A method for preparing carbon-based adsorption catalytic material
By optimizing the preparation method of carbon-based adsorption catalytic materials and employing drying, carbonization, oxidation modification, and cooling treatment, the problems of long production cycle and high energy consumption of existing activated carbon materials have been solved, achieving high efficiency and stability in flue gas purification and reducing costs.
Patent Information
- Application Number
- CN202410464736.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-04-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-04-17
AI Technical Summary
Existing activated carbon materials for flue gas purification have long production cycles, high energy consumption, and poor purification performance, making it difficult to meet higher flue gas purification requirements and resulting in high operating costs for activated carbon-based flue gas purification technology.
By optimizing the preparation method of carbon-based adsorption catalytic materials, coal powder, active components and binders are mixed and shaped, and then dried, carbonized, oxidized and cooled. Combined with specific gas modification treatment, the process parameters are optimized to improve the porosity and oxygen-containing functional groups of the material, and reduce or replace the activation process.
A carbon-based adsorbent material with short production cycle, low energy consumption, excellent desulfurization and denitrification performance, and high cycle stability has been developed, which reduces production costs and improves purification efficiency, meeting higher flue gas purification requirements.
Smart Images

Figure CN118320808B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a carbon-based material for flue gas purification, and in particular to a method for preparing a carbon-based adsorption catalytic material, belonging to the technical field of carbon-based materials for flue gas purification. Background Art
[0002] With the increasing requirements of environmental protection in my country, more and more types of air pollutants are being controlled, and emission standards are becoming increasingly stringent, and the demand for multi-pollutant treatment of industrial flue gas is becoming more urgent. Activated carbon flue gas purification technology with carbon-based materials as the core has been rapidly applied and promoted due to its advantages of high pollutant removal efficiency, no secondary pollution, simple operation, low operating cost, and resource-based by-products.
[0003] The production process of activated carbon materials for flue gas purification generally requires grinding, kneading, granulation, carbonization, cooling, activation, cooling, packaging and other processes. Carbonization and activation are the heat treatment processes for activated carbon production, and they are also the two core processes for activated carbon production. The technical level and production stability of the processes directly determine the quality of the activated carbon finished product. In the existing process, in order to ensure the purification performance of activated carbon on flue gas, the activation time of activated carbon is relatively long (generally 5 hours or more), and the temperature required for the activation process is high, resulting in high energy consumption and low production efficiency. Furthermore, with the rapid promotion of activated carbon flue gas purification technology, the market demand for flue gas purification activated carbon material products has grown rapidly, and the requirements for performance indicators have also been continuously improved. At present, the quality of flue gas purification activated carbon material products still has the problems of low desulfurization and denitrification performance and poor stability, which makes it difficult to adapt to higher flue gas purification requirements, and also directly leads to the high operating cost of activated carbon flue gas purification technology; the above problems will affect the quality assurance of activated carbon materials, which will in turn restrict the further development of activated carbon flue gas purification technology. Summary of the invention
[0004] In view of the problems in the prior art that the existing activated carbon materials for flue gas purification have a long production cycle, high energy consumption and poor purification performance, the present invention provides a method for preparing a carbon-based adsorption catalytic material. Through process optimization, a mixture consisting of coal powder, active components, a binder and water is formed into granules and then dried, carbonized, oxidized, cooled and other treatments are performed in sequence to obtain a carbon-based adsorption material for flue gas purification with rich and uniform pores, high and stable strength, and rich oxygen-containing functional groups on the surface of the material. The carbon-based adsorption material has the advantages of short production cycle, low energy consumption, excellent desulfurization and denitrification performance, and high cycle stability. Furthermore, by optionally performing or not performing activation treatment, the purification performance of the carbon-based material can be further guaranteed and improved.
[0005] In order to achieve the above technical objectives, the technical solutions adopted by the present invention are specifically described as follows:
[0006] A method for preparing a carbon-based adsorption catalytic material, the method comprising:
[0007] 1) Coal powder, active components, binder and water are mixed to obtain a mixture, and then the mixture is extruded to obtain pellets.
[0008] 2) The pellets are sequentially dried, carbonized, oxidized and cooled to obtain a carbon-based adsorption catalytic material.
[0009] Among them, oxidation modification is to use water-containing air, water vapor, protective gas and oxygen as the modified mixed gas to modify the granular material. When performing oxidation modification, the content of oxygen in the modified mixed gas is adjusted according to the process conditions of the material to ensure the modification effect of the granular material.
[0010] Preferably, step 2) is to sequentially dry, carbonize, activate, oxidize and cool the granular material to obtain a carbon-based adsorption catalytic material.
[0011] Preferably, in step 1), the active component is one or more of coal with a volatile matter of not less than 30%, porous carbon powder, wood ash, and a pore-forming agent, preferably one or more of lignite, porous carbon powder, wood ash, ammonium bicarbonate, and stearic acid.
[0012] Preferably, in step 1), the amount of the active component added is 0-30% by mass of the coal powder, preferably 1-20% by mass.
[0013] Preferably, in step 1), the binder is one or more of coal tar, carboxymethyl cellulose, polyvinyl alcohol, sesbania powder, phenolic resin, starch, and bentonite.
[0014] Preferably, in step 1), the amount of the binder added is 1-35% by mass of the coal powder, preferably 2-30% by mass.
[0015] Preferably, in step 1), the mass content of water in the mixture is 8-28%, preferably 10-24%.
[0016] Preferably, in step 1), the particle size of the mixture is no greater than 200 mesh, preferably no greater than 300 mesh.
[0017] Preferably, in step 1), the extrusion molding includes stirring and kneading, pre-extrusion and molding in sequence. The particle size of the granules is 3 to 15 mm, preferably 4 to 12 mm. The shape of the granules includes but is not limited to one of spherical, cylindrical, rectangular, honeycomb, and amorphous, preferably spherical or cylindrical.
