Titanium alloy air bottle manufacturing method
Through roller hot spinning molding and optimized process parameters, combined with heat treatment and surface treatment, the problems of difficulty in machining and complex quality control in the manufacturing process of titanium alloy air bottles have been solved, and the structural accuracy and safety performance of the air bottles have been improved.
Patent Information
- Application Number
- CN202410784615.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-18
- Publication Date
- 2024-10-01
- Estimated Expiration
- 2044-06-18
AI Technical Summary
In the manufacturing process of titanium alloy air bottles, there are limitations such as difficulty in machining, low blank utilization rate, long production cycle, high manufacturing cost, easy defects in welds, and the suitability of spinning method for small-diameter bottles, resulting in complex quality control and safety performance. Potential hazards.
Using roller hot spinning technology, the spinning temperature is 930-960℃, and the molding passes are 14-15 times. It combines heat treatment, surface shot peening and fine processing to ensure the pressure-bearing capacity and structure of the head part. Precision, using titanium alloy and copper materials, and improving quality through ultrasonic flaw detection and hydrostatic testing.
It improves the pressure-bearing capacity of the air bottle head and the fatigue life of the air bottle, improves the structural dimensional accuracy and material mechanical properties, and ensures the safety and reliability of the air bottle.
Smart Images

Figure CN118357688B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of high-pressure air bottles, and in particular to a method for manufacturing a titanium alloy air bottle. Background Art
[0002] At present, with the rapid development of aviation, aerospace, navigation and other fields, the performance requirements for air bottles are becoming increasingly stringent, especially in terms of weight, strength and toughness. In this context, titanium alloys have gradually emerged as an ideal material for the manufacture of new generation air bottles with their excellent properties such as high strength, high elastic modulus, low density and high temperature resistance.
[0003] However, the current manufacturing process of titanium alloy air bottles still faces many challenges. Traditional manufacturing methods usually involve rough machining to form the cylinder and the head, followed by precision machining, and finally assembly through electron beam welding technology. This method is not only difficult to machine, resulting in low blank utilization, but also has a long production cycle and high manufacturing costs. More importantly, due to the presence of multiple welds, defects are easily formed at these welds, making quality control particularly complex and difficult. In addition, this method is generally only applicable to the manufacture of small-caliber titanium alloy air bottles. On the other hand, if you try to apply the traditional spinning method to the forming process of titanium alloy air bottles, although it seems feasible, it is often easy to have chrysanthemums and wrinkles at the head, which undoubtedly brings potential risks to the safety performance of the air bottle.
[0004] Therefore, the manufacturing process of titanium alloy air cylinders still needs further exploration and optimization to find suitable processing technology and process parameters to meet the growing performance requirements and market expectations. Summary of the invention
[0005] The object of the present invention is to provide a method for manufacturing a titanium alloy air bottle that can solve the above-mentioned problems.
[0006] In order to achieve the above object, the present invention provides a method for manufacturing a titanium alloy air bottle, comprising the following steps:
[0007] S1 Raw material inspection: Check whether the raw materials of titanium alloy pipes meet the manufacturing requirements;
[0008] S2 hot spinning: The tube is spin-formed by roller hot spinning to obtain the air bottle body; wherein the spinning temperature is 930-960°C, the spindle speed is 27.23rad / s, the mold speed is 0.0025rad / s, the forming passes are 14-15 times, and the roller feed amount of each pass is evenly distributed;
[0009] S3 preliminary processing: sawing the bottle mouth, rough drilling, rough turning the bottle shoulder, and rough grinding the bottle shoulder of the bottle body in step S2;
[0010] S4 Preliminary Inspection: Measure the thickness of the bottle shoulder to see if it meets the requirements, and check whether there are cracks or defects in the bottle body through penetration test;
[0011] S5 heat treatment: heat treatment to adjust the structure and properties of the bottle body titanium alloy;
[0012] S6 secondary processing: polishing the outer surface of the bottle body, and sandblasting or painting the inner surface of the bottle body;
[0013] S7 Secondary Inspection: Perform ultrasonic flaw detection and penetration inspection on the bottle body;
[0014] S8 three-stage processing: surface treatment of the bottle body; fine processing of the bottle mouth part of the bottle body, including thread processing; cleaning the inner surface of the bottle body to remove impurities or residues;
[0015] S9 three tests: measuring the wall thickness of the bottle; conducting a water pressure test on the bottle; conducting nondestructive testing on the bottle using ultrasonic detection; and measuring the volume and weight of the bottle;
[0016] S10 fourth processing: grinding, cleaning and drying the inner surface of the bottle body;
[0017] S11 Finished product inspection: weld a plug at one end of the bottle body, and assemble a terminal, an air guide tube and a sealing gasket at the other end of the bottle body to obtain a titanium alloy air bottle.
