A cylindrical sodium ion battery
By using sodium zinc borate and sodium bismuth titanate to coat the cathode material in the sodium-ion battery, and adding specific additives to the electrolyte to form an SEI film, the problems of insufficient cycle stability and high-temperature performance of the sodium-ion battery are solved and achieved. Efficient battery performance improvement and cost reduction.
Patent Information
- Application Number
- CN202410782127.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-18
AI Technical Summary
Existing sodium-ion batteries have shortcomings in cycle stability and high-temperature performance. In particular, the dissolution of transition metal elements and side reactions in the cathode material lead to a decrease in battery performance. Moreover, the material cost is high and environmentally unfriendly, making it difficult to meet the requirements of commercial applications. .
Sodium zinc borate and sodium bismuth titanate are used to coat sodium nickel ferromanganate layered oxide as the positive electrode material, and bis[2-(trimethylsilyl)ethyl]diisopropylamino is added to the electrolyte. Phosphate ester and triallyl phosphate form a dense SEI film to improve the protection of the cathode surface. At the same time, the electrode material and electrolyte formula are optimized, and the dislocated bipolar ear structure is designed.
Significantly improve the cycle life and high-temperature performance of sodium-ion batteries, achieve high-current discharge above 10C, low-temperature discharge capacity reaches 77% of room temperature, reduce battery internal resistance, improve volume specific energy and high-rate discharge performance.
Smart Images

Figure CN118352656B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the field of sodium ion batteries, in particular to a cylindrical 26700-3300mAh sodium ion battery. Background Art
[0002] In recent years, the gradual depletion of fossil energy and the increasingly severe environmental protection situation have led to a shift in the focus on new sustainable clean energy, such as solar energy, wind energy, geothermal energy, and tidal energy. However, since these energy sources are unstable, intermittent, regional and environmentally dependent, it is necessary to establish supporting energy storage and conversion equipment in order to apply these energy sources to the actual life of society. In order to effectively utilize these energy sources, large-scale power storage systems are usually required to store the electricity converted from these energy sources and promote their use. At present, the more mature energy storage technologies include physical, electromagnetic and chemical energy storage, among which chemical energy storage has gradually become the mainstream of energy storage technology development due to its simplicity, high efficiency and real-time response.
[0003] Although lithium-ion batteries have been widely used in various fields, especially for large-scale energy storage, China's lithium resource production distribution is only 14%, and its high-quality battery-grade lithium carbonate reserves are even less, while sodium reserves are high, 420 times that of lithium reserves. Therefore, it is urgent to develop resource-rich, low-cost new energy storage secondary batteries as a substitute for lithium-ion batteries. According to the demand forecast for potential application scenarios of sodium-ion batteries, in terms of energy storage: it is expected that the energy storage installed capacity demand will be 48GWh in 2025; 41GWh for two-wheeled vehicles; 34GWh for A00-class vehicles. If sodium-ion batteries are used in all the above scenarios, the market space is expected to be 54.5 / 53.2 / 53.7 billion yuan from 2023 to 2025. In order to adapt to the expanding energy storage and power market, it is urgent to accelerate the development and promotion of sodium-ion batteries. It is expected that after the large-scale application of sodium-electric materials, the material cost of the sodium-electric system will be reduced by about 30%-40% compared with the lithium iron phosphate battery system. If it is to be widely used in commercial energy storage, in addition to energy density, it is also necessary to meet the requirements of long cycle life, high rate performance, good safety and cost-effectiveness. Taking various factors into consideration, SIBs have the great potential to replace lithium-ion batteries and become the new generation of energy storage devices for large-scale grid applications due to their low cost, abundant element reserves, environmental friendliness and good safety.
