Antistatic long glass fiber reinforced polypropylene composite material and preparation method thereof

By using maleic anhydride grafted polypropylene and silane coupling agent in long fiber strong polypropylene composite materials, the problem of glass fiber floating fiber and electrostatic leakage is solved, and the smooth molding of the material and excellent anti-static properties are achieved.

CN118359890BActive Publication Date: 2024-11-12SICHUAN LANGDI NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410760838.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-11-12
Estimated Expiration
2044-06-13

AI Technical Summary

Technical Problem

Long fiber strong polypropylene composite materials are prone to glass fiber floating fiber phenomenon and are difficult to leak static electricity, which affects its electrical insulation and application value.

Method used

Maleic anhydride grafted polypropylene and long glass fibers are used for surface pretreatment, combined with silane coupling agent and polyethylene wax, improve adhesion and fluidity, reduce floating fiber phenomenon, and pass glyceryl stearate and carbon black Enhance antistatic properties.

Benefits of technology

It effectively reduces the phenomenon of glass fiber floating fiber, improves the antistatic function and mechanical properties of the material, and ensures the smooth forming of the material and excellent electrical insulation performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

The present invention relates to the technical field of glass fiber reinforced polypropylene composite materials, and specifically discloses an antistatic long glass fiber reinforced polypropylene composite material and a preparation method thereof, comprising the following components by weight: 30-40 parts of maleic anhydride grafted polypropylene I, 20-30 parts of maleic anhydride grafted polypropylene II, 30-50 parts of long glass fibers, 5-8 parts of polyacrylamide, 2-5 parts of glyceryl stearate, 1-2 parts of silane coupling agent, and 2-4 parts of polyethylene wax; wherein the grafting rate of maleic anhydride grafted polypropylene I is 0.8-1.0%, and the melt index is 80-120 g / 10min; the grafting rate of maleic anhydride grafted polypropylene II is 1.2-1.5%, and the melt index is 300-350g / 10min. The present invention can not only effectively reduce the glass fiber floating fiber phenomenon of the long glass fiber reinforced polypropylene composite material, but also the long glass fiber reinforced polypropylene composite material has excellent antistatic function.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of glass fiber reinforced polypropylene composite materials, and in particular to an antistatic long glass fiber reinforced polypropylene composite material and a preparation method thereof. Background Art

[0002] Glass fiber reinforced polypropylene composite materials have the advantages of low density, low cost, low specific gravity, short molding cycle, no chemical reaction during processing, good mechanical properties, and recyclability. They are widely used in high-cutting, high-strength, heat-resistant, water-resistant and chemical-resistant fields, mainly including the automotive industry, electronics industry and aerospace industry.

[0003] According to the different fibers, glass fiber reinforced polypropylene composites can be divided into short fiber strong polypropylene composites, long fiber strong polypropylene composites and continuous fiber strong polypropylene composites. Among them, long fiber strong polypropylene composites have better mechanical properties than short fiber strong polypropylene composites. Therefore, how to produce long fiber strong polypropylene composites with good performance has good market application value.

[0004] Although long fiber strong polypropylene composite materials have good mechanical properties, they are prone to glass fiber floating phenomenon. In addition, although long fiber strong polypropylene composite materials have good electrical insulation and high resistivity, the static electricity accumulated in themselves is difficult to leak, which often turns this advantage into a disadvantage. This requires antistatic modification of long fiber strong polypropylene composite materials. Summary of the invention

[0005] The purpose of the present invention is to provide an antistatic long glass fiber reinforced polypropylene composite material and a preparation method thereof, which can not only effectively reduce the glass fiber floating phenomenon of the long glass fiber reinforced polypropylene composite material, but also the long glass fiber reinforced polypropylene composite material has excellent antistatic function.

