified carbon fiber-polyurethane film to obtain a liquid metal-polyurethane film in the middle layer, and then scrape solution b on the liquid metal-polyurethane film to obtain an upper and lower layer of modified carbon fiber-polyurethane film, and a three-layer sandwich structure film with a liquid metal-polyurethane film in the middle layer, which is an electromagnetic shielding film with high folding resistance.

[0076] Embodiment 11

[0077] An electromagnetic shielding film with high folding resistance, comprising a three-layer sandwich structure film of upper and lower modified carbon fiber-polyurethane films prepared by step-by-step scraping by a scraping mold and a scraping machine, and a middle layer of liquid metal-polyurethane film;

[0078] The electromagnetic shielding film with high folding resistance is manufactured by the following steps:

[0079] Step A1, mixing the modified polyurethane particles with DMF solvent, heating to 53° C. and stirring for 13 hours to obtain solution a, wherein the mass ratio of the modified polyurethane particles to the DMF solvent is 1:4.2;

[0080] Step A2: mixing the modified carbon fiber with solution a to obtain solution b, wherein the mass ratio of the modified carbon fiber to the modified polyurethane particles in solution a is 1.7:1;

[0081] Step A3, mixing the liquid metal with solution a to obtain solution c, wherein the mass ratio of the liquid metal to the modified polyurethane particles in solution a is 3.5:1;

[0082] Step A4, scrape solution b through a scraping mold and a scraper to obtain a modified carbon fiber-polyurethane film, scrape solution c on the modified carbon fiber-polyurethane film to obtain a liquid metal-polyurethane film in the middle layer, and then scrape solution b on the liquid metal-polyurethane film to obtain an upper and lower layer of modified carbon fiber-polyurethane film, and a three-layer sandwich structure film with a liquid metal-polyurethane film in the middle layer, which is an electromagnetic shielding film with high folding resistance.

[0083] Example 12

[0084] An electromagnetic shielding film with high folding resistance, comprising a three-layer sandwich structure film of upper and lower modified carbon fiber-polyurethane films prepared by step-by-step scraping by a scraping mold and a scraping machine, and a middle layer of liquid metal-polyurethane film;

[0085] The electromagnetic shielding film with high folding resistance is manufactured by the following steps:

[0086] Step A1, mixing the modified polyurethane particles with DMF solvent, heating to 55° C. and stirring for 15 hours to obtain solution a, wherein the mass ratio of the modified polyurethane particles to the DMF solvent is 1:4.5;

[0087] Step A2: mixing the modified carbon fiber with solution a to obtain solution b, wherein the mass ratio of the modified carbon fiber to the modified polyurethane particles in solution a is 2:1;

[0088] Step A3, mixing the liquid metal with solution a to obtain solution c, wherein the mass ratio of the liquid metal to the modified polyurethane particles in solution a is 4:1;

[0089] Step A4, scrape solution b through a scraping mold and a scraper to obtain a modified carbon fiber-polyurethane film, scrape solution c on the modified carbon fiber-polyurethane film to obtain a liquid metal-polyurethane film in the middle layer, and then scrape solution b on the liquid metal-polyurethane film to obtain an upper and lower layer of modified carbon fiber-polyurethane film, and a three-layer sandwich structure film with a liquid metal-polyurethane film in the middle layer, which is an electromagnetic shielding film with high folding resistance.

[0090] Comparative Example 1

[0091] Electromagnetic shielding film produced by Guangzhou Tongde Electronic Technology Co., Ltd.

[0092] Comparative Example 2

[0093] The preparation method of the electromagnetic shielding film of Comparative Example 2 refers to that of Example 10, except that in step A4, only solution b is scraped to obtain a modified carbon fiber-polyurethane film.

[0094] Comparative Example 3

[0095] The preparation method of the electromagnetic shielding film of Comparative Example 3 refers to that of Example 10, except that in step A4, only solution c is scraped to obtain a liquid metal-polyurethane film.

[0096] The electromagnetic shielding films obtained in Examples 10-12 and Comparative Examples 1-3 were subjected to the following performance tests: 1. Electromagnetic shielding effectiveness test method: the test was carried out in accordance with GB / T30142-2013 standard; 2. Bending performance: refer to standard IPC-TM-650. The shielding film samples were cut into test samples with a length of 15 cm and a width of 1 cm and pressed (180°C, 100 Kgf / cm 2, 2min) to the surface of the flexible circuit board. After the sample matures for 1 hour, it is placed on the MIT folding tester for testing. The shielding layer (ultra-thin copper foil) is not exposed as the standard to record the number of shielding film folding times; the test results are shown in Table 1:

[0097] Table 1

[0098]

[0099] It can be seen from Table 1 that, compared with Comparative Examples 1-3, the electromagnetic shielding films prepared in Examples 10-12 have better shielding effectiveness and bending performance.

[0100] In the description of the specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.