[0018] Furthermore, in the step S2, the spinning temperature is 950°C, and the number of forming passes is 15; under the above conditions, the quality of the manufactured air bottle is better.
[0019] Furthermore, eight fixed torches and two manual welding torches are arranged above the pipe for supplementary heating, so that the temperature can be kept stable during the spinning process.
[0020] Furthermore, in step S5, the heat treatment adopts a trolley-type resistance heating furnace with a system of 930°C~935°C / 1h.AC, a charging temperature less than or equal to 500°C, and natural gas is heated to 910°C to achieve a better heat treatment system and realize a reasonable match between organization and performance.
[0021] Furthermore, in step S8, the surface treatment includes an internal and external shot peening process, and the process uses steel balls with a diameter of 1.8 mm to 2.5 mm. The surface treatment removes the oxide scale on the surface of the air bottle, increases the surface compressive stress to improve the fatigue resistance of the air bottle, and the surface of the treated air bottle is clean, free of oxide scale and residual steel shots, and local smooth depressions are allowed.
[0022] Furthermore, the shot peening coverage is greater than or equal to 90%; and ultrasonic flaw detection is performed after the internal and external shot peening is completed.
[0023] Furthermore, the surface treatment also includes alkali pickling of the inner and outer surfaces of the bottle body after the shot peening process is completed to remove the contamination layer.
[0024] Furthermore, in the step S2, before hot spinning, the required shape and size are cut from the titanium alloy tube according to the design requirements of the air bottle, and the tube is preheated to 35° C. for 90 minutes.
[0025] Furthermore, in the step S11, the plug, the end and the air guide tube are made of titanium alloy material, the sealing gasket is made of copper material, and the sealing gasket is annealed.
[0026] Furthermore, the percentage of each component in the titanium alloy pipe is: 4.2%~4.7%Al, 2.4%~2.8%Mo, 1.1%~1.4%V, 0~0.2%Fe, 0~0.05%C, 0~0.05%Si, 0~0.05%Zr, 0~0.03%N, 0~0.008%H and 0~0.105%O, and the balance is Ti, so that the air bottle has better strength, plasticity and toughness and lower yield strength ratio.
[0027] Furthermore, in the ultrasonic flaw detection, the scanning sensitivity is increased by 14 dB on the basis of the reference sensitivity to improve the inspection standard of the bottle body and further improve the quality of the manufactured air bottle.
[0028] Compared with the prior art, the titanium alloy air bottle manufacturing method described in the present invention has the beneficial effect of adopting roller-type hot spinning forming technology, using spinning forming temperature of 930-960°C, and forming passes of 14-15 times as process parameters, small deformation, precise temperature control, improving the pressure bearing capacity of the air bottle head and the fatigue life of the air bottle, and effectively improving the structural dimensional accuracy and material mechanical properties of the air bottle body and head. BRIEF DESCRIPTION OF THE DRAWINGS
[0029] Figure 1 is a flow chart of a method for manufacturing a titanium alloy air bottle in an embodiment of the present invention;
[0030] Figure 2 It is a schematic structural diagram of a titanium alloy air bottle manufactured by the titanium alloy air bottle manufacturing method in an embodiment of the present invention.
[0031] In the figure, 1. bottle body; 2. end cap; 3. plug; 4. air guide tube; 5. sealing gasket; 6. end cap. DETAILED DESCRIPTION
[0032] The specific implementation of the present invention is further described in detail below in conjunction with the accompanying drawings and examples. The following examples are used to illustrate the present invention, but are not intended to limit the scope of the present invention.
[0033] In the description of the present invention, it should be understood that the terms "up", "down", "front", "back", "left", "right", "vertical", "horizontal", "top", "bottom", "inside" and "outside" used in the present invention to indicate the orientation or position relationship are based on the orientation or position relationship shown in the accompanying drawings, and are only for the convenience of describing the present invention and simplifying the description, rather than indicating or implying that the device or element referred to must have a specific orientation, be constructed and operated in a specific orientation, and therefore cannot be understood as a limitation on the present invention.