[0006] The present invention is achieved through the following technical solutions:

[0007] An antistatic long glass fiber reinforced polypropylene composite material comprises the following components in parts by weight:

[0008] 30-40 parts of maleic anhydride grafted polypropylene I, 20-30 parts of maleic anhydride grafted polypropylene II, 30-50 parts of long glass fiber, 5-8 parts of polyacrylamide, 2-5 parts of glyceryl stearate, 1-2 parts of silane coupling agent, and 2-4 parts of polyethylene wax; wherein the long glass fiber is a fiber subjected to surface pretreatment with a coupling agent, wherein the grafting rate of maleic anhydride grafted polypropylene I is 0.8-1.0%, and the melt index is 80-120 g / 10min; the grafting rate of maleic anhydride grafted polypropylene II is 1.2-1.5%, and the melt index is 300-350g / 10min.

[0009] The floating fiber phenomenon is caused by the exposure of glass fibers. White glass fibers are exposed on the surface during the flow of plastic melt filling the mold. After condensation and molding, radial white marks are formed on the surface of the plastic part. When the plastic part is black, the difference in color will be greater and the marks will be more obvious. The applicant conducted an in-depth analysis of the floating fiber phenomenon and found that:

[0010] One of the main reasons for the floating glass fiber phenomenon is that during the flow of plastic melt, due to the difference in fluidity and mass density between glass fiber and resin, the two tend to separate. The glass fiber with low density floats to the surface, and the resin with high density sinks inside, thus forming the phenomenon of exposed glass fiber.

[0011] Based on the above findings, the applicant considered enhancing the adhesion between the long glass fiber and the resin (commonly used polypropylene), increasing the interfacial bonding strength, and reducing the separation of the long glass fiber and the resin, thereby improving the glass fiber exposure phenomenon. However, increasing the adhesion will lead to an uneven distribution of the long glass fiber content, thereby affecting the mechanical properties of the manufactured product. At the same time, increasing the adhesion will also affect the material molding process, resulting in obstructed molding.

[0012] Therefore, when solving the problem of floating glass fibers, it is necessary not only to consider increasing the adhesion between long glass fibers and resin (commonly used polypropylene), but also to consider the uniformity of long glass fiber distribution and the fluidity of the system during material molding.

[0013] The invention adopts maleic anhydride grafted polypropylene to replace the polypropylene raw material in the existing long glass fiber reinforced polypropylene composite material. Compared with polypropylene, maleic anhydride grafted polypropylene has better bonding effect with long glass fiber, which is beneficial to reducing the floating fiber phenomenon of the long glass fiber reinforced polypropylene composite material.

[0014] In addition, the present invention adopts two kinds of maleic anhydride grafted polypropylenes (maleic anhydride grafted polypropylene I and maleic anhydride grafted polypropylene II) with different grafting rates and melt indexes, wherein the grafting rate and melt index of maleic anhydride grafted polypropylene I are relatively low, while the grafting rate and melt index of maleic anhydride grafted polypropylene II are relatively high. Maleic anhydride grafted polypropylene I and maleic anhydride grafted polypropylene II are used in different processes of preparing electrostatic long glass fiber reinforced polypropylene composite materials, which can reduce the molding process of materials affected by the viscosity problem of maleic anhydride grafted polypropylene under the premise of ensuring that maleic anhydride grafted polypropylene has good adhesion with long glass fibers. Among them, maleic anhydride grafted polypropylene I with relatively low grafting rate and melt index is used in the dispersion and impregnation process of long glass fibers to ensure the adhesion effect between long glass fibers and maleic anhydride grafted polypropylene and reduce floating fibers; maleic anhydride grafted polypropylene II with relatively high grafting rate and melt index is used in the extrusion molding process to ensure fluidity during molding.

[0015] Moreover, in order to further control the fluidity of the molten system during material molding so as to be more appropriate, which will not affect the molding and the bonding effect between the long glass fiber and the maleic anhydride grafted polypropylene, silane coupling agent and polyethylene wax are added to the formula. By adding a certain amount of polyethylene wax to the formula, the fluidity of the molten system during material molding can be increased, and the polyethylene wax and maleic anhydride grafted polypropylene II work together to increase the fluidity of the molten system; by adding a certain amount of silane coupling agent to the formula, the adhesion between the maleic anhydride grafted polypropylene (maleic anhydride grafted polypropylene I and maleic anhydride grafted polypropylene II) and the long glass fiber in the molten system during material molding can be improved to ensure the reduction of the floating fiber effect, that is, through the joint action of maleic anhydride grafted polypropylene I, maleic anhydride grafted polypropylene II, polyethylene wax and silane coupling agent, the fluidity of the molten system during material molding can be controlled within a reasonable range, which can not only achieve smooth molding, but also reduce the floating fiber phenomenon of the product.