[0018] Preferably, the stirring and kneading is carried out by using one of a vertical strong stirring mixer, a horizontal strong stirring mixer, and an oblique horizontal strong stirring mixer. The pre-extrusion is carried out by using one of a vertical screw extruder, a horizontal screw extruder, and an oblique horizontal screw extruder. The molding is carried out by using one of a flat die granulator, a ring die granulator, a screw extrusion granulator, a disc granulator, a double roller granulator, and an extrusion granulator.
[0019] As a preferred method, the oxygen content in the modified mixed gas is adjusted as follows: the oxygen content in the modified mixed gas is set as x 0 , %, then:
[0020] (1)
[0021] In the above formula (1), m is the correction constant, which is 6.5 to 7. a is the increment of volatile matter in the pellets, which is 0.01 to 2%. 1 is the volume of water-containing air introduced per unit time, m 3 .v 2 is the volume of water vapor introduced per unit time, m 3 .v 3 is the volume of protective gas introduced per unit time, m 3 .x 1 is the oxygen content in water-containing air, %. 2 is the oxygen content in water vapor, %. 1 is the density of water-containing air, kg / m 3 ρ 2 is the density of water vapor, kg / m 3 ρ 3 is the density of the protective gas, kg / m 3 ρ 4 is the bulk density of the pellets, kg / m 3 .c 1 is the specific heat capacity of air containing water, J / (kg×℃). 2 is the specific heat capacity of water vapor, J / (kg×℃). 3 is the specific heat capacity of the protective gas, J / (kg×℃). 4 is the specific heat capacity of the pellets, which is 840 J / (kg×℃). b is the incremental correction coefficient of the functional groups on the surface of the pellets, which is 0.67~1.33. k is the heat transfer coefficient between the pellets and the modified mixed gas, which is 0.5~0.99. s is the contact area parallel to the airflow when the mixed modified gas is passed into the pellet layer, m 2 h is the average bed thickness of the granular material layer parallel to the airflow, m. 1 is the real-time temperature of the particle material layer before oxidation modification, °C. t2 is the target temperature of the particle material layer after oxidation modification, °C. t 3 is the temperature of the modified mixed gas before oxidation modification, °C. 4 is the temperature of the modified mixed gas after oxidation modification, ℃. Preferably, 200℃≤t 1 ≤800℃,t 2 <50℃.
[0022] Preferably, in step 2), the flow rate of the modified mixed gas is set as V, m / s. Then:
[0023] V=(v 1 +v 2 +v 3 ) / (T*s) (2).
[0024] In formula (2), T is the time for the modified mixed gas to vertically contact the particle material layer, in minutes. Preferably, 5 minutes ≤ T ≤ 240 minutes (more preferably, 10 minutes ≤ T ≤ 180 minutes).
[0025] Preferably, the protective gas is one or more of nitrogen, inert gas and carbon dioxide.
[0026] Preferably, in step 2), the drying is online drying, and the drying temperature is lower than 300° C., preferably 100-260° C. The moisture content of the granules after drying is lower than 8wt%, preferably lower than 6wt%.
[0027] Preferably, in step 2), the carbonization temperature is 200-1000° C., preferably 300-900° C. The carbonization time is 0.3-3 h, preferably 0.5-2.5 h.
[0028] Preferably, the equipment for drying the pellets is an electric heat dryer or an air heat dryer, and the drying method is contact heat exchange drying or indirect heat exchange drying. The equipment used for carbonization is a translationally propelled belt electric heating furnace or a belt electric heating and flue gas combustion mixed heating furnace.
[0029] Preferably, the preparation method further comprises:
[0030] 3) The flue gas generated during the carbonization process is incinerated to obtain high-temperature tail gas, which is recycled for drying treatment or transported to the waste heat boiler to produce hot water or water vapor. The water-containing air generated during the drying process and the water vapor generated by the waste heat boiler are recycled for oxidation modification treatment.
[0031] Preferably, in step 2), the activation temperature is 850-1100° C., preferably 900-1000° C. The activation time is 1-6 hours, preferably 2-5 hours.
[0032] Preferably, the activation device is a Slep activation furnace.
[0033] In the present invention, the formula of carbon-based adsorption catalytic materials for flue gas purification is optimized, mainly using ordinary raw coal powder (usually including various types of coking coal, semi-coke, coke powder, bituminous coal, anthracite, etc.) with active components (such as lignite, porous carbon powder, wood ash, ammonium bicarbonate, stearic acid, etc.) and binders (such as coal tar, carboxymethyl cellulose, polyvinyl alcohol, sesbania powder, phenolic resin, starch, bentonite, etc.) and then adding water to participate in granulation. Specifically, the ordinary raw coal and the active components are prepared in proportion and pre-mixed, and then sent to the grinding equipment through a belt to grind through a 200-mesh or 300-mesh sieve. The raw coal and the active components are preliminarily mixed and then ground into a certain particle size, so that it is easier to carry out uniform stirring and later carbonization to form strength and activation to form pores. The amount of the active component added is 0-30% (preferably 1-20%, more preferably 3-15%) of the raw coal mass. It is further preferred that the addition ratio of high-quality young coal (such as lignite) is 0-20% (preferably 1-15%, more preferably 5-12%) of the raw coal mass; the addition ratio of porous carbon powder is 0-30% (preferably 5-20%, more preferably 5-15%) of the raw coal mass; the addition ratio of pore former (or pore expander) is 0-10% (preferably 2-8%, more preferably 3-5%) of the raw coal mass. The desulfurization value of carbon-based purification material products can be greatly improved by adding active raw materials to the raw materials to optimize the coal blending scheme.