[0004] In addition to the similar working principle of sodium-ion batteries and lithium-ion batteries - the "rocking chair principle", the two are also very similar in the entire battery structure. The structure of a sodium-ion battery consists of a battery shell, a positive electrode material, a negative electrode material, a separator, an electrolyte, and a current collector. Sodium-ion batteries follow the same shell as lithium-ion batteries. The membrane used in sodium-ion batteries is commonly used in commercial lithium-ion batteries. For example, the polyolefin-based membrane commonly used in lithium-ion batteries can also be directly used in sodium-ion full batteries. The positive electrode materials of sodium-ion batteries on the market currently mainly include P2&O3 type layered structure oxides, Prussian blue compounds, polyanion compounds, and organic compounds. Advantages of the three positive electrode materials: layered oxides have high theoretical specific capacity, layered ion channels are suitable for sodium ion diffusion, small electrochemical polarization, low voltage platform, and slightly poor structure and thermal stability; Prussian blue compounds: transition metal hexacyanoferrate Na2M[Fe(CN)6], M=TM, etc., the lattice defect Fe(CN)6 vacancy is replaced by (H2O)6, and the coordinated water formed is difficult to remove, which is not conducive to long-cycle performance, and the material contains toxic group cyanide. Its synthesis process is very dangerous and has poor thermal stability, which has significant safety risks; polyanion compounds are NASICON and olivine structures, such as Na3V2(PO4)3 and NaFePO4, with high potential framework structure, good stability, poor conductivity (poor rate capability), slightly lower material cost, good cycle performance, and small compaction, but the materials of vanadium and fluorine systems are expensive and environmentally unfriendly, and the energy density of sodium iron pyrophosphate system is low, which is not suitable for commercial applications. Layered transition metal oxides are the most promising cathode materials for sodium-ion batteries due to their high theoretical specific capacity, good conductivity and fast diffusion kinetics. They are currently the most promising materials for energy storage and electric tools. Compared with soft-pack batteries, cylindrical batteries have higher steel shell strength and will not form obvious bulges after gas production. Therefore, cylindrical batteries are more suitable for the research and promotion of sodium-ion energy storage batteries. Summary of the invention
[0005] A cylindrical sodium ion battery, the invention adopts an optimized pole piece and electrolyte formula and a staggered bipolar ear structure design, so that the battery has high specific capacity and low internal resistance. The battery can have improved high current charge and discharge cycle performance, and can achieve a low-temperature discharge capacity of 77% of room temperature at -40°C, and the low-temperature performance is significantly better than that of lithium ion batteries. And it has a high cycle life at high temperature, and is mainly used in the fields of power tools and energy storage.
[0006] The present invention provides a cylindrical sodium ion battery, comprising an electrode assembly, an electrolyte and a cylindrical battery shell, characterized in that: the battery electrode group is a winding type electrode assembly, the electrode assembly comprises an inner layer diaphragm, a negative electrode sheet, a middle diaphragm and a positive electrode sheet, and the positive electrode sheet comprises sodium zinc borate Na3ZnB5O 10 and sodium bismuth titanate Na0.5 Bi 0.5 TiO3 composite coated sodium nickel iron manganese oxide layered oxide and polyacrylonitrile, wherein the mass ratio of sodium nickel iron manganese oxide layered oxide: sodium zinc borate: sodium bismuth titanate is 100:1.8-2.5:0.5-1, the electrolyte contains additives di[2-(trimethylsilyl)ethyl]diisopropylaminophosphoric acid ester and triallyl phosphate, and the mass percentage of sodium salt is 10-12% based on the total mass of the electrolyte; the mass percentage of organic solvent is 83-88% based on the total mass of the electrolyte; the mass percentage of di[2-(trimethylsilyl)ethyl]diisopropylaminophosphoric acid ester is 0.5-1%, and the mass percentage of triallyl phosphate is 1.5-4% based on the total mass of the electrolyte.
[0007] Furthermore, the outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, the outer layer of the middle diaphragm is wound around the positive electrode sheet, the inner diaphragm and the middle diaphragm are microporous composite films with a single-sided sodium bismuth titanate ceramic layer, the thickness of the inner diaphragm and the middle diaphragm is 9-16μm, and the ceramic layer faces the positive electrode sheet; the positive electrode sheet is aluminum foil, and a positive electrode blank section is left at the middle 1 / 3 and 2 / 3 of the positive electrode sheet, and the remaining position is coated with positive electrode slurry, and the positive electrode blank section is welded with the positive electrode The inner and outer pole ears, the inner and outer pole ears of the positive electrode are glued with high-temperature tape, the negative electrode sheet is copper foil or aluminum foil, the negative electrode sheet has negative electrode blank sections at the front and rear ends, and the negative electrode slurry is coated in the middle, the negative electrode inner and outer pole ears are welded on the negative electrode blank sections at the front and rear ends of the negative electrode sheet, and the negative electrode inner and outer pole ears are glued with high-temperature tape, wherein the width of the positive electrode inner and outer pole ears and the negative electrode inner and outer pole ears is 4mm, and the width of the high-temperature tape glued on the positive electrode inner and outer pole ears and the negative electrode inner and outer pole ears is 11mm.
[0008] Furthermore, the positive electrode sheet is prepared by the following method: sodium zinc borate Na3ZnB5O 10 and sodium bismuth titanate Na 0.5 Bi 0.5 TiO3 and sodium nickel iron manganese oxide layered oxide are mixed, placed in a ball mill, ethanol is used as a ball milling medium, and ball milled for 16-30 hours. The mixture is taken out and dried. Then the layered oxide material, polyacrylonitrile and conductive agent are placed in an N-methylpyrrolidone solution containing a binder, and a positive electrode slurry is formed by stirring and mixing, which is then coated on an aluminum foil.