[0016] Meanwhile, the long glass fiber of the present invention is a fiber that has been surface pretreated with a coupling agent. The pretreated long glass fiber can better bond with maleic anhydride grafted polypropylene, thereby increasing the interface adhesion between the two.

[0017] Furthermore, in order to improve the uniformity of dispersion of the long glass fibers in the system, the present invention adds a certain amount of polyacrylamide as a dispersant in the formula, so that the long glass fibers can be uniformly dispersed in the maleic anhydride grafted polypropylene I during the impregnation stage, and can be uniformly dispersed in the molten system during the material molding stage.

[0018] Meanwhile, the invention adds a certain amount of glyceryl stearate in the formula, and glyceryl stearate (GMS) is used as an antistatic agent to enable the prepared antistatic long glass fiber reinforced polypropylene composite material to have an antistatic function.

[0019] In summary, the antistatic long glass fiber reinforced polypropylene composite material prepared by the above formula of the present invention can not only effectively reduce the glass fiber floating phenomenon of the long glass fiber reinforced polypropylene composite material, but also the long glass fiber reinforced polypropylene composite material has excellent antistatic function.

[0020] In a preferred embodiment, in order to improve the antistatic effect of the antistatic long glass fiber reinforced polypropylene composite material, the formula also includes the following components in parts by weight:

[0021] 2-3 parts of carbon black.

[0022] Carbon black and glyceryl stearate work together to improve the antistatic effect of antistatic long glass fiber reinforced polypropylene composites from two aspects: glyceryl stearate (GMS) as an antistatic agent gives the prepared antistatic long glass fiber reinforced polypropylene composites antistatic function; carbon black as a conductive material gives the antistatic long glass fiber reinforced polypropylene composites a certain conductivity, thereby improving the antistatic function.

[0023] In a preferred embodiment, in order to improve the corrosion resistance and antioxidant effect of the material, the formula also includes the following components in parts by weight:

[0024] 1-2 parts of antioxidant.

[0025] The antioxidant may specifically be a phenolic antioxidant, for example: 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane.

[0026] By adding a certain amount of antioxidant in the process of preparing antistatic long glass fiber reinforced polypropylene composite materials, the overall antioxidant effect of the material is improved, thereby reducing corrosion caused by oxidation. Therefore, while improving the antioxidant effect of the material, its corrosion resistance is also improved.

[0027] In a preferred embodiment, the silane coupling agent is a liquid silane coupling agent. Specifically, the liquid silane coupling agent is composed of the following components in weight percentage:

[0028] Ethoxysilane 20%, anhydrous ethanol 72%, purified water 8%.

[0029] By adding a certain amount of silane coupling agent to the formula, the bonding effect between maleic anhydride grafted polypropylene (maleic anhydride grafted polypropylene Ⅰ and maleic anhydride grafted polypropylene Ⅱ) and long glass fibers can be increased, and floating fibers can be reduced; when the silane coupling agent is used in the melting system during material molding, the silane coupling agent can help maintain the bonding effect between maleic anhydride grafted polypropylene (maleic anhydride grafted polypropylene Ⅰ and maleic anhydride grafted polypropylene Ⅱ) and long glass fibers, and the dispersion uniformity of the silane coupling agent in the system during the preparation process will affect the effect of increasing the bonding degree between maleic anhydride grafted polypropylene and long glass fibers. If the silane coupling agent is unevenly distributed in the system, it will cause the parts where the silane coupling agent is more concentrated to have too high bonding, while the parts without silane coupling agent have less bonding. Too high bonding has a greater impact on the extrusion molding of the material, while too low bonding will lead to a poor effect of reducing floating fibers.

[0030] The invention adopts liquid silane coupling agent, which is beneficial to the dispersion of the silane coupling agent on the surface of the material, that is, it is beneficial to the uniform distribution of the silane coupling agent in the system.