[0034] In the present invention, when the oxidation modification treatment is carried out, according to the process conditions of the materials (including the increment of volatile matter in the granular material, the volume of water-containing air introduced into the oxidation equipment (such as a rotary kiln), the volume of water vapor introduced, the volume of protective gas introduced, the oxygen content in the water-containing air, the oxygen content in the water vapor, the density of the water-containing air, the density of the water vapor, the density of the protective gas, the bulk density of the granular material, the specific heat capacity of the water-containing air, the specific heat capacity of the water vapor, the specific heat capacity of the protective gas, the specific heat capacity of the granular material, the contact area of the modified mixed gas in the direction parallel to the airflow when the modified mixed gas is introduced into the granular material layer, The average bed thickness of the particle material layer along the direction parallel to the airflow, the real-time temperature of the particle material layer before oxidation modification, the target temperature of the particle material layer after oxidation modification, the temperature of the modified mixed gas before oxidation modification, the temperature of the modified mixed gas after oxidation modification, the vertical contact modification time of the modified mixed gas and the carbon-based material, the flow rate of the modified mixed gas, etc.), the incremental correction coefficient of the functional group on the surface of the particle material, the heat exchange coefficient between the particle material and the modified mixed gas are introduced. When performing oxidation modification treatment, the modification effect of the particle material is ensured by adjusting the oxygen content in the modified mixed gas.
[0035] Furthermore, in the present invention, in the automatic batching process, the coal powder and the binder can be directly introduced into the mixing device separately, or they can be mixed together and then introduced into the mixing device simultaneously; water can be added to the mixing device by flowing into the spraying or spraying method. The intensive mixing device can be a vertical, horizontal or oblique mixer with stirring blades, preferably a vertical intensive mixer. The pre-extrusion device can be a vertical, horizontal or oblique screw extruder, preferably a horizontal screw extruder. The appearance of the granular material can be spherical (including elliptical spherical), cylindrical, rectangular, honeycomb, amorphous, preferably spherical or cylindrical. The molding is carried out by using one of a flat die granulator, a ring die granulator, a screw extrusion granulator, a disc granulator, a double roller granulator, and an extrusion granulator, and the size of the granular material is generally 3~15mm.
[0036] In the present invention, the carbon-based material molding material (i.e., granular material) obtained by extrusion molding has a high moisture content and is generally soft. If it is directly carbonized, it is easy to break during the carbonization process, resulting in a low yield. At the same time, direct carbonization of the molding material with a high moisture content will also affect the porosity and strength of the carbon-based material, resulting in the performance of the carbon-based material being affected. In addition, the water and volatile matter volatilized by the carbon-based material during the carbonization process will mix together to reduce the overall calorific value of the carbonization exhaust gas, making it difficult to ignite stably, resulting in the need for external coal burning, which increases energy consumption and costs. Therefore, in the present invention, the formed pellets are first conveyed into a drying device via a belt conveyor for online drying treatment, so that the moisture content is reduced to a certain range and the strength is improved to a certain extent. The dried tail gas can be sent to the oxidation modification process for use; when the pellets are dried to a certain moisture content (such as a moisture content lower than 8wt%) and a certain strength, they are then conveyed into a belt carbonization furnace via a belt, and carbonized from low temperature to high temperature for a period of time under an environment of 200-1000°C (the final carbonization temperature is preferably 600-900°C, more preferably 650-800°C; the carbonization time of the belt carbonization process is preferably 0.3-3h), and the flue gas generated can be sent to an incinerator for online combustion, and a part of the tail gas generated by the combustion is used for the online drying process, and a part enters the waste heat boiler for heat exchange to generate steam, and the generated steam is used for activation and oxidation modification processes or for waste heat power generation.
[0037] Furthermore, in the present invention, the drying equipment can be an electric heating auxiliary equipment, or a sealed equipment with direct heat exchange of tail gas; the drying temperature is generally not higher than 300°C, and can be reasonably adjusted according to the actual working conditions. The belt carbonization furnace is preferably a horizontal translational push-type electric heating furnace. Through high-temperature belt carbonization heat treatment, the raw coal and other materials can be condensed and melted at high temperature to finally form a carbon-based material with a high skeleton strength and a certain pore structure; using a belt furnace for carbonization in a relatively static state can reduce the wear of the granular material and improve the yield of the carbonization process; the temperature control and stability of the belt furnace are greatly improved compared to the rotary furnace, which helps to ensure uniform carbonization of the material and reduce performance fluctuations; at the same time, in the belt carbonization furnace, a multi-layer and multi-row material distribution method can be used, so that the use of a belt furnace for carbonization can greatly increase the single-machine capacity of carbonization.
[0038] In the present invention, the carbonized pellets can be oxidatively modified by steam-compounded protective gas and air (i.e., modified mixed gas) during the cooling process (including the cooling cylinder) of the pellets discharged from the carbonization furnace; the carbonized pellets react with the modified mixed gas composed of water-containing air, water vapor, protective gas (such as nitrogen or inert gas or carbon dioxide) and oxygen at a higher temperature to increase the specific oxygen-containing functional groups on the surface of the carbon-based material, thereby greatly promoting the improvement of the denitrification rate while ensuring that other indicators are qualified; the presence of steam and protective gas can prevent the pellets from catching fire, and at the same time, water vapor and carbon will also undergo a chemical reaction at a certain temperature to absorb heat, which can partially offset the temperature rise caused by the oxidation reaction, thereby preventing the local temperature from being too high.
[0039] In the present invention, the carbonized material still has a relatively high temperature. Therefore, the hot material after carbonization is subjected to oxidation modification treatment by introducing a modified mixed gas into the carbonization cooling section. On the one hand, the heat demand for modification can be met by utilizing the waste heat after the carbonization of the material, without the need for an additional heat source, thereby reducing energy consumption. In addition, since the raw material formula is optimized and matched and a specially matched modified mixed gas is used for the oxidation modification process with targeted oxygen content control, the material that has only undergone oxidation modification treatment can have better adsorption catalytic purification performance, and can meet the purification demand for flue gas without activation treatment. Moreover, the oxidation modification cycle is much lower than the existing activation cycle, which significantly reduces the production cycle of carbon-based materials while reducing the investment in the activation process, thereby having significant social and economic benefits.