[0009] Furthermore, the preparation of the negative electrode sheet is as follows: placing hard carbon and a conductive agent in a deionized water solution containing a binder, stirring and mixing to form a negative electrode slurry, and coating the mixture on a copper foil.
[0010] Furthermore, the mass ratio of the positive electrode slurry: the layered oxide material: polyacrylonitrile: conductive agent: binder = (90-97): (1-2): (1-8): (1-8).
[0011] Furthermore, the mass ratio of the negative electrode slurry: hard carbon: conductive agent: binder = (90-96): (1-6): (1-6).
[0012] Furthermore, the conductive agent is one or more of Super P, conductive graphite, Ketjen black, and carbon nanotubes, and the binder is one or more of polyvinylidene fluoride, styrene-butadiene rubber SBR, and PAA.
[0013] Furthermore, the electrolyte solution is prepared by dissolving NaPF6 and NaClO4 sodium salts in an organic carbonate solvent.
[0014] Beneficial technical effects of the present invention
[0015] The beneficial effects of the present invention compared with the traditional process are:
[0016] 1) The surface of the positive electrode active material is coated with sodium zinc borate (Na3ZnB5O 10 ) and sodium bismuth titanate (Na 0.5 Bi 0.5 TiO3), and the co-coating of sodium zinc borate and sodium bismuth titanate can improve the ionic conductivity of the positive electrode active material and provide more channels for the insertion and extraction of sodium ions; sodium zinc borate and sodium bismuth titanate are rich in sodium ions, which can replenish free sodium ions for the battery during the cycle, thereby improving the cycle life of the sodium ion battery;
[0017] 2) Adding polyacrylonitrile to the positive electrode, polyacrylonitrile can be coated on the surface of the active material, which can prevent the dissolution of transition metal elements in the positive electrode active material, such as Zn ions, thereby improving the cycle stability; at the same time, the electrolyte contains additives di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate and triallyl phosphate, which can form a dense SEI film on the positive electrode surface, thereby reducing the side reactions of the electrolyte on the positive electrode surface, thereby improving the cycle performance of sodium ion batteries at high temperatures;
[0018] 3) The sodium ion battery manufactured by the present invention uses suitable electrode materials and electrolytes to create a large battery capacity, not less than 3300mAh, a long battery cycle life, and a capacity retention rate of >90% for 2000 cycles of 10C discharge cycles; 2C charging, 3C discharge cycle 2000 cycles capacity retention rate >93%. The battery has good safety performance and has passed heavy impact, extrusion, single battery overcharge, 5S2P battery pack overcharge, normal temperature and high temperature short circuit, roller, drop, and low pressure tests. The battery can achieve a large current discharge of more than 10C, high discharge efficiency, and excellent cycle performance. It can achieve a low-temperature discharge capacity of -40℃ of 77% of room temperature, and its low-temperature performance is significantly better than that of lithium-ion batteries. The use of active materials with higher gram capacity and new conductive agents and binders, and the optimization of process parameters such as pole piece length and compaction density have significantly improved the battery's volume specific energy and high-rate discharge performance, as well as excellent high and low temperature performance. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 A schematic diagram of the structure of a battery electrode assembly made in the present invention;
[0020] Figure 2 It is a schematic diagram of the structure of the positive electrode sheet of the present invention;
[0021] Figure 3 It is a schematic diagram of the structure of the negative electrode sheet of the present invention;
[0022] Figure 4 1C discharge curves of the battery at different temperatures made in Example 1 of the present invention;
[0023] Figure 5 The capacity retention rate graph of the battery made for Example 1 of the present invention for >1000 cycles. DETAILED DESCRIPTION
[0024] The present invention will be described in more detail below through specific embodiments, but the protection scope of the present invention is not limited to these embodiments.
[0025] Taking the manufacture of cylindrical 26700mAh lithium battery as an example, the tap density is 1.6g / cm 3 , specific surface area 0.5m 2 / g, D50 at 5μm, gram capacity of 130mAh / g layered oxide material NaNi 0.33 Mn 0.33 Fe 0.33 O2, and a predetermined mass percentage of nano-Na3ZnB5O 10 and nano-Na 0.5 Bi 0.5 TiO3 was mixed and placed in a planetary ball mill, with ethanol as the ball milling medium, and the ball milling was performed for 20 hours. The mixture was taken out and dried to obtain a positive electrode active material.
[0026] Select a tap density of 0.8g / cm 3 , specific surface area 6m 2 / g, D50 at 6μm, and hard carbon with gram capacity of 300mAh / g as the negative electrode material.
