Metal surface treatment agent and treatment process

By using raw materials such as γ-aminopropyltriethoxysilane and ultrasonic treatment technology, chemical conversion films are formed, combined with chelating agents and surfactants, the adhesion and durability of metal surfactants are solved, and high efficiency is achieved. Environmentally friendly metal surface protection improves the performance and service life of magnesium-aluminum alloy.

CN118291960BActive Publication Date: 2024-11-22FOSHAN RENCHANG TECH
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410403995.X
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-04-05
Publication Date
2024-11-22
Estimated Expiration
2044-04-05

AI Technical Summary

Technical Problem

Existing metal surface treatment agents have problems such as the use of toxic chemicals, insufficient performance trade-offs, poor adhesion and durability, high processing efficiency and cost, which limit their application in certain environments.

Method used

Using γ-aminopropyltriethoxysilane, complexing agent, fluorinated salt, fluorinated acid and other raw materials, chemical conversion film is formed by stirring and ultrasonic treatment, chelating agent, corrosion inhibitor and surfactant are added to optimize the formulation. To improve adhesion, corrosion resistance and stability.

Benefits of technology

It achieves high adhesion, corrosion resistance, wear resistance and stability, extends the service life of the metal surface, significantly improves the protection effect of magnesium-aluminum alloy, and reduces the treatment cost.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004776600540000101
    Figure BDA0004776600540000101
Patent Text Reader

Abstract

The present invention provides a metal surface treatment agent and a preparation process. The treatment agent of the present invention is mainly composed of γ-aminopropyl triethoxysilane, a complexing agent, a fluoride salt, a fluoride-containing acid, etc., and is obtained by a specific preparation process. Wherein, the complexing agent is potassium tartrate, the fluoride salt is potassium fluoride, and the fluoride-containing acid is fluorophosphoric acid. In particular, the chelating agent is composed of ethylenediaminetetraacetic acid, sodium tripolyphosphate and phytic acid in a specific mass ratio, and the corrosion inhibitor comprises molybdate, 2-mercaptobenzothiazole and polyaspartic acid. The chemical conversion film is mixed with sodium chromate, potassium phytate, silicon dioxide and carboxymethyl chitosan. Through a multi-step preparation process, including raw material mixing, the addition of a chemical conversion film precursor, the stirring of a chelating agent and a corrosion inhibitor, and ultrasonic treatment, a treatment agent is finally obtained. This scheme improves the hardness, wear resistance and corrosion resistance of the metal surface, and the preparation process is environmentally friendly and safe, and has good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal surface treatment, and in particular to a metal surface treatment agent and a treatment process. Background Art

[0002] Magnesium-aluminum alloys have been widely used in many fields such as aviation, automobiles, electronics, and military due to their unique properties, such as low density, high specific strength, good vibration damping, electromagnetic shielding, and good electrical and thermal conductivity. However, magnesium alloys are chemically highly active and easily react with oxygen and water in the environment, resulting in poor corrosion resistance. This characteristic limits the application of magnesium alloys in certain environments, especially in humid environments or environments containing corrosive gases.

[0003] In modern industry, metal surface treatment is a key technology that can improve the corrosion resistance, heat resistance, wear resistance and appearance of metals. The development and application of metal surface treatment agents are of great significance to improving the service life and reliability of metal materials. Metal surface treatment agent is a substance that coats the metal surface with a protective film. Its main function is to prevent corrosion on the metal surface, improve the wear resistance and impact resistance of the metal surface, and make the metal surface have a certain aesthetics. At present, the Chinese metal surface treatment agent market has developed maturely, but there are still some problems. The existing metal surface treatment agents have some defects and limitations, which limit their application in certain fields.

[0004] First, traditional metal surface treatment agents often rely on toxic or harmful chemicals, such as hexavalent chromium, which pose potential risks to the environment and human health. With increasingly stringent environmental regulations, the use of these treatment agents containing harmful substances has been restricted, and there is an urgent need to develop more environmentally friendly alternatives.