[0040] In the present invention, according to the granulation and index requirements of the target carbon-based material, the coal powder, active component, binder, and water are mixed by automatic batching and then sent to a strong mixing device in sequence for stirring and kneading, and the uniformly stirred primary mixture is sent to a pre-extrusion device for pre-extrusion treatment to obtain a secondary mixture that has been partially air-expelled and preliminarily compacted, and finally the pre-extruded secondary mixture is sent to a molding device to obtain a molding material, and a granular material can be obtained. The automatic batching system can improve the continuity of each raw material falling into the stirring device, and the automatic control of the discharge by the equipment can achieve a relatively accurate material stable ratio, which is beneficial to the stability of production and the stability of product performance. The strong mixing device can realize the continuity and automation of the whole process of the coal powder mixture from entering the stirring to being sent to the granulation, and can also make the solid coal powder, binder and liquid water stirred and kneaded more evenly, further ensuring the stability of product performance. The coal powder kneaded material can be preliminarily extruded and compacted by the pre-extrusion process to discharge the air in the kneaded material, which will help to improve the compactness and density of the particles during subsequent granulation and reduce the appearance of bubble holes. That is to say, the present invention can greatly improve the continuity and automation level of the pre-granulation process by using automatic batching, strong mixing and pre-extrusion processes, while improving the uniformity and compactness of the mixed materials, and has a significant optimization effect on the uniformity of subsequent product performance.
[0041] In the present invention, the modification effect of the pellets is ensured by adjusting the content of oxygen in the modified mixed gas according to the process conditions of the materials. Specifically, the space velocity and oxygen content of the modified mixed gas when the pellets are oxidized and modified are calculated according to the device structure, ambient temperature, material layer thickness, etc. of the carbon-based material, so that the pellets can be oxidized as evenly as possible, and high temperature or combustion is avoided, effectively ensuring the qualified rate and uniformity of the finished carbon-based materials. Wherein: adjusting the content of oxygen in the modified mixed gas is specifically: setting the content of oxygen in the modified mixed gas to be x 0 , %, then:
[0042] (1)
[0043] In the above formula (1), m is the correction constant, which is 6.5 to 7. a is the increment of volatile matter in the pellets, which is 0.01 to 2%. 1 is the volume of water-containing air introduced per unit time, m 3 .v 2 is the volume of water vapor introduced per unit time, m 3 .v 3 is the volume of protective gas introduced per unit time, m 3 .x 1 is the oxygen content in water-containing air, %. 2 is the oxygen content in water vapor, %.1 is the density of water-containing air, kg / m 3 ρ 2 is the density of water vapor, kg / m 3 ρ 3 is the density of the protective gas, kg / m 3 ρ 4 is the bulk density of the pellets, kg / m 3 .c 1 is the specific heat capacity of air containing water, J / (kg×℃). 2 is the specific heat capacity of water vapor, J / (kg×℃). 3 is the specific heat capacity of the protective gas, J / (kg×℃). 4 is the specific heat capacity of the pellets, which is 840 J / (kg×℃). b is the incremental correction coefficient of the functional groups on the surface of the pellets, which is 0.67~1.33. k is the heat transfer coefficient between the pellets and the modified mixed gas, which is 0.5~0.99. s is the contact area parallel to the airflow when the mixed modified gas is passed into the pellet layer, m 2 h is the average bed thickness of the granular material layer parallel to the airflow, m. 1 is the real-time temperature of the particle material layer before oxidation modification, °C. t 2 is the target temperature of the particle material layer after oxidation modification, °C. t 3 is the temperature of the modified mixed gas before oxidation modification, °C. 4 is the temperature of the modified mixed gas after oxidation modification, ℃. Preferably, 200℃≤t 1 ≤800℃,t 2 <50℃.
[0044] In a preferred embodiment of the present invention, the modified mixed gas is a mixed gas obtained by combining steam with a protective gas and then combining air and / or oxygen.
[0045] Furthermore, by controlling the flow rate of the modified mixed gas, the oxidation modification effect is further improved, and the flow rate of the modified mixed gas is set to V, m / s. Then:
[0046] V=(v 1 +v 2 +v 3 ) / (T*s) (2).
[0047] In formula (2), T is the time for the modified mixed gas to vertically contact the particle material layer, min. Preferably, 5 min ≤ T ≤ 240 min.