[0034] In the description of the present invention, it should be understood that the terms "connected", "connected", "fixed" and the like used in the present invention should be understood in a broad sense, for example, it can be a fixed connection, a detachable connection, or an integral connection; it can be a mechanical connection or a welding connection; it can be directly connected or indirectly connected through an intermediate medium, it can be the internal connection of two elements or the interaction relationship between two elements, unless otherwise clearly defined. For ordinary technicians in this field, the specific meanings of the above terms in the present invention can be understood according to specific circumstances.
[0035] The present invention uses the terms "first", "second", etc. to describe various information, but these information should not be limited to these terms, and these terms are only used to distinguish the same type of information from each other. For example, without departing from the scope of the present invention, "first" information may also be referred to as "second" information, and similarly, "second" information may also be referred to as "first" information.
[0036] Reference Figure 1 The method for manufacturing a titanium alloy air bottle according to an embodiment of the present invention comprises the following steps:
[0037] S1 Raw material inspection: Check whether the raw materials of titanium alloy pipes meet the manufacturing requirements.
[0038] S2 hot spinning: The tube is spin-formed by roller hot spinning to obtain the air bottle body; wherein the spinning temperature is 930-960°C, the spindle speed is 27.23rad / s, the mold speed is 0.0025rad / s, the forming passes are 14-15 times, and the roller feed amount of each pass is evenly distributed;
[0039] S3 Preliminary processing: The bottle body is machined by sawing the bottle mouth, rough drilling, rough turning the bottle shoulder, and rough grinding the bottle shoulder to accurately control its size and shape for subsequent more refined processing.
[0040] S4 Preliminary Inspection: Measure the thickness of the bottle shoulder to see if it meets the requirements, and use a penetration test to check if there are any tiny cracks or defects on the bottle body.
[0041] S5 heat treatment: The structure and properties of the titanium alloy of the bottle body are adjusted through heat treatment to improve its strength and corrosion resistance. After heat treatment, the air bottle is subjected to hardness test and performance test to ensure that it meets the design requirements.
[0042] S6 Secondary processing: Polish the outer surface of the bottle and sandblast or paint the inner surface to improve its appearance quality and corrosion resistance.
[0043] S7 Secondary Inspection: Ultrasonic detection and penetration inspection are performed on the bottle body to ensure the quality and integrity of the air bottle.
[0044] S8 three-stage processing: surface treatment of the bottle body, fine processing of the bottle mouth, including thread processing, to ensure the sealing and reliability of the bottle mouth; at the same time, clean the inner surface of the bottle body to remove any impurities or residues. Rough turn the end face and inner and outer diameters of the bottle mouth, and turn the outer arc of the head according to the drawing. In this process, it is necessary to ensure that the bottle mouth thread has sufficient processing allowance and select the appropriate feed amount to prevent problems such as rolling of the arc part.
[0045] S9 three times inspection: measure the wall thickness of the bottle body, conduct water pressure test on the bottle body to check its sealing and pressure resistance; then use ultrasonic flaw detection to perform non-destructive testing on the bottle body, and measure the volume and weight of the bottle body to ensure that it meets the design requirements.
[0046] S10 Four-step processing: Grind the inner surface of the bottle to remove possible burrs or uneven parts, then clean and blow dry to ensure that the inside of the bottle is clean and free of impurities. Specifically, the raised ridges on the shoulder of the bottle are polished with a grinding wheel and penetrant testing is performed according to NB / T47013.
[0047] S11 Finished product inspection: weld a plug at one end of the bottle body, assemble the end cap, air guide tube and gasket at the other end of the bottle body, and conduct a final appearance and performance inspection; conduct a penetration test after welding the plug to check the quality and sealing of the welded plug; conduct an air tightness test on the air bottle after assembly.
[0048] Reference Figure 2 The titanium alloy air bottle manufactured by the method comprises a bottle body 1, an end cap 2, a plug 3, an air guide tube 4, a sealing gasket 5, and a sealing head 6. The bottle body 1 adopts a double-opening structure, and both ends of the bottle mouth have internal threads; the sealing head 6 is a pointed spherical shape. The end cap 2 is connected to one end of the bottle mouth of the bottle body 1 by threads and sealed with a sealing gasket 5. The plug 3 is first connected to the other end of the bottle mouth by threads and then sealed by welding.