[0027] Example 1: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.5:1, 94.65% by mass of positive electrode active material, 1% polyacrylonitrile, 1.75% SP, 1.8% polyvinylidene fluoride (PVDF), and 0.8% carbon nanotubes (CNTs) were added with 50% of solid volume of N-methylpyrrolidone solvent and mixed evenly to make positive electrode slurry, and the positive electrode slurry was coated on 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it was rolled into a positive electrode sheet with a thickness of 0.120mm.
[0028] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1.8% of CMC and 1.2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0029] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive aluminum tabs are folded inward, ultrasonically welded first, and then laser welded on the cap. The negative nickel tab is folded inward and resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive pressure-negative pressure cycles. Finally, it is placed at a high temperature of 45°C for 48 hours to form a capacity, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO4 6%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 0.6%, triallyl phosphate 2.5%, PC30%, EC 30%, and the balance is DMC.
[0030] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3320mAh, an average battery internal resistance of 8.5mΩ, a 10C discharge cycle life of more than 2000 times, a room temperature capacity retention rate of 90%, and a capacity retention rate of 85% at 45 degrees Celsius.
[0031] Example 2: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.0:0.8, 94.5% by mass of positive electrode active material, 1% polyacrylonitrile, 2% SP, 1.5% polyvinylidene fluoride (PVDF), and 1.0% carbon nanotubes (CNTs), are added with N-methylpyrrolidone solvent accounting for about 50% of the solid volume and mixed evenly to make positive electrode slurry, and the positive electrode slurry is coated on a 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at a temperature of 80°C, it is rolled into a positive electrode sheet with a thickness of 0.12mm.
[0032] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1.4% of CMC and 1.6% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0033] like Figure 1-3Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 A composite film of a TiO3 ceramic layer, wherein the ceramic layer faces the positive electrode. The two positive electrode tabs are folded inward, first ultrasonically welded, and then laser welded to the cap. The negative electrode tab is folded inward and then resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive-negative pressure cycles. Finally, it is placed at a high temperature of 45°C for 48 hours to form a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 0.5%, triallyl phosphate 1.5%, PC30%, EC 30%, and the balance is DMC.
[0034] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3320mAh, an average battery internal resistance of 8.3mΩ, a 10C discharge cycle life of more than 2000 times, a capacity retention rate of 89%, and a capacity retention rate of 83% at 45 degrees Celsius.
[0035] Example 3: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.2:0.6, 95.5% by mass of positive electrode active material, 1% polyacrylonitrile, 2% SP, 1.5% polyvinylidene fluoride (PVDF), add about 50% of the solid volume of N-methylpyrrolidone solvent and mix evenly to make positive electrode slurry, coat the positive electrode slurry on 15μm thick metal aluminum foil with a coating thickness of 180μm, dry at 80°C, and roll it into a positive electrode sheet with a thickness of 0.12mm.
[0036] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1% of CMC, and 2% of SBR to make the solid content reach 45%, mix them evenly, and make negative electrode slurry. Coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0037] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive pole ears are folded inward, first ultrasonically welded, and then laser welded on the cap. After the negative pole ear is folded inward, it is resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive pressure-negative pressure cycles. Finally, it is placed at a high temperature of 45°C for 48 hours and then the components are divided into capacities, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 1.5%, triallyl phosphate 4%, PC30%, EC30%, and the balance is DMC.
[0038] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3320mAh, an average battery internal resistance of 9.1mΩ, a 10C discharge cycle life of more than 2000 times, a capacity retention rate of 86.9%, and a capacity retention rate of 82.1% at 45 degrees Celsius.
[0039] Example 4: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5TiO3=100:1.8:1, 95% by mass of positive electrode active material, 1% polyacrylonitrile, 1.5% SP, 1.5% polyvinylidene fluoride (PVDF), and 1% carbon nanotubes (CNTs) are added with N-methylpyrrolidone solvent accounting for about 50% of the solid volume and mixed evenly to make positive electrode slurry, and the positive electrode slurry is coated on a 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at a temperature of 80°C, it is rolled into a positive electrode sheet with a thickness of 0.12mm.
[0040] Add appropriate amount of deionized water to 95.5% by mass of hard carbon, 1.5% of SP, 1.8% of CMC and 1.2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0041] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive pole ears are folded inward, first ultrasonically welded, and then laser welded on the cap. After the negative pole ear is folded inward, it is resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive pressure-negative pressure cycles. Finally, it is placed at a high temperature of 45°C for 48 hours and then the components are divided into capacities, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 0.6%, triallyl phosphate 3%, PC30%, EC30%, and the balance is DMC.
[0042] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3360mAh, an average battery internal resistance of 10mΩ, a 10C discharge cycle life of more than 2000 times, a capacity retention rate of 87.2%, and a capacity retention rate of 78.2% at 45 degrees Celsius.