[0031] In one possible implementation, the long glass fiber is a continuous alkali-free glass fiber, and the diameter of the single fiber is 14-17 μm.

[0032] A method for preparing an antistatic long glass fiber reinforced polypropylene composite material comprises the following steps:

[0033] S1. Pretreatment of long glass fibers: using a coupling agent to pretreat the surface of the long glass fibers;

[0034] S2. Dispersion of long glass fibers: the maleic anhydride grafted polypropylene I and the long glass fibers are uniformly mixed according to a certain proportion, and then heated to a molten state and maintained for 1-3 hours;

[0035] S3, impregnation of long glass fibers: adding the polyacrylamide to the molten system of step S2, mixing and maintaining for 2-10 seconds;

[0036] S4, extrusion molding: the molten system obtained in step S3 is mixed evenly with the maleic anhydride grafted polypropylene II, the stearic acid glyceryl ester, the silane coupling agent and the polyethylene wax, and then put into an extruder for extrusion molding, cooling and pelletizing.

[0037] The preparation method of the present invention can improve the bonding effect between the long glass fiber and the maleic anhydride grafted polypropylene I by pretreating, dispersing and impregnating the long glass fiber in sequence before extrusion molding, and improve the dispersion effect and maintenance of the bonding effect of the long glass fiber in the melting system during extrusion molding, thereby ensuring the smooth progress of the extrusion molding, while maintaining the bonding effect between the long glass fiber and the maleic anhydride grafted polypropylene, and ensuring that the prepared antistatic long glass fiber reinforced polypropylene composite material can reduce the glass fiber floating phenomenon as much as possible.

[0038] Furthermore, in step S1, the specific process of preprocessing is:

[0039] S11, cleaning and drying the long glass fibers;

[0040] S12, soaking the long glass fiber treated in step S11 in a 10%-15% potassium permanganate solution under ultrasonic vibration for 30-60 minutes;

[0041] S13. Under ultrasonic vibration conditions, immerse the long glass fiber treated in step S12 in a silane coupling agent solution for 30-60 minutes.

[0042] The surface modification effect of the long glass fiber can be improved by first soaking in a potassium permanganate solution and then soaking in a silane coupling agent solution, and the soaking process is carried out under ultrasonic vibration conditions, which can further improve the surface modification effect of the long glass fiber.

[0043] Further, the silane coupling agent solution is composed of the following components in weight percentage:

[0044] Ethoxysilane 25%, anhydrous ethanol 69%, purified water 6%.

[0045] Furthermore, in step S4, the molding equipment includes a twin-screw extruder, the processing temperature of the twin-screw extruder is 280°C to 300°C, the main engine speed is 350rpm to 500rpm, and the vacuum degree is ≥0.08MPa; the temperature of the infiltration mold is 290°C to 310°C.

[0046] The processing temperature of the twin-screw extruder is 290°C, the main engine speed is 450rpm, the vacuum degree is 0.08MPa; the temperature of the wetting die is 300°C.

[0047] Compared with the prior art, the present invention has the following advantages and beneficial effects:

[0048] 1. The present invention adopts two kinds of maleic anhydride grafted polypropylenes (maleic anhydride grafted polypropylene I and maleic anhydride grafted polypropylene II) with different grafting rates and melt indexes and long glass fibers to prepare antistatic long glass fiber reinforced polypropylene composite materials. Maleic anhydride grafted polypropylene I and maleic anhydride grafted polypropylene II are used in different processes respectively, and are matched with pretreated long glass fibers to improve the connection effect between the long glass fibers and the maleic anhydride grafted polypropylene. At the same time, silane coupling agent and polyethylene wax are added to the formula. Through the joint action of maleic anhydride grafted polypropylene I, maleic anhydride grafted polypropylene II, polyethylene wax and silane coupling agent, the fluidity of the molten system during extrusion molding can be controlled within a reasonable range, which can not only achieve smooth molding, but also reduce the floating fiber phenomenon of the product glass fibers.

[0049] 2. The present invention adds an antistatic agent and a conductive filler into the molten system so that the prepared long glass fiber reinforced polypropylene composite material has antistatic properties.