[0048] It should be noted that although similar oxidation modification is also carried out when preparing activated carbon in the prior art, the oxygen content in the gas introduced is within a fixed range. However, in the actual process, due to changes in raw materials, changes in process conditions, different gas compositions, etc., it is difficult to ensure the modification effect of activated carbon when using a gas with a fixed range of oxygen content for oxidation modification of activated carbon. After a large number of experiments, the inventor explored the factors that affect the modification of carbon-based adsorption catalytic materials when the carbon-based adsorption catalytic materials are oxidatively modified, and found that the oxygen content in the mixed gas needs to be adjusted according to the specific process. If the raw materials change, the process conditions change, and the gas composition changes, the content of oxygen in the mixed gas introduced must be adjusted according to the actual process conditions to ensure the modification effect of the carbon-based purification material. The inventors verified through experiments that the content of oxygen in the introduced mixed gas is directly related to the increment of volatile matter in the granular material, the volume of water-containing air introduced into the oxidation equipment (such as a rotary kiln), the volume of water vapor introduced, the volume of protective gas introduced, the oxygen content in the water-containing air, the oxygen content in the water vapor, the density of the water-containing air, the density of the water vapor, the density of the protective gas, the bulk density of the granular material, the specific heat capacity of the water-containing air, the specific heat capacity of the water vapor, the specific heat capacity of the protective gas, the specific heat capacity of the granular material, the contact area of the mixed modified gas with the direction parallel to the airflow when the mixed modified gas is introduced into the granular material layer, the average bed thickness of the granular material layer along the direction parallel to the airflow, the real-time temperature of the granular material layer before oxidation modification, the target temperature of the granular material layer after oxidation modification, the temperature of the modified mixed gas before oxidation modification, the temperature of the modified mixed gas after oxidation modification, the vertical contact modification time of the modified mixed gas with the carbon-based material, the flow rate of the modified mixed gas, etc. In order to ensure the modification effect of the carbon-based adsorption catalytic material, it is necessary to comprehensively consider the specific process conditions. The present invention introduces a correction coefficient of the incremental functional group on the surface of the particle material and a heat exchange coefficient between the particle material and the modified mixed gas to fit the control means when controlling the oxygen content in the mixed gas in combination with specific process conditions, thereby obtaining a method for controlling the oxygen content in the mixed gas in combination with specific process conditions.
[0049] In the present invention, when the carbon-based material is subjected to oxidation modification, if the oxygen content in the mixed gas is too high, the carbon-based material will easily react violently with oxygen and heat up or catch fire; if the oxygen content in the mixed gas is too low, it will be difficult to achieve the purpose of increasing the oxygen-containing functional groups of the carbon-based material through oxidation modification, and it will be difficult to achieve the effect of improving the denitrification rate. Therefore, when the carbon-based material is subjected to oxidation modification, the oxygen content in the mixed gas needs to be strictly controlled; and the oxygen content in the mixed gas is not a fixed range value, but should be calculated according to specific process conditions. The inventors of the present application have obtained a specific method for controlling the oxygen content in the mixed gas through experimental research.
[0050] In the present invention, in order to further improve the flue gas purification performance of the carbon-based adsorption catalytic material, the material can be selectively activated before the oxidation modification treatment, and the activation treatment method is basically consistent with the activation process of the prior art. In other words, through the activation treatment, the various performance indicators of the carbon-based material can be optimized in advance, which is conducive to the subsequent product performance after the oxidation modification treatment to be able to cope with and meet the higher demand for flue gas purification in the future. It should be noted that, since the oxidation modification treatment is required in the future in the present invention, the duration of the activation treatment can be reduced relative to the prior art during the activation treatment, that is, when the material is activated first under the premise of adding the oxidation modification treatment process, the activation cycle can be significantly shortened.
[0051] In the present invention, the granular material that has been initially oxidatively modified needs to be added to an activation furnace for activation treatment, that is, a certain amount of steam is introduced into the activation section of the activation furnace, and the activation reaction is carried out for a period of time in a thermal environment of 850-1100°C (preferably 900-1000°C). In the environment of high temperature and steam, the granular material has a significant pore opening and pore expansion effect on the carbon-based material particles through the oxidation reaction of water vapor and solid carbon, and the micropores, specific surface area, and pore volume of the carbon-based material particles are sharply increased, thereby improving the adsorption performance of the carbon-based material. The flue gas generated during the activation process is treated in the same manner as the flue gas generated by carbonization.
[0052] Compared with the prior art, the beneficial technical effects of the present invention are as follows:
[0053] 1: The present invention can greatly reduce the production cycle and energy consumption on the basis of ensuring that the carbon-based materials meet the needs of flue gas purification through raw material optimization and process optimization. That is, after adding active components to prepare materials and forming them, drying, carbonization, oxidation modification, cooling and other treatments are carried out in sequence to obtain a carbon-based adsorption catalytic material for flue gas purification with rich and uniform pores, high and stable strength, and rich oxygen-containing functional groups on the surface of the material. The material has the advantages of short production cycle, low energy consumption, excellent desulfurization and denitrification performance, and high cycle stability.
[0054] 2: The present invention can make full use of the waste heat of the pellets by subjecting them to high-temperature oxidation modification in the cooling section of the carbonization furnace, and can obtain high-quality carbon-based materials without increasing energy consumption. At the same time, the air used for oxidation modification can come from the exhaust gas after online drying, and the required steam can come from the steam produced by the waste heat boiler, which can realize the recycling of air flow and heat flow, and improve the efficiency of energy and resource utilization. In addition, by replacing the traditional activation process with high-temperature oxidation modification, the production cycle is greatly reduced and the production energy consumption is significantly reduced while obtaining high-quality carbon-based materials.
[0055] 3: The method of the present invention can further selectively carry out or not carry out the activation process, thereby further enhancing the performance of the carbon-based material, thereby meeting higher requirements for flue gas purification. In addition, the process of the present invention also has the advantages of automatic operation, large production capacity, high production efficiency, high waste heat utilization efficiency, and significant economic, environmental and social benefits. BRIEF DESCRIPTION OF THE DRAWINGS
[0056] Figure 1 The figure is a simplified process flow diagram of the preparation method of the present invention.
[0057] Figure 2 The figure is an overall flowchart of the process of the preparation method of the present invention. DETAILED DESCRIPTION
[0058] The technical solution of the present invention is illustrated below by way of example, and the scope of protection requested by the present invention includes but is not limited to the following embodiments. Example 1
[0059] like Figure 1-2 As shown, a method for preparing a carbon-based adsorption catalytic material comprises:
[0060] 1) Coal powder, active components, binder and water are mixed to obtain a mixture, and then the mixture is extruded to obtain pellets.
[0061] 2) The pellets are sequentially dried, carbonized, oxidized and cooled to obtain a carbon-based adsorption catalytic material.