[0049] The roller forming method is achieved through multiple extrusion passes, which has the advantages of small deformation and precise temperature control. In the manufacturing process of air bottles, spinning and closing is a key process, which has a direct impact on the overall forming and head quality of the air bottle. The entire spinning process is finely divided into 15 forming passes, and hydraulically driven clamps are used for clamping, with an overhang length of 900mm. The feed amount of each pass is small, which effectively reduces the deformation heat. Compared with the plate structure, the roller mold structure has greatly reduced friction, so the temperature rise caused by friction is relatively small, which makes the temperature control of the entire spinning process better. This method can balance the temperature rise of each pass and ensure that the bottle mouth temperature remains below the phase change temperature (about 960℃) of the titanium alloy pipe.
[0050] The three-coordinate coefficient value control technology is also used in the roller hot spinning process of titanium bottles. The precise six-degree-of-freedom displacement of the roller is controlled by linkage to achieve accurate setting and forming of thick-walled titanium alloy tubes with multiple passes and small deformations. During the forming process, the forming temperature is accurately controlled according to the phase transition point temperature of the titanium alloy, ensuring the forming quality while ensuring the forming size.
[0051] In order to accurately evaluate the temperature rise of titanium alloy tubes during roller forming hot spinning, the hot spinning forming process of the head was simulated using DEFORM-3D thermal analysis software. The following process parameters were set: spinning temperature was 950℃, spindle speed was 27.23rad / s, die speed was 0.0025rad / s, forming passes were 15 times, and the roller feed amount for each pass was evenly divided into 15 times.
[0052] The analysis results of DEFORM-3D show that the roller forming method performs well in temperature control. The maximum temperature of the bottleneck is maintained at around 1000°C. This temperature range is exactly the ideal processing temperature window for the titanium alloy pipe, which verifies the feasibility of the roller forming method.
[0053] In some improved solutions of the present application, in step S2, in order to ensure the temperature stability of the spinning process, eight fixed torches and two manual welding torches are set above the pipe for supplementary heating during the spinning process.
[0054] In response to the problems that occurred in the early air bottle spinning, this application also made the following improvements to the spinning equipment: 1) An advanced spinning forming CNC program was designed to ensure that the air bottle structure can be accurately manufactured according to the design drawings; 2) It was equipped with a complete heating control system, combining a medium frequency furnace and natural gas to heat the bottle body 1, and a high-precision temperature sensor was configured to achieve heating accuracy within ±10°C; 8 heat replenishment guns were installed on the spinning machine to replenish air as needed during the spinning process; 3) The matching between the equipment clamping cylinder and the bottle body 1 was improved, and a special conveying tooling was designed to ensure that the air bottle can be directly clamped during the transportation process from taking out of the furnace to clamping, without adding a transition pipe, effectively avoiding the problem of slipping of the bottle body 1 when rolling; 4) The equipment rigidity of the spinning machine was improved to provide sufficient deformation force.
[0055] In some improved solutions of the present application, the heat treatment in step S5 adopts a trolley-type resistance heating furnace, the system is 930℃~935℃ / 1h.AC, the charging temperature is less than or equal to 500℃, and the natural gas is heated to 910℃. At the same time, in order to ensure the external dimensions after heat treatment, the air bottle must be placed stably during the heat treatment process and when it is taken out of the furnace, and it is placed on a flat plate and is not allowed to contact with sharp objects.
[0056] In some improved schemes of the present application, in step S8, the surface treatment includes internal and external shot peening processes, which use steel balls with a diameter of 1.8mm to 2.5mm after being screened by a sand screening machine; when spraying internally, stir the spray gun to ensure that the inner surface of the air bottle can be completely covered. For the simplified part of the air bottle, it is sufficient to cover it, and the arc surface of the air bottle is treated with emphasis. The surface oxide scale of the air bottle is removed by surface treatment, and the surface compressive stress is increased to improve the fatigue resistance of the air bottle. The surface of the treated air bottle is clean, free of oxide scale and residual steel balls, and local smooth depressions are allowed.
[0057] In some improved schemes of the present application, dust or dirt is cleaned with a pneumatic tool before the shot peening machine is used; the air bottle shot peening coverage is greater than or equal to 90%; and ultrasonic flaw detection is performed after the internal and external shot peening is completed.
[0058] In some improved solutions of the present application, the surface treatment further includes alkaline pickling, and after the shot peening process is completed, the inner and outer surfaces of the bottle body 1 are subjected to alkaline pickling to remove the contamination layer.