[0005] Secondly, some metal surface treatment agents may sacrifice other important properties, such as heat resistance and wear resistance, while providing protective properties. This limits the application of treatment agents in high temperature or high load environments. While improving corrosion resistance, the coating may affect other properties of magnesium alloys, such as electrical conductivity, thermal conductivity or mechanical properties, which requires a trade-off when designing the coating.

[0006] Finally, some metal surface treatment agents may lack sufficient adhesion, durability and corrosion resistance. Although some coatings can provide good initial protection, they may gradually fail in long-term use or extreme environments, causing the coating or conversion film to easily peel off or be damaged in actual use, thus affecting the protective effect of the metal and requiring regular maintenance or re-coating. In some surface treatment processes, such as cold spray aluminum metal coatings, micropores and microcracks may exist at the local particle interface. These defects may become the starting point of corrosion and affect the overall protective effect of the coating.

[0007] In addition, metal surface treatment agents in the prior art may be insufficient in terms of treatment efficiency and cost-effectiveness. Some treatment agents require complex multi-step processes, which not only increases production costs but also may lead to low treatment efficiency. Summary of the invention

[0008] In view of this, the present invention proposes a metal surface treatment agent and a treatment process to solve the above problems.

[0009] The technical solution of the present invention is achieved as follows: a metal surface treatment agent and treatment process: comprising the following raw materials in parts by weight: 42-88 parts of γ-aminopropyltriethoxysilane, 22-40 parts of complexing agent, 5-7 parts of fluoride salt, 12-22 parts of fluorine-containing acid, 5-8 parts of chemical conversion film, 2-4 parts of chelating agent, 1-3 parts of corrosion inhibitor, 2-4 parts of surfactant, and 20-40 parts of water; the chemical conversion film is chromate, phytate, silicon dioxide and carboxymethyl chitosan in a mass ratio of (8-12):(3-7):(2-5):(1-4).

[0010] Furthermore, a metal surface treatment agent and treatment process: including the following raw materials in parts by weight: 60 parts of γ-aminopropyltriethoxysilane, 30 parts of complexing agent, 6 parts of fluoride salt, 17 parts of fluorine-containing acid, 6 parts of chemical conversion film, 3 parts of chelating agent, 2 parts of corrosion inhibitor, 3 parts of surfactant, and 30 parts of water.

[0011] Furthermore, the complexing agent is any one or a combination of tartaric acid, sodium tartrate, potassium tartrate, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, potassium citrate and sodium citrate.

[0012] Furthermore, the fluoride salt is sodium fluoride or potassium fluoride.

[0013] Furthermore, the fluorine-containing acid is fluorozirconic acid, fluorotitanic acid or fluorophosphoric acid.

[0014] Furthermore, the chelating agent comprises ethylenediaminetetraacetic acid, sodium tripolyphosphate and phytic acid in a mass ratio of (6.5-9.7):(1.2-1.8):(0.3-0.8).

[0015] Furthermore, the corrosion inhibitor comprises molybdate, 2-mercaptobenzothiazole and polyaspartic acid in a mass ratio of (2-5):(1-3):(4-8).

[0016] Furthermore, the surfactant includes sulfonate, phosphate and carboxylate in a weight ratio of (6-10):(2-4):(1-3).

[0017] Furthermore, the chromate is any one or a combination of calcium chromate, magnesium chromate, potassium chromate, sodium chromate, copper chromate, and ammonium chromate, and the phytate is any one or a combination of calcium phytate, magnesium phytate, potassium phytate, sodium phytate, or iron phytate.