[0050] 3. The present invention improves the anti-oxidation effect of the material and the corrosion resistance thereof by adding an antioxidant into the molten system. DETAILED DESCRIPTION

[0051] In order to make the purpose, technical scheme and advantages of the present invention clearer, the present invention is further described in detail below in conjunction with the embodiments. The schematic implementation mode of the present invention and its description are only used to explain the present invention and are not intended to limit the present invention. The embodiments described below are part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.

[0052] In the following description, a large number of specific details are set forth in order to provide a thorough understanding of the present invention. However, it is apparent to those of ordinary skill in the art that these specific details do not have to be employed to practice the present invention. In other embodiments, in order to avoid confusing the present invention, known structures, materials or methods are not specifically described. The materials, instruments and reagents used in the following examples, unless otherwise specified, can be obtained from commercial sources. The technical means used in the examples, unless otherwise specified, are conventional means well known to those skilled in the art.

[0053] The existing long glass fiber reinforced polypropylene composite material has a serious problem of glass fiber floating phenomenon and is prone to static electricity. In order to solve the above problems, this embodiment provides an antistatic long glass fiber reinforced polypropylene composite material, including the following components by weight:

[0054] 30-40 parts of maleic anhydride grafted polypropylene I, 20-30 parts of maleic anhydride grafted polypropylene II, 30-50 parts of long glass fiber, 5-8 parts of polyacrylamide, 2-5 parts of glyceryl stearate, 1-2 parts of silane coupling agent, and 2-4 parts of polyethylene wax; wherein the long glass fiber is a fiber subjected to surface pretreatment with a coupling agent, wherein the grafting rate of maleic anhydride grafted polypropylene I is 0.8-1.0%, and the melt index is 80-120 g / 10min; the grafting rate of maleic anhydride grafted polypropylene II is 1.2-1.5%, and the melt index is 300-350g / 10min.

[0055] The melt index is the flow rate measured at 230° C. and a load of 2.16 kg.

[0056] Specifically, the long glass fiber is a continuous alkali-free glass fiber with a single fiber diameter of 14-17 μm.

[0057] In a preferred case, the silane coupling agent is a liquid silane coupling agent, and the liquid silane coupling agent is composed of the following components in weight percentage:

[0058] Ethoxysilane 20%, anhydrous ethanol 72%, purified water 8%.

[0059] In a preferred embodiment, the following components in parts by weight are also included:

[0060] 2-3 parts of carbon black.

[0061] In a preferred embodiment, the following components in parts by weight are also included:

[0062] 1-2 parts of antioxidant. The antioxidant may be a phenolic antioxidant, for example, 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane.

[0063] The method for preparing the above-mentioned antistatic long glass fiber reinforced polypropylene composite material comprises the following steps:

[0064] S1. Pretreatment of long glass fiber: Use coupling agent to pretreat the surface of long glass fiber; specifically:

[0065] The specific process of preprocessing is:

[0066] S11, cleaning and drying the long glass fibers;

[0067] S12, soaking the long glass fiber treated in step S11 in a 10%-15% potassium permanganate solution under ultrasonic vibration for 30-60 minutes;

[0068] S13, under ultrasonic vibration conditions, immersing the long glass fiber treated in step S12 in a silane coupling agent solution for 30-60 minutes, specifically:

[0069] The silane coupling agent solution is composed of the following components in weight percentage: 25% ethoxysilane, 69% anhydrous ethanol, and 6% purified water.

[0070] S2. Dispersion of long glass fibers: The maleic anhydride grafted polypropylene I and the long glass fibers are uniformly mixed according to a certain proportion, and then heated to a molten state and maintained for 1-3 hours.

[0071] S3, impregnation of long glass fibers: adding the polyacrylamide to the molten system of step S2, mixing and maintaining for 2-10 seconds;

[0072] S4, extrusion molding: the molten system obtained in step S3 is mixed with the maleic anhydride grafted polypropylene II, the stearic acid glyceryl ester, the silane coupling agent and the polyethylene wax, and then put into an extruder for extrusion molding, cooling and pelletizing; the extruder can be a twin-screw extruder, the processing temperature of the twin-screw extruder is 280°C to 300°C, the main engine speed is 350rpm to 500rpm, and the vacuum degree is ≥0.08MPa; the temperature of the infiltration mold is 290°C to 310°C.