[0062] Among them, oxidation modification is to use water-containing air, water vapor, protective gas and oxygen as the modified mixed gas to modify the granular material. When performing oxidation modification, the content of oxygen in the modified mixed gas is adjusted according to the process conditions of the material to ensure the modification effect of the granular material. Example 2
[0063] Example 1 was repeated, except that in step 1), the active component was lignite (volatile matter content of about 37%). Example 3
[0064] Example 2 was repeated, except that in step 1), the amount of the active component added was 12% of the mass of the coal powder. Example 4
[0065] Example 3 was repeated, except that in step 1), the binder was starch. Example 5
[0066] Example 4 was repeated, except that in step 1), the amount of the binder added was 3.3% of the mass of the coal powder. Example 6
[0067] Example 5 was repeated, except that in step 1), the mass content of water in the mixture was 18%. Example 7
[0068] Example 6 was repeated, except that in step 1), the particle size of the mixture was no greater than 200 mesh. Example 8
[0069] Example 7 is repeated, except that in step 1), the extrusion molding sequentially includes stirring and kneading, pre-extrusion and molding. The average particle size of the granules is 9 mm. The shape of the granules includes but is not limited to cylindrical. Example 9
[0070] Example 8 was repeated, except that the stirring and kneading was performed using a vertical strong stirring mixer, the pre-extrusion was performed using a horizontal screw extruder, and the molding was performed using an extrusion granulator. Example 10
[0071] Example 9 was repeated except that the protective gas was nitrogen. Embodiment 11
[0072] Example 10 was repeated, except that the oxygen content in the modified mixed gas was adjusted as follows: the oxygen content in the modified mixed gas was set to x 0 , %, then:
[0073] (1)
[0074] In the above formula (1), m is the correction constant, which is 6.9. a is the increment of volatile matter in the pellets, which is 1.7%. 1 is the volume of water-containing air introduced per unit time, m 3 .v 2 is the volume of water vapor introduced per unit time, m 3 .v 3 is the volume of protective gas introduced per unit time, m 3 .x 1 is the oxygen content in water-containing air, %. 2 is the oxygen content in water vapor, %. 1 is the density of water-containing air, kg / m 3 ρ 2 is the density of water vapor, kg / m 3 ρ 3 is the density of the protective gas, kg / m 3 ρ 4 is the bulk density of the pellets, kg / m 3 .c 1is the specific heat capacity of air containing water, J / (kg×℃). 2 is the specific heat capacity of water vapor, J / (kg×℃). 3 is the specific heat capacity of the protective gas, J / (kg×℃). 4 is the specific heat capacity of the pellets, which is 840 J / (kg×℃). b is the incremental correction coefficient of the functional groups on the surface of the pellets, which is 0.98. k is the heat transfer coefficient between the pellets and the modified mixed gas, which is 0.71. s is the contact area parallel to the gas flow when the mixed modified gas passes into the pellet layer, m 2 h is the average bed thickness of the granular material layer parallel to the airflow, m. 1 is the real-time temperature of the particle material layer before oxidation modification, °C. t 2 is the target temperature of the particle material layer after oxidation modification, °C. t 3 is the temperature of the modified mixed gas before oxidation modification, °C. 4 is the temperature of the modified mixed gas after oxidation modification, °C. t 1 =450±30℃,t 2 =30±5℃. Example 12
[0075] Example 11 is repeated, except that the flow rate of the modified mixed gas is recorded as V, m / s. Then:
[0076] V=(v 1 +v 2 +v 3 ) / (T*s) (2).
[0077] In formula (2), T is the time for the modified mixed gas to vertically contact the particle material layer, T = 60 min. Example 13
[0078] Example 12 was repeated, except that the drying was performed online at a temperature of 200±10° C. The moisture content of the granules after drying was about (4±0.5) wt %. Embodiment 14
[0079] Example 13 was repeated except that the carbonization temperature was 800±50° C. and the carbonization time was 0.8 h. Embodiment 15
[0080] Example 14 was repeated, except that the equipment used to dry the pellets was an air-heated dryer with electric auxiliary heating. The drying method was indirect heat exchange drying. The equipment used for carbonization was a belt-type electric heating furnace with translational propulsion. Example 16
[0081] Example 15 was repeated, except that the preparation method further included:
[0082] 3) The flue gas generated during the carbonization process is incinerated to obtain high-temperature tail gas, which is recycled for drying treatment or transported to the waste heat boiler to produce hot water and water vapor. The water-containing air generated during the drying process and the water vapor generated by the waste heat boiler are recycled for oxidation modification treatment. Embodiment 17
[0083] Example 16 was repeated, except that in step 2), the granular material was sequentially dried, carbonized, activated, oxidatively modified and cooled to obtain a carbon-based adsorption catalytic material. Embodiment 18
[0084] Example 17 was repeated except that the activation temperature was 950±50° C. and the activation time was 2.5 h. Embodiment 19
[0085] Example 18 was repeated except that the activation equipment used was a Slep activation furnace.
[0086] Application Example 1
[0087] The carbon-based adsorption catalytic material was prepared by the preparation method described in Example 16. Under the current working conditions, the increment a of the volatile matter in the pellet material was 1.7%, the increment correction coefficient b of the functional group on the surface of the pellet material was 0.98, and the heat exchange coefficient k between the pellet material and the modified mixed gas was 0.71. Other working condition data of the material were obtained according to the test (where: t 1 465℃, t 2 The oxygen content in the modified mixed gas during oxidation treatment was calculated by using formulas (1)-(2) to be 1.45% and the flow rate of the modified mixed gas was 5.85 m / s. After the oxidation treatment, the carbon-based adsorption catalytic material was obtained by cooling and screening.
[0088] After testing, it was found that the wear resistance of the carbon-based adsorption catalytic material prepared in this application example was 97.6%, the coefficient of variation of the compressive strength was 15.6% (much lower than the average value of 30% of activated carbon purchased on the market), the flue gas desulfurization efficiency was 23.4 mg / g, and the denitrification efficiency was 62.2%.