[0018] Furthermore, a preparation process of a metal surface treatment agent comprises the following steps:

[0019] S1, first add water to the reaction stirring container, then add γ-aminopropyltriethoxysilane, complexing agent, fluoride salt, and fluorine-containing acid to the above container in sequence, turn on the stirrer, maintain medium speed stirring for 20-40 minutes, so that the components are mixed evenly to obtain a mixed solution 1; the medium speed is a stirring rate of 60-120rpm;

[0020] S2, chromate, phytate, silicon dioxide and carboxymethyl chitosan are mixed evenly to form a chemical conversion film precursor, the chemical conversion film precursor is slowly added to the above mixture 1, and stirring is continued for 15-55 minutes to ensure that the components are fully mixed to obtain a mixed solution 2;

[0021] S3, the prepared chelating agent raw material is added to the mixed solution 2 in sequence, the stirring speed is increased to 250-350rpm, and stirring is continued for 10-20min until a uniform mixed solution is formed, and then the corrosion inhibitor and surfactant raw materials are added, and stirring is maintained at a constant speed to obtain a mixed solution 3;

[0022] S4. Adjust the pH value of the mixed solution 3 to 7-9, and perform ultrasonic treatment at a temperature of 25-28° C. for 30-40 min, with an ultrasonic frequency of 180-250 kHz and an ultrasonic power of 40-60 W, to obtain a metal surface treatment agent.

[0023] Compared with the prior art, the present invention has the following beneficial effects:

[0024] The invention selects specific raw materials and optimizes the proportions, uses gamma-aminopropyl triethoxysilane, a complexing agent, a fluoride salt, and a fluoride-containing acid as main components, and is helpful to enhance the adhesion and corrosion resistance of the metal surface. The selection and proportion of the complexing agent, the fluoride salt, the fluoride-containing acid and other raw materials can act synergistically to improve the treatment effect of the metal surface and increase the hardness and wear resistance of the surface. The chemical conversion film of the invention is selected and scientifically proportioned to better adhere to the metal surface, thereby improving the adhesion and uniformity of the coating. The addition of a chelating agent, a corrosion inhibitor and a surfactant can further improve the stability and treatment effect of the treatment agent, reduce corrosion and oxidation of the metal surface, and extend the service life of the metal.

[0025] Through the step-by-step preparation process, it is ensured that the various components can be fully mixed and reacted to form a uniform and stable metal surface treatment agent; the adjustment of the stirring rate helps to control the reaction process and ensure that the various components can fully contact and react; the application of ultrasonic treatment can further improve the dispersibility and permeability of the treatment agent, so that it can better adhere to the metal surface and improve the treatment effect.

[0026] The present invention has passed the test, and the ISO grade of the embodiment group is 0, the cutting edge of the coating is completely smooth without any peeling; the salt spray exposure corrosion area is less than 1.3%, the mass wear rate is less than 1.4%, the volume wear rate is less than 1.9%, the hardness reduction rate is within 2.2%, and the tensile strength reduction rate is within 3.2%. DETAILED DESCRIPTION

[0027] In order to better understand the technical content of the present invention, specific embodiments are provided below to further illustrate the present invention.

[0028] Unless otherwise specified, the experimental methods used in the embodiments of the present invention are all conventional methods.

[0029] Unless otherwise specified, the materials, reagents, etc. used in the embodiments of the present invention can be obtained from commercial sources.

[0030] Example 1

[0031] A metal surface treatment agent, comprising the following raw materials in parts by weight: 42 parts of γ-aminopropyltriethoxysilane, 22 parts of a complexing agent, 5 parts of a fluoride salt, 12 parts of a fluoride-containing acid, 5 parts of a chemical conversion film, 2 parts of a chelating agent, 1 part of a corrosion inhibitor, 2 parts of a surfactant, and 20 parts of water;

[0032] The complexing agent is tartaric acid; the fluoride salt is sodium fluoride; the fluoride-containing acid is fluorozirconic acid;

[0033] The chelating agent includes ethylenediaminetetraacetic acid, sodium tripolyphosphate and phytic acid in a mass ratio of 6.5:1.2:0.3;

[0034] The corrosion inhibitor comprises molybdate, 2-mercaptobenzothiazole and polyaspartic acid in a mass ratio of 2:1:4;

[0035] The chemical conversion film is composed of chromate, phytate, silicon dioxide and carboxymethyl chitosan in a mass ratio of 8:3:2:1;

[0036] The chromate is calcium chromate, and the phytate is calcium phytate.