[0073] Preferably, the processing temperature of the twin-screw extruder is 290°C, the main engine speed is 450rpm, the vacuum degree is 0.08MPa; and the temperature of the wetting die is 300°C.

[0074] In this embodiment, two kinds of maleic anhydride grafted polypropylenes with different grafting rates and melt indexes (maleic anhydride grafted polypropylene I and maleic anhydride grafted polypropylene II) and long glass fibers are used to prepare antistatic long glass fiber reinforced polypropylene composite materials. Maleic anhydride grafted polypropylene I and maleic anhydride grafted polypropylene II are used in different processes, respectively. Among them, maleic anhydride grafted polypropylene I with relatively low grafting rate and melt index is used in the dispersion and impregnation process of long glass fibers to ensure the bonding effect between long glass fibers and maleic anhydride grafted polypropylene and reduce floating fibers; maleic anhydride grafted polypropylene I with relatively low grafting rate and melt index is used in the dispersion and impregnation process of long glass fibers to ensure the bonding effect between long glass fibers and maleic anhydride grafted polypropylene and reduce floating fibers; A relatively high number of maleic anhydride grafted polypropylene II is used in the material molding process to ensure fluidity during molding. Together with the pretreated long glass fiber, the connection effect between the long glass fiber and the maleic anhydride grafted polypropylene can be improved. At the same time, silane coupling agent and polyethylene wax are added to the formula. Through the joint action of maleic anhydride grafted polypropylene I, maleic anhydride grafted polypropylene II, polyethylene wax and silane coupling agent, the fluidity of the molten system during material molding can be controlled within a reasonable range, which can not only achieve smooth molding, but also reduce the floating fiber phenomenon of the product glass fiber.

[0075] In addition, in this embodiment, an antistatic agent (glyceryl stearate) and a conductive filler (carbon black) are added to the molten system, so that the prepared long glass fiber reinforced polypropylene composite material has antistatic properties.

[0076] In order to better illustrate the technical effect of this embodiment, the following examples and comparative examples are used for analysis and explanation:

[0077] Embodiment 1:

[0078] An antistatic long glass fiber reinforced polypropylene composite material, composed of the following components in parts by weight:

[0079] 40 parts of maleic anhydride grafted polypropylene I, 30 parts of maleic anhydride grafted polypropylene II, 40 parts of long glass fiber, 6 parts of polyacrylamide, 4 parts of glyceryl stearate, 2 parts of silane coupling agent, and 4 parts of polyethylene wax; wherein the long glass fiber is a fiber that has been surface pretreated with a coupling agent, wherein the grafting rate of maleic anhydride grafted polypropylene I is 1.0%, and the melt index is 100g / 10min; the grafting rate of maleic anhydride grafted polypropylene II is 1.2, and the melt index is 320g / 10min.

[0080] Specifically, maleic anhydride grafted polypropylene I is maleic anhydride grafted polypropylene (PP-g-MAH), BONDYRAM 1001, Pulilang Plastic Industry Co., Ltd., with a grafting rate of 1.0%, a melting point of 160°C, and a density of 0.9 g / cm 3 ; Under the conditions of 230℃ and 2.16kg load, the melt index is 100g / 10min.

[0081] Specifically, maleic anhydride grafted polypropylene II is obtained by melt extrusion of polypropylene with a melt index of about 320 g / 10 min and maleic anhydride, and the specific process is as follows:

[0082] Polypropylene, cumene peroxide, styrene, maleic anhydride and dioctyl adipate were mixed in a weight ratio of 100:0.2:1.5:2:0.8, extruded by a twin-screw extruder, and cooled to obtain the obtained product. The extrusion temperature was set at 200 °C and the screw speed was set at 190 rpm. The grafting rate of the prepared maleic anhydride grafted polypropylene II was 1.2%, and the melt index was 320 g / 10 min at 230 °C and a load of 2.16 kg.

[0083] Among them, polypropylene, cumene peroxide, styrene, maleic anhydride and dioctyl adipate can all be purchased commercially. Among them, polypropylene can also be obtained by copolymerizing ethylene as a monomer to obtain polypropylene with a desired melt index. The specific process is well known in the art and will not be repeated here.