[0043] Example 5: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.0:0.5, 94.5% by mass of positive electrode active material, 1% polyacrylonitrile, 1.5% SP, 2% polyvinylidene fluoride (PVDF), and 1% carbon nanotubes (CNTs), are added with N-methylpyrrolidone solvent accounting for about 50% of the solid volume and mixed evenly to make positive electrode slurry, and the positive electrode slurry is coated on a 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at a temperature of 80°C, it is rolled into a positive electrode sheet with a thickness of 0.12mm.
[0044] Add appropriate amount of deionized water to 95.5% by mass of hard carbon, 1.5% of SP, 1.4% of CMC and 1.6% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0045] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive pole ears are folded inward, first ultrasonically welded, and then laser welded on the cap. After the negative pole ear is folded inward, it is resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive pressure-negative pressure cycles. Finally, it is placed at a high temperature of 45°C for 48 hours to form a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 1%, triallyl phosphate 2.5%, PC30%, EC30%, and the balance is DMC.
[0046] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3320mAh, an average battery internal resistance of 9.4mΩ, a 20A discharge cycle life of more than 2000 times, a capacity retention rate of 85.9%, and a capacity retention rate of 81.1% at 45 degrees Celsius.
[0047] Example 6: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100: 2.5:0.5, 94.4% by mass of positive electrode active material, 1% polyacrylonitrile, 2% SP, 1.8% polyvinylidene fluoride (PVDF), and 0.8% carbon nanotubes (CNTs) are added with N-methylpyrrolidone solvent accounting for about 50% of the solid volume and mixed evenly to make positive electrode slurry, and the positive electrode slurry is coated on a 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it is rolled into a positive electrode sheet with a thickness of 0.12mm.
[0048] Add appropriate amount of deionized water to 95.5% by mass of hard carbon, 1.5% of SP, 1% of CMC and 2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0049] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5A composite film of a TiO3 ceramic layer, wherein the ceramic layer faces the positive electrode. The two positive electrode tabs are folded inward, first ultrasonically welded, and then laser welded on the cap. After the negative electrode tab is folded inward, it is resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive-negative pressure cycles. Finally, it is placed at a high temperature of 45°C for 48 hours to form a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 0.6%, triallyl phosphate 2.5%, PC30%, EC 30%, and the balance is DMC.
[0050] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3300mAh, an average battery internal resistance of 8.7mΩ, a 10C discharge cycle life of more than 2000 times, a capacity retention rate of 87.2%, and a capacity retention rate of 82.5% at 45 degrees Celsius.
[0051] Example 7: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:1.8:0.5, 94.95% by mass of positive electrode active material, 1% polyacrylonitrile, 1.75% SP, 1.8% polyvinylidene fluoride (PVDF), and 0.5% carbon nanotubes (CNTs), added with N-methylpyrrolidone solvent accounting for about 50% of the solid volume and mixed evenly to make positive electrode slurry, and the positive electrode slurry was coated on a 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it was rolled into a positive electrode sheet with a thickness of 0.12mm.
[0052] Add appropriate amount of deionized water to 95.25% by mass of hard carbon, 1.75% of SP, 1.4% of CMC and 1.6% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0053] like Figure 1-3Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 A composite film of a TiO3 ceramic layer, wherein the ceramic layer faces the positive electrode. The two positive electrode tabs are folded inward, first ultrasonically welded, and then laser welded on the cap. After the negative electrode tab is folded inward, it is resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive-negative pressure cycles. Finally, it is placed at a high temperature of 45°C for 48 hours to form a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 0.6%, triallyl phosphate 2.5%, PC30%, EC 30%, and the balance is DMC.
[0054] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3350mAh, an average battery internal resistance of 10.2mΩ, a 10C discharge cycle life of more than 2000 times, a capacity retention rate of 86.2%, and a capacity retention rate of 80.2% at 45 degrees Celsius.
[0055] Example 8: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.2:1.0, 94.25% by mass of positive electrode active material, 1% polyacrylonitrile, 1.75% SP, 2% polyvinylidene fluoride (PVDF), and 1% carbon nanotubes (CNTs), are added with N-methylpyrrolidone solvent accounting for about 50% of the solid volume and mixed evenly to make positive electrode slurry, and the positive electrode slurry is coated on a 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at a temperature of 80°C, it is rolled into a positive electrode sheet with a thickness of 0.12mm.
[0056] Add appropriate amount of deionized water to 95.25% by mass of hard carbon, 2% of SP, 1.75% of CMC, 1% of SBR, and 2% of PAA to make the solid content reach 45%, mix them evenly, and make negative electrode slurry. Coat the negative electrode slurry on a 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0057] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 A composite film of a TiO3 ceramic layer, wherein the ceramic layer faces the positive electrode. The two positive electrode tabs are folded inward, first ultrasonically welded, and then laser welded to the cap. After the negative electrode tab is folded inward, it is resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive-negative pressure cycles. Finally, it is placed at a high temperature of 45°C for 48 hours to form a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 0.5%, triallyl phosphate 3.0%, PC30%, EC 30%, and the balance is DMC.