[0037] Example 2

[0038] A metal surface treatment agent, comprising the following raw materials in parts by weight: 88 parts of γ-aminopropyltriethoxysilane, 40 parts of a complexing agent, 7 parts of a fluoride salt, 22 parts of a fluoride-containing acid, 8 parts of a chemical conversion film, 4 parts of a chelating agent, 3 parts of a corrosion inhibitor, 4 parts of a surfactant, and 40 parts of water;

[0039] The complexing agent is sodium tartrate;

[0040] The fluoride salt is potassium fluoride;

[0041] The fluorine-containing acid is fluorotitanic acid;

[0042] The chelating agent comprises ethylenediaminetetraacetic acid, sodium tripolyphosphate and phytic acid in a mass ratio of 9.7:1.8:0.8;

[0043] The corrosion inhibitor comprises molybdate, 2-mercaptobenzothiazole and polyaspartic acid in a mass ratio of 5:3:8.

[0044] The chemical conversion film is chromate, phytate, silicon dioxide and carboxymethyl chitosan in a mass ratio of 12:7:5:4;

[0045] The chromate is magnesium chromate, and the phytate is magnesium phytate.

[0046] Example 3

[0047] A metal surface treatment agent, comprising the following raw materials in parts by weight: 60 parts of γ-aminopropyltriethoxysilane, 30 parts of a complexing agent, 6 parts of a fluoride salt, 17 parts of a fluoride-containing acid, 6 parts of a chemical conversion film, 3 parts of a chelating agent, 2 parts of a corrosion inhibitor, 3 parts of a surfactant, and 30 parts of water;

[0048] The complexing agent is potassium tartrate;

[0049] The fluoride salt is potassium fluoride;

[0050] The fluorine-containing acid is fluorophosphoric acid;

[0051] The chelating agent comprises ethylenediaminetetraacetic acid, sodium tripolyphosphate and phytic acid in a mass ratio of 7.5:1.5:0.5;

[0052] The corrosion inhibitor comprises molybdate, 2-mercaptobenzothiazole and polyaspartic acid in a mass ratio of 3:2:6.

[0053] The chemical conversion film is chromate, phytate, silicon dioxide and carboxymethyl chitosan in a mass ratio of 10:5:3:3;

[0054] The chromate is sodium chromate, and the phytate is potassium phytate;

[0055] The above examples 1-3 are prepared according to the following method:

[0056] S1, first add water to the reaction stirring container, then add γ-aminopropyltriethoxysilane, complexing agent, fluoride salt, and fluorine-containing acid to the above container in sequence, turn on the stirrer, and keep stirring at a medium speed for 30 minutes to mix the components evenly to obtain a mixed solution 1; the medium speed is a stirring rate of 90 rpm;

[0057] S2, chromate, phytate, silicon dioxide and carboxymethyl chitosan are mixed evenly to form a chemical conversion film precursor, the chemical conversion film precursor is slowly added to the above mixture 1, and stirring is continued for 35 minutes to ensure that the components are fully mixed to obtain a mixed solution 2;

[0058] S3, the prepared chelating agent raw material is added to the mixed solution 2 in sequence, the stirring speed is increased to 300 rpm, and stirring is continued for 15 min until a uniform mixed solution is formed, and then the corrosion inhibitor and surfactant raw materials are added, and stirring is maintained at a constant speed to obtain a mixed solution 3;

[0059] S4. Adjust the pH of the mixed solution 3 to 8, and perform ultrasonic treatment at 27° C. for 35 min with an ultrasonic frequency of 220 kHz and an ultrasonic power of 50 W to obtain a metal surface treatment agent.

[0060] Example 4

[0061] A metal surface treatment agent, comprising the following raw materials in parts by weight: 60 parts of γ-aminopropyltriethoxysilane, 30 parts of a complexing agent, 6 parts of a fluoride salt, 17 parts of a fluoride-containing acid, 6 parts of a chemical conversion film, 3 parts of a chelating agent, 2 parts of a corrosion inhibitor, 3 parts of a surfactant, and 30 parts of water;

[0062] The complexing agent is potassium tartrate;

[0063] The fluoride salt is potassium fluoride;

[0064] The fluorine-containing acid is fluorophosphoric acid;

[0065] The chelating agent comprises ethylenediaminetetraacetic acid, sodium tripolyphosphate and phytic acid in a mass ratio of 7.5:1.5:0.5;

[0066] The corrosion inhibitor comprises molybdate, 2-mercaptobenzothiazole and polyaspartic acid in a mass ratio of 3:2:6.