[0084] Among them, the long glass fiber is continuous alkali-free glass fiber, and the single fiber diameter is 14-17μm.

[0085] Wherein, the silane coupling agent is a liquid silane coupling agent, and the liquid silane coupling agent is composed of the following components in weight percentage:

[0086] Ethoxysilane 20%, anhydrous ethanol 72%, purified water 8%.

[0087] The preparation method of the antistatic long glass fiber reinforced polypropylene composite material of this embodiment comprises the following steps:

[0088] S1. Pretreatment of long glass fiber:

[0089] S11, cleaning and drying the long glass fibers;

[0090] S12, soaking the long glass fiber treated in step S11 in a 15% potassium permanganate solution under ultrasonic vibration for 30 minutes;

[0091] S13, under ultrasonic vibration conditions, immersing the long glass fiber treated in step S12 in a silane coupling agent solution for 30 minutes, specifically:

[0092] The silane coupling agent solution is composed of the following components in weight percentage: 25% ethoxysilane, 69% anhydrous ethanol, and 6% purified water.

[0093] S2. Dispersion of long glass fibers: The maleic anhydride grafted polypropylene I and the long glass fibers are uniformly mixed according to a certain proportion, and then heated to a molten state and maintained for 2 hours.

[0094] S3. Infiltration of long glass fibers: Add the polyacrylamide into the molten system of step S2, mix well and keep for 5 seconds.

[0095] S4, extrusion molding: the molten system obtained in step S3 is mixed with the maleic anhydride grafted polypropylene II, the stearic acid glyceryl ester, the silane coupling agent and the polyethylene wax, and then put into an extruder for extrusion molding, cooling and pelletizing. The processing temperature of the twin-screw extruder is 290°C, the main engine speed is 450rpm, and the vacuum degree is 0.08MPa; the temperature of the impregnation die is 300°C.

[0096] Embodiment 2:

[0097] This embodiment is based on the embodiment, and the difference from the embodiment 1 is that carbon black and an antioxidant are also added to the formula, and the antioxidant is specifically 1,1,3-tris(2-methyl-4-hydroxy-5-tert-butylphenyl)butane. The specific formula is as follows:

[0098] An antistatic long glass fiber reinforced polypropylene composite material, composed of the following components in parts by weight:

[0099] Maleic anhydride grafted polypropylene I 40 parts, maleic anhydride grafted polypropylene II 30 parts, long glass fiber 40 parts, polyacrylamide 6 parts, stearic acid glyceryl 4 parts, silane coupling agent 2 parts, polyethylene wax 4 parts, carbon black 3 parts, 1,1,3-tris (2-methyl-4-hydroxy-5-tert-butylphenyl) butane 1 part.

[0100] Embodiment 3:

[0101] This embodiment is based on the embodiment, and the difference from the embodiment 1 is that the dosage of each component in the formula is different, as follows:

[0102] An antistatic long glass fiber reinforced polypropylene composite material, composed of the following components in parts by weight:

[0103] 30 parts of maleic anhydride grafted polypropylene I, 20 parts of maleic anhydride grafted polypropylene II, 30 parts of long glass fibers, 5 parts of polyacrylamide, 2 parts of stearic acid glyceryl ester, 1 part of silane coupling agent, and 2 parts of polyethylene wax.

[0104] Comparative Example 1:

[0105] This comparative example is based on Example 1, and the difference from Example 1 is that:

[0106] An equal amount of maleic anhydride grafted polypropylene II is used to replace maleic anhydride grafted polypropylene I, and the impregnation and dispersion steps of long glass fibers are not performed. The various components in the formula are directly mixed evenly, melt extruded, and then heat treated. The specific formula is as follows:

[0107] An antistatic long glass fiber reinforced polypropylene composite material, composed of the following components in parts by weight:

[0108] Maleic anhydride grafted polypropylene II 70 parts, long glass fiber 40 parts, polyacrylamide 6 parts, stearic acid glyceryl 4 parts, silane coupling agent 2 parts, polyethylene wax 4 parts.