[0089] Cycle stability: After 5 cycles of use, the desulfurization efficiency of the carbon-based adsorption catalytic material prepared in this application example was maintained at 23.1 mg / g (higher than 20.6 mg / g of carbon-based materials purchased on the market), and the denitrification efficiency was approximately 73.1%; after 10 cycles of use, the desulfurization efficiency of the carbon-based adsorption catalytic material prepared in this example was maintained at 22.6 mg / g (higher than 20.6 mg / g of carbon-based materials purchased on the market), and the denitrification efficiency was approximately 83.5%.
[0090] Application Example 2
[0091] The carbon-based adsorption catalytic material was prepared by the preparation method described in Example 19. Under the current working conditions, the increment a of the volatile matter in the pellet material was 1.6%, the increment correction coefficient b of the functional group on the surface of the pellet material was 0.98, and the heat exchange coefficient k between the pellet material and the modified mixed gas was 0.71. Other working condition data of the material were obtained according to the test (wherein: t 1 570℃, t 2 The oxygen content in the modified mixed gas during oxidation treatment was calculated by using formulas (1)-(2) to be 1.32% and the flow rate of the modified mixed gas was 5.85 m / s. After the oxidation treatment, the carbon-based adsorption catalytic material was obtained by cooling and screening.
[0092] After testing, it was found that the wear resistance of the carbon-based adsorption catalytic material prepared in this application example was 97.5%, the coefficient of variation of the compressive strength was 17.5% (much lower than the average value of 30% of activated carbon purchased on the market), the flue gas desulfurization efficiency was 25.1 mg / g, and the denitrification efficiency was 63.1%.
[0093] Cycle stability: After 5 cycles of use, the desulfurization efficiency of the carbon-based adsorption catalytic material prepared in this application example was maintained at 24.5 mg / g (higher than 20.6 mg / g of carbon-based materials purchased on the market), and the denitrification efficiency was maintained at 74.7%; after 10 cycles of use, the desulfurization efficiency of the carbon-based adsorption catalytic material prepared in this example was maintained at 23.9 mg / g (higher than 20.6 mg / g of carbon-based materials purchased on the market), and the denitrification efficiency was maintained at 85.6%.
[0094] Application Example 3
[0095] Example 1 was applied repeatedly, except that the oxygen content in the modified mixed gas was increased from 1.45% to 1.51% under the premise that the operating conditions remained unchanged.
[0096] Application Example 4
[0097] Example 1 was applied repeatedly, except that the oxygen content in the modified mixed gas was reduced from 1.45% to 1.36% under the premise that the operating conditions remained unchanged.
[0098] Application Example 5
[0099] Example 2 was applied repeatedly, except that the oxygen content in the modified mixed gas was increased from 1.32% to 1.68% under the premise that the operating conditions remained unchanged.
[0100] Application Example 6
[0101] Example 2 was applied repeatedly, except that the oxygen content in the modified mixed gas was reduced from 1.32% to 1.15% under the premise that the operating conditions remained unchanged.
[0102] Comparative Example 1
[0103] Example 2 was repeated, except that the oxidation modification treatment was not performed, and the activation temperature was 950±50° C. The activation time was 2.5 h±0.5 h.
[0104] Comparative Example 2
[0105] The method of Example 1 was repeated except that a mixed gas having a volume ratio of water vapor to air of 15.5:1 was used as the modified mixed gas during the oxidation modification treatment.
[0106] Comparative Example 3
[0107] Example 2 was applied repeatedly, except that a mixed gas of water vapor, air and nitrogen in a volume ratio of 10:1:5.5 was used as the modified mixed gas during the oxidation modification treatment.
[0108] The data of each application example and the comparison example are as follows:
[0109]
[0110] In actual working conditions, the desulfurization value of carbon-based purification materials usually shows a gradual downward trend during the process of engineering recycling. This is because although there is an acidification and pore expansion effect during use, the adhesion and pore blocking of fine dust in the flue gas are usually more significant, and during the material operation and screening process, fine dust is difficult to fall off from the surface of the material or the inside of the pores, which generally leads to the damage of the adsorption performance of the carbon-based material. In addition, the denitrification rate of carbon-based purification materials usually shows a gradual upward trend during the process of engineering recycling. This is because the carbon-based purification materials are constantly in contact and react with oxygen-containing substances and various acidic and alkaline substances in the flue gas during the adsorption and analysis process, making the surface rich in various oxygen-containing or other active functional groups, and these active functional groups have a great promoting effect on the denitrification reaction, so the denitrification catalytic performance of the carbon-based materials will be improved.