[0067] The chemical conversion film is chromate, phytate, silicon dioxide and carboxymethyl chitosan in a mass ratio of 10:5:3:3;

[0068] The chromate is sodium chromate, and the phytate is potassium phytate;

[0069] The above-mentioned Example 4 is prepared according to the following method:

[0070] S1, first add water to the reaction stirring container, then add γ-aminopropyltriethoxysilane, complexing agent, fluoride salt, and fluorine-containing acid to the above container in sequence, turn on the stirrer, keep stirring at medium speed for 20 minutes to mix the components evenly, and obtain a mixed solution 1; the medium speed is a stirring rate of 60 rpm;

[0071] S2, chromate, phytate, silicon dioxide and carboxymethyl chitosan are mixed evenly to form a chemical conversion film precursor, the chemical conversion film precursor is slowly added to the above mixture 1, and stirring is continued for 15 minutes to ensure that the components are fully mixed to obtain a mixed solution 2;

[0072] S3, the prepared chelating agent raw material is added to the mixed solution 2 in sequence, the stirring speed is increased to 250rpm, and stirring is continued for 10min until a uniform mixed solution is formed, and then the corrosion inhibitor and surfactant raw materials are added, and stirring is maintained at a constant speed to obtain a mixed solution 3;

[0073] S4. Adjust the pH of the mixed solution 3 to 7, and perform ultrasonic treatment at 25° C. for 30 min. The ultrasonic frequency is 180 kHz and the ultrasonic power is 40 W to obtain a metal surface treatment agent.

[0074] Example 5

[0075] A metal surface treatment agent, comprising the following raw materials in parts by weight: 60 parts of γ-aminopropyltriethoxysilane, 30 parts of a complexing agent, 6 parts of a fluoride salt, 17 parts of a fluoride-containing acid, 6 parts of a chemical conversion film, 3 parts of a chelating agent, 2 parts of a corrosion inhibitor, 3 parts of a surfactant, and 30 parts of water;

[0076] The complexing agent is potassium tartrate;

[0077] The fluoride salt is potassium fluoride;

[0078] The fluorine-containing acid is fluorophosphoric acid;

[0079] The chelating agent comprises ethylenediaminetetraacetic acid, sodium tripolyphosphate and phytic acid in a mass ratio of 7.5:1.5:0.5;

[0080] The corrosion inhibitor comprises molybdate, 2-mercaptobenzothiazole and polyaspartic acid in a mass ratio of 3:2:6.

[0081] The chemical conversion film is chromate, phytate, silicon dioxide and carboxymethyl chitosan in a mass ratio of 10:5:3:3;

[0082] The chromate is sodium chromate, and the phytate is potassium phytate;

[0083] The above-mentioned Example 5 is prepared according to the following method:

[0084] S1, first add water to the reaction stirring container, then add γ-aminopropyltriethoxysilane, complexing agent, fluoride salt, and fluorine-containing acid to the above container in sequence, turn on the stirrer, and keep stirring at a medium speed for 40 minutes to mix the components evenly to obtain a mixed solution 1; the medium speed is a stirring rate of 120 rpm;

[0085] S2, chromate, phytate, silicon dioxide and carboxymethyl chitosan are mixed evenly to form a chemical conversion film precursor, the chemical conversion film precursor is slowly added to the above mixture 1, and stirring is continued for 55 minutes to ensure that the components are fully mixed to obtain a mixed solution 2;

[0086] S3, the prepared chelating agent raw material is added to the mixed solution 2 in sequence, the stirring speed is increased to 350 rpm, and stirring is continued for 20 min until a uniform mixed solution is formed, and then the corrosion inhibitor and surfactant raw materials are added, and stirring is maintained at a constant speed to obtain a mixed solution 3;

[0087] S4. Adjust the pH value of the mixed solution 3 to 9, and perform ultrasonic treatment at 28° C. for 40 min. The ultrasonic frequency is 250 kHz and the ultrasonic power is 60 W to obtain a metal surface treatment agent.