[0059] In some improved solutions of the present application, in step S2, before hot spinning, the required shape and size are cut from the titanium alloy tube according to the design requirements of the air bottle, and the tube is preheated to 35°C for 90 minutes. During the heating process, it is confirmed again that the tool, the length of the stop block, and the distance between the stop plate of the feed cylinder and the end face of the spindle are correct.
[0060] In some improved solutions of the present application, the step S1 specifically includes:
[0061] S1-1 Material Re-testing: Re-testing titanium alloy raw materials through chemical composition analysis and physical property testing is an important step to ensure that the titanium alloy raw materials used meet production standards and quality requirements.
[0062] S1-2 Material inspection: Check whether the pipe has defects to further confirm the quality and performance of the material and ensure that there are no parts that do not meet the requirements.
[0063] S1-3 Material Ultrasonic Testing: Use ultrasonic flaw detection technology to test titanium alloy pipes to detect whether there are cracks or pores inside the pipes to ensure the integrity of the materials.
[0064] In some improved solutions of the present application, in step S11, the plug 3, the end 2 and the air guide tube 4 of the air bottle are made of titanium alloy material, and the sealing gasket 5 is made of copper material, wherein the sealing gasket 5 is annealed.
[0065] Since the use environment of air bottles is usually relatively harsh, they need to have good comprehensive performance matching such as strength, plasticity, and toughness. At the same time, they also require a relatively low yield strength to improve the safety reserve of air bottles. In some improvement schemes of this application, the percentage of each component in the titanium alloy pipe is: 4.2%~4.7%Al, 2.4%~2.8%Mo, 1.1%~1.4%V, 0~0.2%Fe, 0~0.05%C, 0~0.05%Si, 0~0.05%Zr, 0~0.03%N, 0~0.008%H and 0~0.105%O, and the balance is Ti. By optimizing the alloy composition of the material, strictly controlling the impurity composition, smelting and forging quality, formulating a reasonable heat treatment system, and strictly controlling the process temperature, the reasonable matching optimization of the strength and toughness of the pipe is achieved, the comprehensive performance of the pipe is improved, and the pressure bearing and fatigue life requirements of the air bottle are met.
[0066] In some improvement schemes of the present application, in ultrasonic flaw detection, referring to NB / T 47013.3-2015 "Nondestructive Testing of Pressure Equipment Part 3: Ultrasonic Testing", an artificial reflector of Class I size is used to calibrate the equipment sensitivity, and the echo height is adjusted to 80% of the full scale as the benchmark sensitivity, and the scanning sensitivity is increased by 14dB on the basis of the benchmark sensitivity.
[0067] The roller hot spinning forming in this application relies on roller extrusion to complete the forming, and requires multiple passes to form step by step. Through calculation and analogy, the heating temperature changes from 900℃-980℃, and the forming passes are changed from 12 to 16 as variables. The roller feed amount of each pass is evenly distributed, the spindle speed is 27.23rad / s, and the mold speed is 0.0025rad / s. Experimental comparison is carried out. The forming quality data under different forming passes and temperature conditions are shown in Table 1.
[0068] Table 1 Molding quality data under different molding passes and different temperature conditions
[0069]
[0070] (×: unqualified, √: qualified)
[0071] As can be seen from the table above, when the number of passes is 14-15 and the molding temperature is 930℃-960℃, the molding quality is qualified and determined as the molding process parameters. Among them, when the molding number / temperature is 15 passes / 950℃, the inner and outer diameters of the air bottle mouth are qualified, the metal fluidity is the best, the inner wall is flat, there are no obvious wrinkles, and the quality is good; under other conditions, although the quality is qualified, the performance is average. For example, under the conditions of 14 passes / 940℃, the inner and outer diameters of the air bottle mouth are qualified, but the metal fluidity is still insufficient, and there is an "orange peel" phenomenon on the inner surface.
[0072] Therefore, the specific parameters of the hot spin forming method of the present application are set as follows: the spin forming temperature is 950°C, the spindle speed is 27.23rad / s, the mold speed is 0.0025rad / s, the forming passes are 15 times, and the roller feed amount of each pass is evenly distributed.
[0073] In summary, the method for manufacturing a titanium alloy air bottle provided in the embodiment of the present application has the following advantages:
[0074] 1) An innovative titanium alloy air bottle forming process route was proposed, which adopted roller hot spinning forming technology, adopted spinning forming temperature of 930-960℃ and forming passes of 14-15 times, which effectively improved the structural dimensional accuracy and material mechanical properties of the air bottle body and head, enhanced the pressure bearing capacity of the head and the fatigue life of the air bottle.