[0058] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3350mAh, an average battery internal resistance of 9.7mΩ, a 10C discharge cycle life of more than 2000 times, a capacity retention rate of 86.2%, and a capacity retention rate of 80.6% at 45 degrees Celsius.
[0059] Comparative Example 1: Uncoated NaNi 0.33 Mn 0.33 Fe 0.33O2 is used as the positive electrode active material, and 95.65% by mass of the positive electrode active material, 1.75% of SP, 1.8% of polyvinylidene fluoride (PVDF), and 0.8% of carbon nanotubes (CNTs) are added with 50% of the solid volume of N-methylpyrrolidone solvent and mixed evenly to make a positive electrode slurry. The positive electrode slurry is coated on a 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it is rolled into a positive electrode sheet with a thickness of 0.120mm.
[0060] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1.8% of CMC and 1.2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0061] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive electrode tabs are folded inward, ultrasonically welded first, and then laser welded on the cap. The negative electrode tab is folded inward and resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive-negative pressure cycles. Finally, it is placed at high temperature of 45°C for 48 hours to form the components, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, PC30%, EC 30%, and the balance is DMC.
[0062] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3315mAh, an average battery internal resistance of 9.2mΩ, a 10C discharge cycle life of more than 2000 times, a room temperature capacity retention rate of 83%, and a 45 degrees Celsius capacity retention rate of 78%.
[0063] Comparative Example 2: NaNi 0.33 Mn 0.33 Fe 0.33O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.5:1, 95.65% by mass of positive electrode active material, 1.75% of SP, 1.8% of polyvinylidene fluoride (PVDF), and 0.8% of carbon nanotubes (CNTs) were added with 50% of solid volume of N-methylpyrrolidone solvent and mixed evenly to make positive electrode slurry, which was coated on 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it was rolled into a positive electrode sheet with a thickness of 0.120mm.
[0064] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1.8% of CMC and 1.2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0065] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive pole ears are folded inward, first ultrasonically welded, and then laser welded on the cap. The negative pole ear is folded inward and resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive-negative pressure cycles. Finally, it is placed at high temperature of 45°C for 48 hours to form the components, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF65%, NaClO46%, PC30%, EC 30%, and the balance is DMC.
[0066] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3310mAh, an average battery internal resistance of 8.4mΩ, a 10C discharge cycle life of more than 2000 times, a room temperature capacity retention rate of 86%, and a capacity retention rate of 75% at 45 degrees Celsius.
[0067] Comparative Example 3: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.5:1, 94.65% by mass of positive electrode active material, 1% polyacrylonitrile, 1.75% SP, 1.8% polyvinylidene fluoride (PVDF), and 0.8% carbon nanotubes (CNTs) were added with 50% of solid volume of N-methylpyrrolidone solvent and mixed evenly to make positive electrode slurry, and the positive electrode slurry was coated on 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it was rolled into a positive electrode sheet with a thickness of 0.120mm.
[0068] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1.8% of CMC and 1.2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0069] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive electrode tabs are folded inward, ultrasonically welded first, and then laser welded on the cap. The negative electrode tab is folded inward and resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive-negative pressure cycles. Finally, it is placed at high temperature of 45°C for 48 hours to form the components, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, PC30%, EC 30%, and the balance is DMC.
[0070] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3315mAh, an average battery internal resistance of 8.6mΩ, a 10C discharge cycle life of more than 2000 times, a room temperature capacity retention rate of 88%, and a 45 degrees Celsius capacity retention rate of 76%.
[0071] Comparative Example 4: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.5:1, 95.65% by mass of positive electrode active material, 1.75% of SP, 1.8% of polyvinylidene fluoride (PVDF), and 0.8% of carbon nanotubes (CNTs) were added with 50% of solid volume of N-methylpyrrolidone solvent and mixed evenly to make positive electrode slurry, which was coated on 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it was rolled into a positive electrode sheet with a thickness of 0.120mm.
[0072] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1.8% of CMC and 1.2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0073] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode sheet. The two positive electrode tabs are folded inward, ultrasonically welded first, and then laser welded on the cap. The negative electrode tab is folded inward and resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive pressure-negative pressure cycles. Finally, it is placed at high temperature of 45°C for 48 hours to form the components, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 0.6%, triallyl phosphate 2.5%, PC30%, EC 30%, and the balance is DMC.
[0074] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3320mAh, an average battery internal resistance of 8.4mΩ, a 10C discharge cycle life of more than 2000 times, a room temperature capacity retention rate of 86%, and a capacity retention rate of 82% at 45 degrees Celsius.