[0088] Comparative Example 1

[0089] The difference between this comparative example and Example 3 is that the metal surface treatment agent includes the following raw materials in parts by weight: 30 parts of γ-aminopropyltriethoxysilane, 50 parts of complexing agent, 11 parts of fluoride salt, 28 parts of fluorine-containing acid, 10 parts of chemical conversion film, 1 part of chelating agent, 5 parts of corrosion inhibitor, 1 part of surfactant, and 50 parts of water.

[0090] Comparative Example 2

[0091] The difference between this comparative example and Example 3 is that the metal surface treatment agent is not added into the chemical conversion film.

[0092] Comparative Example 3

[0093] The difference between this comparative example and Example 3 is that no chelating agent is added to the metal surface treatment agent.

[0094] Comparative Example 4

[0095] The difference between this comparative example and Example 3 is that no complexing agent is added to the metal surface treatment agent.

[0096] Comparative Example 5

[0097] The difference between this comparative example and Example 3 is that the chemical conversion film is chromate, phytate, silicon dioxide and carboxymethyl chitosan in a mass ratio of 1:1:1:1.

[0098] 1. Effect Verification

[0099] The surface treatment agents of the above-mentioned embodiments 1-5 and comparative examples 1-5 are used to perform surface treatment on the magnesium-aluminum alloy respectively, and the specific steps are as follows:

[0100] (1) Metal surface preparation: Select the magnesium and aluminum metal samples to be processed, ensure that the surface is free of oil, impurities and rust, and use sandpaper or a polishing machine to preliminarily treat the metal surface to remove surface unevenness and oxide layer;

[0101] (2) Cleaning the metal surface: Use a cleaning agent (such as a petroleum-based cleaning agent, a chlorinated hydrocarbon-based cleaning agent, or an alkaline cleaning agent) to thoroughly clean the metal surface to remove oil and other contaminants, and rinse with clean water to ensure that no cleaning agent remains;

[0102] (3) Applying the metal surface treatment agent: Use a brush, roller or spraying equipment to evenly apply the metal surface treatment agent of the present invention on the metal surface. Depending on the requirements of the treatment agent, multiple layers may need to be applied, and each layer needs to wait for the previous layer to completely dry;

[0103] (4) Curing the metal surface treatment agent: drying the applied surface treatment agent at 50°C;

[0104] (5) Inspection and testing: Inspect the treated metal surface to ensure that it is free of defects, bubbles and good uniformity. Perform adhesion test, corrosion resistance, wear resistance, heat resistance test and hardness test to verify the treatment effect.

[0105] (6) Test standards:

[0106] a. Adhesion: Adhesion is usually assessed by a cross-cut test (such as GB / T9286-1998), in which the coating is cut into a grid pattern and then peeled off with tape to observe the shedding of the coating.

[0107] Result evaluation: Evaluated according to ISO grade standards

[0108] Level 0: The cutting edge of the coating is completely smooth without any peeling;

[0109] Level 1: There is a small flake peeling at the intersection of the cut, but the actual damage in the cross-cut area does not exceed 5%;

[0110] Level 2: There is flaking at the edge and / or intersection of the cut, and the flaking area is greater than 5% but less than 15%;

[0111] Level 3: There is partial or complete peeling along the edge of the cut, and some or all of the intersections peel off, with the peeling area ranging from 15% to 35%;

[0112] Level 4: Large pieces of the cut edge peel off, and / or some intersections peel off completely, with the peeling area exceeding 35% but not more than 65%;

[0113] Level 5: Exceeding all the above levels, i.e. peeling occurs on the edges and most intersections of the cut.