[0101] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. An electromagnetic shielding film having high folding resistance, characterized in that: The method comprises preparing a three-layer sandwich structure film with upper and lower layers of modified carbon fiber-polyurethane film and a middle layer of liquid metal-polyurethane film by step-by-step scraping through a scraping mold and a scraping machine; The electromagnetic shielding film is prepared by the following steps: Step A1, mixing the modified polyurethane particles with DMF solvent, heating to 50-55° C. and stirring for 10-15 hours to obtain solution a; Step A2, mixing the modified carbon fiber with solution a to obtain solution b; Step A3, mixing the liquid metal with solution a to obtain solution c; Step A4, scraping solution b through a scraping mold and a scraping machine to obtain a modified carbon fiber-polyurethane film, scraping solution c on the modified carbon fiber-polyurethane film to obtain a liquid metal-polyurethane film in the middle layer, and then scraping solution b on the liquid metal-polyurethane film to obtain a three-layer sandwich structure film with upper and lower layers being modified carbon fiber-polyurethane films and a middle layer being liquid metal-polyurethane film, that is, an electromagnetic shielding film with high folding resistance; The modified carbon fiber is prepared by the following steps: Step S1, immersing the carbon fiber in an acetone solution for 4-5 hours for degumming, then washing with distilled water, immersing the degummed carbon fiber in a solution of concentrated HNO3 and concentrated H2SO4 mixed in a volume ratio of 1:4, etching for 5-6 hours for coarsening, then neutralizing the obtained solution with a sodium hydroxide solution, centrifuging and washing in sequence, immersing the coarsened carbon fiber in a sensitizing solution prepared with 20g / LSnCl2·H2O and 3.5mLHCl for sensitization for 20-30min, centrifuging the obtained solution, then washing with distilled water 2-3 times, immersing the sensitized carbon fiber in a 100mL solution prepared with 0.5g silver nitrate and 1.5mL ammonia water for 30-40min, centrifuging the obtained solution, washing with anhydrous ethanol 2-3 times, and then placing it in a vacuum drying oven at 60°C for 3h to obtain the treated carbon fiber; Step S2, cobalt acetate, nickel acetate and polyvinyl pyrrolidone are placed in a beaker, ethylene glycol is added, and sodium hydroxide is dissolved in the mixed solution after magnetic stirring for 30-50 minutes, and magnetic stirring is performed until a uniform solution is obtained, and the uniform solution is ultrasonicated at room temperature for 40-60 minutes, and then transferred to a stainless steel reactor and the treated carbon fiber is added, and the reaction is carried out at 175-185° C. for 10-14 hours, and then the obtained reaction solution is centrifuged, washed with anhydrous ethanol for 2-3 times, and then placed in a vacuum drying oven for 4-5 hours to obtain a modified carbon fiber; Liquid metal is prepared by the following steps: Step C1, put metal gallium, indium and tin into a graphite crucible, heat it to 500-600°C under argon protection and keep it for 5-6 hours, scrape off the scum on the surface and set it aside; Step C2, adding the metal treated in step C1 to a beaker, adding anhydrous ethanol and 3-mercaptopropionic acid, ultrasonically treating in an ice water bath for 1-1.5h, ultrasonicating the suspension in an ultrasonic bath at 20-25°C for 30-40min, centrifuging the suspension, removing the supernatant, adding ethanol, removing excess 3-mercaptopropionic acid, and storing the product in ethanol for later use to obtain a liquid metal; The modified polyurethane particles are prepared by the following steps: The polyurethane particles are washed with deionized water and anhydrous ethanol for 2-3 times, then dried at 62-65° C. for 2-3 hours, placed in a tris(hydroxymethyl)aminomethane aqueous solution containing dopamine for 20-25 hours, and then dried at 55-60° C. for 3-5 hours to obtain modified polyurethane particles.

2. The electromagnetic shielding film with high folding resistance according to claim 1, characterized in that: The usage ratio of the carbon fiber, cobalt acetate, nickel acetate, polyvinyl pyrrolidone, ethylene glycol and sodium hydroxide in step S2 is 40-50 mg: 0.2-0.28 g: 0.2-0.25 g: 0.3-0.4 g: 50-60 mL: 0.3-0.35 g.

3. The method for preparing an electromagnetic shielding film with high folding resistance according to claim 1, characterized in that: The method comprises the following preparation steps: Step A1, mixing the modified polyurethane particles with DMF solvent, heating to 50-55° C. and stirring for 10-15 hours to obtain solution a; Step A2, mixing the modified carbon fiber with solution a to obtain solution b; Step A3, mixing the liquid metal with solution a to obtain solution c; Step A4, scrape solution b through a scraping mold and a scraper to obtain a modified carbon fiber-polyurethane film, scrape solution c on the modified carbon fiber-polyurethane film to obtain a liquid metal-polyurethane film in the middle layer, and then scrape solution b on the liquid metal-polyurethane film to obtain an upper and lower layer of modified carbon fiber-polyurethane film, and a three-layer sandwich structure film with a liquid metal-polyurethane film in the middle layer, which is an electromagnetic shielding film with high folding resistance.