[0075] Comparative Example 5: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.5:1, 94.65% by mass of positive electrode active material, 1% polyacrylonitrile, 1.75% SP, 1.8% polyvinylidene fluoride (PVDF), and 0.8% carbon nanotubes (CNTs) were added with 50% of solid volume of N-methylpyrrolidone solvent and mixed evenly to make positive electrode slurry, and the positive electrode slurry was coated on 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it was rolled into a positive electrode sheet with a thickness of 0.120mm.
[0076] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1.8% of CMC and 1.2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0077] like Figure 1-3Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive electrode tabs are folded inward, first ultrasonically welded, and then laser welded on the cap. The negative electrode tab is folded inward and then resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive pressure-negative pressure cycles. Finally, it is placed at high temperature of 45°C for 48 hours to form the components, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphorate 0.6%, PC30%, EC 30%, and the balance is DMC.
[0078] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3315mAh, an average battery internal resistance of 8.6mΩ, a 10C discharge cycle life of more than 2000 times, a room temperature capacity retention rate of 89%, and a 45 degrees Celsius capacity retention rate of 78%.
[0079] Comparative Example 6: NaNi 0.33 Mn 0.33 Fe 0.33 O2:Na3ZnB5O 10 :Na 0.5 Bi 0.5 TiO3=100:2.5:1, 94.65% by mass of positive electrode active material, 1% polyacrylonitrile, 1.75% SP, 1.8% polyvinylidene fluoride (PVDF), and 0.8% carbon nanotubes (CNTs) were added with 50% of solid volume of N-methylpyrrolidone solvent and mixed evenly to make positive electrode slurry, and the positive electrode slurry was coated on 15μm thick metal aluminum foil with a coating thickness of 180μm. After drying at 80°C, it was rolled into a positive electrode sheet with a thickness of 0.120mm.
[0080] Add appropriate amount of deionized water to 95% by mass of hard carbon, 2% of SP, 1.8% of CMC and 1.2% of SBR to make the solid content reach 45%, mix them evenly to make negative electrode slurry, coat the negative electrode slurry on 15μm thick metal aluminum foil, dry it at 80°C, coat it with a thickness of 160μm, and roll it into a negative electrode sheet with a thickness of 0.150mm.
[0081] like Figure 1-3 Two gap areas are reserved at 1 / 3 and 2 / 3 of the length of the positive electrode sheet. The aluminum ear is welded in the center at this position with a width of 4mm and covered with rubber. The width of the rubber is 11mm. The length of the negative electrode is 75cm. Two nickel ears are welded at both ends of the negative electrode. The width is 4mm and covered with rubber. The width of the rubber is 11mm. Welding two or more ears helps to improve the current density overload. The positive and negative electrode sheets are stacked and wound into a cylindrical electrode group. The aluminum ear on the positive electrode sheet and the nickel ear on the negative electrode sheet are in the same radial direction of the cylindrical electrode group. The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The diaphragm used is a single-sided Na coated diaphragm with a thickness of 13μm. 0.5 Bi 0.5 The composite film of TiO3 ceramic layer, the ceramic layer faces the positive electrode. The two positive pole ears are folded inward, first ultrasonically welded, and then laser welded on the cap. The negative pole ear is folded inward and resistance welded to the bottom of the steel shell. After the electrolyte is injected, it is sealed after several rounds of positive pressure-negative pressure cycles. Finally, it is placed at high temperature of 45°C for 48 hours and then divided into components, that is, assembled into a 26700 battery. The mass percentage of each component in the electrolyte is NaPF6 5%, NaClO46%, triallyl phosphate 2.5%, PC30%, EC 30%, and the balance is DMC.
[0082] Using the above parameters and manufacturing process, the cylindrical steel shell battery has a shell diameter of 26mm, a height of 70mm, a capacity of 3325mAh, an average battery internal resistance of 8.6mΩ, a 10C discharge cycle life of more than 2000 times, a room temperature capacity retention rate of 89%, and a capacity retention rate of 82% at 45 degrees Celsius.
[0083] It can be seen from the experimental data that Na3ZnB5O 10 and Na 0.5 Bi 0.5TiO3 coating of positive electrode materials can effectively reduce internal resistance, while polyacrylonitrile coating can improve capacity retention rate at room temperature, but both of them do not improve the capacity retention rate of the battery at high temperature. When polyacrylonitrile is coated, after adding di[2-(trimethylsilyl)ethyl]diisopropylaminophosphoryl ester and triallyl phosphate to the electrolyte at the same time, the high temperature performance is significantly improved. According to experimental data, it can be determined that polyacrylonitrile, di[2-(trimethylsilyl)ethyl]diisopropylaminophosphoryl ester and triallyl phosphate work together to improve the cycle performance at high temperature.