[0114] b. Corrosion resistance: Evaluate the corrosion area by salt spray test (such as GB / T10125-2012) for 24 hours of salt spray exposure;

[0115] c. Wear resistance: Use Taber wear resistance tester for testing, select CS-10 grinding wheel, set the speed to 100 rpm, load pressure to 500g, wear track to circular, temperature to 23±1℃, humidity to 65±5%; calculate the wear rate by comparing the mass loss or thickness reduction of the coating before and after the test;

[0116] The calculation formula of mass loss wear rate is:

[0117] M = (m1-m0) / m0×100%;

[0118] Where m0 is the mass of the sample before the test (g), and m1 is the mass of the sample after the test (g);

[0119] Volume loss wear rate calculation formula:

[0120] V = (v1-v0) / v0×100%;

[0121] Where v0 is the mass of the sample before testing (mm 3 ), v1 is the mass of the sample after the test (mm 3 );

[0122] d. Heat resistance: According to standard ASTM D6944-15 (2020), 500 thermal cycle tests were carried out at temperatures of 100°C and 400°C. The hardness and tensile strength were tested at the same time, and the change values ​​were calculated.

[0123] Hardness change rate = (hardness value before aging - hardness value after aging) / hardness value before aging × 100%;

[0124] Tensile strength change rate = (new tensile strength - original tensile strength) / original tensile strength × 100%.

[0125] (7) Test results:

[0126]

[0127] The above results show that after treating the surface of the magnesium-aluminum alloy, the metal treatment agent of the present invention forms a stable and dense composite protective coating with excellent adhesion, corrosion resistance, wear resistance and better mechanical properties.

[0128] By comparing the example group with comparative example 1, the optimization of the raw material ratio enables the metal surface treatment agent prepared by the present invention to perform well in terms of hardness, wear resistance, corrosion resistance, etc. At the same time, the treatment agent has good stability and long-term effectiveness, and can maintain the excellent performance of the metal surface for a long time.

[0129] Compared with Comparative Examples 2 and 5, the addition of a chemical conversion film made of chromate, phytate, silicon dioxide and carboxymethyl chitosan in a specific ratio can significantly improve the performance of the metal surface, wherein chromate, as the main component, can significantly improve the corrosion resistance of the metal surface and effectively resist the erosion of environmental factors such as moisture and salt. Phytate can further enhance the protective performance of the surface and make it more durable; the addition of silicon dioxide can increase the hardness and wear resistance of the conversion film, making the metal surface harder, resisting scratches and wear, and extending the service life of metal parts; carboxymethyl chitosan has good film-forming properties and adhesion, which helps the chemical conversion film to better adhere to the metal surface and improve the adhesion and uniformity of the coating. At the same time, it can also provide a good base layer for the subsequent coating process and enhance the overall performance of the coating.

[0130] Compared with Comparative Example 3, the addition of a specific ratio of chelating agent can significantly improve the performance of the metal surface, enhance stability, improve the microstructure of the metal surface, make it more uniform and smooth, help improve coating adhesion and uniformity, can react with the ions on the metal surface, form a stable protective film, enhance the corrosion resistance and oxidation resistance of the metal surface, and have the advantages of environmental protection and safety. EDTA can form a stable chelate with metal ions, effectively preventing the adverse reaction of metal ions during surface treatment. At the same time, sodium tripolyphosphate and phytic acid can also form chelation with metal ions, further enhancing the chelating effect. This synergistic effect enables the chelating agent to efficiently remove or stabilize the impurity ions on the metal surface, improve the purity and treatment effect of the metal surface.

[0131] Compared with Comparative Example 4, the addition of the complexing agent of the present invention can form a stable complex with the metal ions, which helps to remove impurities and oxides on the metal surface, thereby obtaining a cleaner and more uniform surface, improving the adhesion between the coating and the metal substrate, and ensuring the durability and stability of the coating.

[0132] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.