[0075] 2) Optimize the heat treatment system to achieve a reasonable match between material organization and performance, ensure the excellent and stable performance of the air bottle material, and improve the safety and reliability of the air bottle.
[0076] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and substitutions can be made without departing from the technical principles of the present invention. These improvements and substitutions should also be regarded as the scope of protection of the present invention.
Claims
1. Titanium alloy air bottle manufacturing method, It is characterized in that The following steps are involved: S1 Raw material inspection: Check whether the raw materials of titanium alloy pipes meet the manufacturing requirements; S2 hot spinning: The tube is spin-formed by roller hot spinning to obtain the air bottle body; wherein the spinning temperature is 930-960°C, the spindle speed is 27.23rad / s, the mold speed is 0.0025rad / s, the forming passes are 15 times, and the roller feed amount of each pass is evenly distributed; S3 preliminary processing: sawing the bottle mouth, rough drilling, rough turning the bottle shoulder, and rough grinding the bottle shoulder of the bottle body in step S2; S4 Preliminary inspection: measure whether the thickness of the bottle shoulder meets the requirements, and check whether there are cracks or defects in the bottle body through penetration test; S5 heat treatment: heat treatment to adjust the structure and properties of the bottle body titanium alloy; S6 secondary processing: polishing the outer surface of the bottle body, and sandblasting or painting the inner surface of the bottle body; S7 Secondary Inspection: Perform ultrasonic flaw detection and penetration testing on the bottle body; S8 three-stage processing: surface treatment of the bottle body; fine processing of the bottle mouth part of the bottle body, including thread processing; cleaning the inner surface of the bottle body to remove impurities or residues; S9 three tests: measuring the wall thickness of the bottle body; conducting a water pressure test on the bottle body; conducting an ultrasonic flaw detection on the bottle body; and measuring the volume and weight of the bottle body; S10 fourth processing: grinding, cleaning and drying the inner surface of the bottle body; S11 Finished product inspection: weld a plug at one end of the bottle body, and assemble a terminal, an air guide tube and a sealing gasket at the other end of the bottle body to obtain a titanium alloy air bottle; The percentage of each component in the titanium alloy pipe is: 4.2%~4.7% Al, 2.4%~2.8% Mo, 1.1%~1.4% V, 0~0.2% Fe, 0~0.05% C, 0~0.05% Si, 0~0.05% Zr, 0~0.03% N, 0~0.008% H and 0~0.105% O, and the balance is Ti.
2. The method for manufacturing a titanium alloy air bottle according to claim 1, It is characterized in that The spin forming temperature is 950°C.
3. The method for manufacturing a titanium alloy air bottle according to claim 1, It is characterized in that Eight fixed torches and two manual welding torches are arranged above the pipes for supplementary heating.
4. The method for manufacturing a titanium alloy air bottle according to claim 1, It is characterized in that In S5, the heat treatment adopts a trolley-type resistance heating furnace with a system of 930°C~935°C / 1h.AC, a furnace charge temperature less than or equal to 500°C, and natural gas is heated to 910°C.
5. The method for manufacturing a titanium alloy air bottle according to claim 4, It is characterized in that In S8, the surface treatment includes an internal and external shot peening process, and the process uses steel balls with a diameter of 1.8 mm to 2.5 mm.
6. The method for manufacturing a titanium alloy air bottle according to claim 5, It is characterized in that The shot peening coverage is greater than or equal to 90%; ultrasonic flaw detection is performed after the internal and external shot peening is completed.
7. The method for manufacturing a titanium alloy air bottle according to claim 6, It is characterized in that The surface treatment also includes alkali pickling of the inner and outer surfaces of the bottle body after the shot peening process is completed to remove the contamination layer.
8. The method for manufacturing a titanium alloy air bottle according to claim 1, It is characterized in that In S2, before hot spinning, the required shape and size are cut from the titanium alloy tube according to the design requirements of the air bottle, and the tube is preheated to 35° C. for 90 minutes.
9. The method for manufacturing a titanium alloy air bottle according to claim 1, It is characterized in that In S11, the plug, the end and the air guide tube are made of titanium alloy material, the sealing gasket is made of copper material, and the sealing gasket is annealed.