[0084] Although the present invention has been described in detail through the above preferred embodiments, it should be appreciated that the above description should not be considered as limiting the present invention.
Claims
1. A cylindrical sodium ion battery, comprising an electrode assembly, an electrolyte and a cylindrical battery housing, characterized in that: The battery electrode group is a wound electrode assembly, which includes an inner layer diaphragm, a negative electrode sheet, a middle diaphragm and a positive electrode sheet, and the positive electrode sheet includes sodium zinc borate Na3ZnB5O 10 and sodium bismuth titanate Na 0.5 Bi 0.5 TiO3 composite coated sodium nickel iron manganese oxide layered oxide and polyacrylonitrile, wherein the mass ratio of sodium nickel iron manganese oxide layered oxide: sodium zinc borate: sodium bismuth titanate is 100:1.8-2.5:0.5-1, the electrolyte contains additives di[2-(trimethylsilyl)ethyl]diisopropylaminophosphoric acid ester and triallyl phosphate, and the mass percentage of sodium salt is 10-12% based on the total mass of the electrolyte; the mass percentage of organic solvent is 83-88% based on the total mass of the electrolyte; the mass percentage of di[2-(trimethylsilyl)ethyl]diisopropylaminophosphoric acid ester is 0.5-1%, and the mass percentage of triallyl phosphate is 1.5-4% based on the total mass of the electrolyte.
2. A cylindrical sodium ion battery according to claim 1, characterized in that: The outer layer of the inner diaphragm is wound around the negative electrode sheet, the outer layer of the negative electrode sheet is wound around the middle diaphragm, and the outer layer of the middle diaphragm is wound around the positive electrode sheet. The inner diaphragm and the middle diaphragm are microporous composite films with a single-sided sodium bismuth titanate ceramic layer, and the thickness of the inner diaphragm and the middle diaphragm is 9-16 μm. The ceramic layer faces the positive electrode sheet; the positive electrode sheet is aluminum foil, and a positive electrode blank section is left at the middle 1 / 3 and 2 / 3 of the positive electrode sheet, and the remaining position is coated with positive electrode slurry. The positive electrode blank section is welded to the positive electrode inner, The outer pole ears, the inner and outer pole ears of the positive electrode are glued with high-temperature tape, the negative electrode sheet is copper foil or aluminum foil, the negative electrode sheet has negative electrode blank sections at the front and rear ends, and the negative electrode slurry is coated in the middle, the negative electrode inner and outer pole ears are welded on the negative electrode blank sections at the front and rear ends of the negative electrode sheet, and the negative electrode inner and outer pole ears are glued with high-temperature tape, wherein the width of the positive electrode inner and outer pole ears and the negative electrode inner and outer pole ears is 4mm, and the width of the high-temperature tape glued on the positive electrode inner and outer pole ears and the negative electrode inner and outer pole ears is 11mm.
3. A cylindrical sodium ion battery according to claim 1 or 2, characterized in that: The positive electrode sheet is prepared by the following method: sodium zinc borate Na3ZnB5O 10 and sodium bismuth titanate Na 0.5 Bi 0.5 TiO3 and sodium nickel iron manganese oxide layered oxide are mixed, placed in a ball mill, ethanol is used as a ball milling medium, and ball milled for 16-30 hours. The mixture is taken out and dried. Then the layered oxide material, polyacrylonitrile and conductive agent are placed in an N-methylpyrrolidone solution containing a binder, and a positive electrode slurry is formed by stirring and mixing, which is then coated on an aluminum foil.
4. A cylindrical sodium ion battery according to claim 1 or 2, characterized in that: The preparation of the negative electrode sheet is as follows: hard carbon and a conductive agent are placed in a deionized water solution containing a binder, and the mixture is stirred to form a negative electrode slurry, which is then coated on a copper foil.
5. A cylindrical sodium ion battery according to claim 3, characterized in that: The mass ratio of the positive electrode slurry: the layered oxide material: polyacrylonitrile: conductive agent: binder = (90-97): (1-2): (1-8): (1-8).
6. A cylindrical sodium ion battery according to claim 4, characterized in that: The mass ratio of the negative electrode slurry: hard carbon: conductive agent: binder = (90-96): (1-6): (1-6).
7. A cylindrical sodium ion battery according to claim 5 or 6, characterized in that: The conductive agent is one or more of SuperP, conductive graphite, Ketjen black, and carbon nanotubes, and the binder is one or more of polyvinylidene fluoride, styrene butadiene rubber SBR, and PAA.
8. A cylindrical sodium ion battery according to claim 1 or 2, characterized in that: The electrolyte is prepared by dissolving NaPF6 and NaClO4 sodium salts in an organic carbonate solvent.