Claims

1. A metal surface treatment agent, characterized in that: The invention comprises the following raw materials in parts by weight: 42-88 parts of γ-aminopropyltriethoxysilane, 22-40 parts of complexing agent, 5-7 parts of fluoride salt, 12-22 parts of fluoride-containing acid, 5-8 parts of chemical conversion film precursor, 2-4 parts of chelating agent, 1-3 parts of corrosion inhibitor, 2-4 parts of surfactant and 20-40 parts of water; the chemical conversion film precursor comprises chromate, phytate, silicon dioxide and carboxymethyl chitosan in a mass ratio of (8-12):(3-7):(2-5):(1-4); the chelating agent comprises ethylenediaminetetraacetic acid, sodium tripolyphosphate and phytic acid in a mass ratio of (6.5-9.7):(1.2-1.8):(0.3-0.8); the corrosion inhibitor comprises molybdate, 2-mercaptobenzothiazole and polyaspartic acid in a mass ratio of (2-5):(1-3):(4-8).

2. A metal surface treatment agent as claimed in claim 1, characterized in that: The invention comprises the following raw materials in parts by weight: 60 parts of gamma-aminopropyltriethoxysilane, 30 parts of complexing agent, 6 parts of fluoride salt, 17 parts of fluorine-containing acid, 6 parts of chemical conversion film precursor, 3 parts of chelating agent, 2 parts of corrosion inhibitor, 3 parts of surfactant and 30 parts of water.

3. A metal surface treatment agent as claimed in claim 1, characterized in that: The complexing agent is any one or a combination of tartaric acid, sodium tartrate, potassium tartrate, ethylenediaminetetraacetic acid, disodium ethylenediaminetetraacetate, potassium citrate and sodium citrate.

4. A metal surface treatment agent as claimed in claim 1, characterized in that: The fluoride salt is sodium fluoride or potassium fluoride.

5. A metal surface treatment agent as claimed in claim 1, characterized in that: The fluorine-containing acid is fluorozirconic acid, fluorotitanic acid or fluorophosphoric acid.

6. A metal surface treatment agent as claimed in claim 1, characterized in that: The surfactant includes sulfonate, phosphate and carboxylate in a weight ratio of (6-10):(2-4):(1-3).

7. A metal surface treatment agent as claimed in claim 1, characterized in that: The chromate is any one or a combination of calcium chromate, magnesium chromate, potassium chromate, sodium chromate, copper chromate, and ammonium chromate; and the phytate is any one or a combination of calcium phytate, magnesium phytate, potassium phytate, sodium phytate, or iron phytate.

8. The process for preparing a metal surface treatment agent according to claim 1, characterized in that: The following steps are involved: S1, first add water to the reaction stirring container, then add γ-aminopropyltriethoxysilane, complexing agent, fluoride salt, and fluorine-containing acid to the above container in sequence, turn on the stirrer, maintain medium speed stirring for 20-40 minutes, so that the components are mixed evenly to obtain a mixed solution 1; the medium speed is a stirring rate of 60-120rpm; S2, chromate, phytate, silicon dioxide and carboxymethyl chitosan are mixed evenly to form a chemical conversion film precursor, the chemical conversion film precursor is slowly added to the above mixed solution 1, and stirring is continued for 15-55 minutes to ensure that the components are fully mixed to obtain a mixed solution 2; S3, the prepared chelating agent raw material is added to the mixed solution 2 in sequence, the stirring speed is increased to 250-350rpm, and stirring is continued for 10-20min until a uniform mixed solution is formed, and then the corrosion inhibitor and surfactant raw materials are added, and stirring is maintained at a constant speed to obtain a mixed solution 3; S4. Adjust the pH value of the mixed solution 3 to 7-9, and perform ultrasonic treatment at a temperature of 25-28° C. for 30-40 min, with an ultrasonic frequency of 180-250 kHz and an ultrasonic power of 40-60 W, to obtain a metal surface treatment agent.

Citation Information

Patent Citations

  • Environment-friendly metal surface treating agent and preparation method thereof

    CN105734547A

  • Metal surface pretreatment agent and preparation method and application thereof

    CN106906462A

  • Passivation skin film agent special for aluminum product and preparation method of passivation skin film agent

    CN107829081A

  • Anti-corrosive coating compositions and methods for metal materials

    EP1002889A2

  • Surface-treated steel sheet excellent in chromium-elution resistance and corrosion resistance