Claims
1. A method for preparing a carbon-based adsorption catalytic material, characterized in that: The method includes: 1) Mixing coal powder, active components, a binder and water to obtain a mixture, and then extruding the mixture to obtain pellets; the active component is one or more of coal with a volatile content of not less than 30% and a pore-forming agent; 2) The pellets are sequentially dried, carbonized, oxidized and cooled to obtain a carbon-based adsorption catalytic material; 3) The flue gas generated in the carbonization process is incinerated to obtain high-temperature tail gas, which is recycled for drying treatment or transported to the waste heat boiler to produce hot water or water vapor; the water-containing air generated in the drying process and the water vapor generated by the waste heat boiler are recycled for oxidation modification treatment; Among them, oxidation modification is to use water-containing air, water vapor, protective gas and oxygen as modified mixed gas to modify the pellets; when performing oxidation modification, the modification effect of the pellets is ensured by adjusting the content of oxygen in the modified mixed gas according to the process conditions of the material; specifically, the content of oxygen in the modified mixed gas is set to x0,%, then: (1) In the above formula (1), m is the correction constant, which is 6.5~7; a is the increment of volatile matter in the pellets, which is 0.01~2%; v1 is the volume of water-containing air introduced per unit time, m 3 ; v2 is the volume of water vapor introduced per unit time, m 3 ; v3 is the volume of protective gas introduced per unit time, m 3 ; x1 is the oxygen content in water-containing air, %; x2 is the oxygen content in water vapor, %; ρ1 is the density of water-containing air, kg / m 3 ; ρ2 is the density of water vapor, kg / m 3 ; ρ3 is the density of the protective gas, kg / m 3 ; ρ4 is the bulk density of the pellets, kg / m 3 ; c1 is the specific heat capacity of water-containing air, J / (kg×℃); c2 is the specific heat capacity of water vapor, J / (kg×℃); c3 is the specific heat capacity of protective gas, J / (kg×℃); c4 is the specific heat capacity of granular material, which is 840J / (kg×℃); b is the incremental correction coefficient of functional groups on the surface of granular material, which is 0.67~1.33; k is the heat transfer coefficient between granular material and modified mixed gas, which is 0.5~0.99; s is the contact area of the mixed modified gas in the direction parallel to the gas flow when it passes into the granular material layer, m 2 ; h is the average bed thickness of the particulate material layer along the direction parallel to the airflow, m; t1 is the real-time temperature of the particulate material layer before oxidation modification, ℃; t2 is the target temperature of the particulate material layer after oxidation modification, ℃; t3 is the temperature of the modified mixed gas before oxidation modification, ℃; t4 is the temperature of the modified mixed gas after oxidation modification, ℃.
2. The preparation method according to claim 1, characterized in that: 200℃≤t1≤800℃, t2<50℃.
3. The preparation method according to claim 1, characterized in that: Step 2) is to sequentially dry, carbonize, activate, oxidize and cool the granular material to obtain a carbon-based adsorption catalytic material.
4. The preparation method according to any one of claims 1 to 3, characterized in that: In step 1), the amount of the active component added is 1-30% of the mass of the coal powder.
5. The preparation method according to claim 4, characterized in that: In step 1), the active component is one or more of lignite, porous carbon powder, plant ash, ammonium bicarbonate, and stearic acid; and / or In step 1), the amount of the active component added is 1-20% of the mass of the coal powder.
6. The preparation method according to any one of claims 1 to 3, characterized in that: In step 1), the binder is one or more of coal tar, carboxymethyl cellulose, polyvinyl alcohol, sesbania powder, phenolic resin, starch, and bentonite; and / or In step 1), the amount of the binder added is 1-35% of the mass of the coal powder; and / or In step 1), the mass content of water in the mixture is 8-28%.
7. The preparation method according to claim 6, characterized in that: In step 1), the amount of the binder added is 2-30% of the mass of the coal powder; and / or In step 1), the mass content of water in the mixture is 10-24%.
8. The preparation method according to any one of claims 1 to 3, characterized in that: In step 1), the particle size of the mixture is no more than 200 meshes.
9. The preparation method according to claim 8, characterized in that: In step 1), the particle size of the mixture is no more than 300 meshes.
10. The preparation method according to any one of claims 1 to 3, characterized in that: In step 1), the extrusion molding includes stirring and kneading, pre-extrusion and molding in sequence; the particle size of the granular material is 3-15 mm; the shape of the granular material is one of spherical, cylindrical, rectangular, honeycomb and amorphous.
11. The preparation method according to claim 10, characterized in that: The particle size of the granules is 4-12 mm; the shape of the granules is spherical or cylindrical.
12. The preparation method according to claim 10, characterized in that: The stirring and kneading is carried out by using one of a vertical strong stirring mixer, a horizontal strong stirring mixer, and an oblique horizontal strong stirring mixer; the pre-extrusion is carried out by using one of a vertical screw extruder, a horizontal screw extruder, and an oblique horizontal screw extruder; the molding is carried out by using one of a flat die granulator, a ring die granulator, a screw extrusion granulator, a disc granulator, a double roller granulator, and an extrusion granulator.
13. The preparation method according to any one of claims 1 to 3, characterized in that: In step 2), the flow rate of the modified mixed gas is set to V, m / s; then: V = (v1 + v2 + v3) / (T*s) (2); In formula (2), T is the time for the modified mixed gas to be in vertical contact with the particle material layer, min.
14. The preparation method according to claim 13, characterized in that: 5min≤T≤240min.
15. The preparation method according to any one of claims 1 to 3, characterized in that: The protective gas is one or more of nitrogen, inert gas and carbon dioxide.
16. The preparation method according to any one of claims 1 to 3, characterized in that: In step 2), the drying is online drying, the drying temperature is lower than 300° C.; the moisture content of the granules after drying is lower than 8wt%; and / or In step 2), the carbonization temperature is 200-1000° C. and the carbonization time is 0.3-3 h.
17. The preparation method according to claim 16, characterized in that: The drying temperature is 100-260°C; the moisture content of the pellets after drying is less than 6wt%; and / or In step 2), the carbonization temperature is 300-900° C. and the carbonization time is 0.5-2.5 h.
18. The preparation method according to any one of claims 1 to 3, characterized in that: The equipment for drying the pellets is an electric drying machine or an air drying machine, and the drying method is contact heat exchange drying or indirect heat exchange drying; the equipment used for carbonization is a translationally propelled belt electric heating furnace or a belt electric heating and flue gas combustion mixed heating furnace.
19. The preparation method according to claim 3, characterized in that: In step 2), the activation temperature is 850-1100° C. and the activation time is 1-6 hours.
20. The preparation method according to claim 19, characterized in that: In step 2), the activation temperature is 900-1000° C. and the activation time is 2-5 hours.
21. The preparation method according to claim 3 or 19, characterized in that: The equipment used for activation is a Slep activation furnace.