[0109] Comparative Example 2:

[0110] This comparative example is based on Example 1, and differs from Example 1 in that the long glass fibers are not pretreated.

[0111] Comparative Example 3:

[0112] This comparative example is based on Example 1, and differs from Example 1 in that the long glass fibers are directly immersed in the silane coupling agent solution without ultrasonic vibration.

[0113] Comparative Example 4:

[0114] This comparative example is based on Example 1, and differs from Example 1 in that no heat treatment is performed.

[0115] Comparative Example 5:

[0116] This comparative example is based on Example 2, and the difference from Example 2 is:

[0117] Instead of using carbon black, carbon black was replaced by an equal amount of glyceryl stearate.

[0118] Comparative Example 6:

[0119] This comparative example is based on Example 1, and the difference from Example 1 is that:

[0120] The maleic anhydride grafted polypropylene I was replaced with the maleic anhydride grafted polypropylene II, and the dispersion and impregnation steps of the long glass fiber were not performed. The various components in the formula were directly mixed evenly and melt extruded. The extrusion molding process was blocked and no subsequent tests were performed. The specific formula is as follows:

[0121] An antistatic long glass fiber reinforced polypropylene composite material, composed of the following components in parts by weight:

[0122] Maleic anhydride grafted polypropylene I 70 parts, long glass fiber 40 parts, polyacrylamide 6 parts, stearic acid glyceryl ester 4 parts, silane coupling agent 2 parts, polyethylene wax 4 parts.

[0123] The antistatic long glass fiber reinforced polypropylene composite materials prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were subjected to performance tests, including tensile strength (test standard: ASTM D638; tensile speed 50 mm / min), flexural strength (test standard: ASTM D790;, bending speed 2 mm / min), flexural modulus (test standard: ASTM D790;, bending speed 2 mm / min), surface resistivity (test standard: ASTM D257) tests, and appearance observation. The test results are shown in Table 1:

[0124] Table 1

[0125]

[0126] The specific implementation methods described above further illustrate the objectives, technical solutions and beneficial effects of the present invention in detail. It should be understood that the above description is only a specific implementation method of the present invention and is not intended to limit the scope of protection of the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the scope of protection of the present invention.

Claims

1. An antistatic long glass fiber reinforced polypropylene composite material, characterized in that: It includes the following components by weight: 30-40 parts of maleic anhydride grafted polypropylene I, 20-30 parts of maleic anhydride grafted polypropylene II, 30-50 parts of long glass fiber, 5-8 parts of polyacrylamide, 2-5 parts of glyceryl stearate, 1-2 parts of silane coupling agent, and 2-4 parts of polyethylene wax; wherein the long glass fiber is a fiber that has been surface pretreated with a coupling agent, wherein the grafting rate of the maleic anhydride grafted polypropylene I is 0.8-1.0%, and the melt index is 80-120 g / 10min; the grafting rate of the maleic anhydride grafted polypropylene II is 1.2-1.5%, and the melt index is 300-350g / 10min; The maleic anhydride grafted polypropylene I is used in the dispersion step in the preparation process of the antistatic long glass fiber reinforced polypropylene composite material; the maleic anhydride grafted polypropylene II, the stearic acid glycerol ester, the silane coupling agent and the polyethylene wax are used in the extrusion molding step in the preparation process of the antistatic long glass fiber reinforced polypropylene composite material.

2. The antistatic long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: Also includes the following components by weight: 2-3 parts of carbon black.

3. The antistatic long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: Also includes the following components by weight: 1-2 parts of antioxidant.

4. The antistatic long glass fiber reinforced polypropylene composite material according to claim 1, characterized in that: The silane coupling agent is a liquid silane coupling agent, and the liquid silane coupling agent is composed of the following components in weight percentage: Ethoxysilane 20%, anhydrous ethanol 72%, purified water 8%.

5. The antistatic long glass fiber reinforced polypropylene composite material according to any one of claims 1 to 4, characterized in that: The long glass fiber is a continuous alkali-free glass fiber, and the diameter of the single fiber is 14-17 μm.

6. The method for preparing the antistatic long glass fiber reinforced polypropylene composite material according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1. Pretreatment of long glass fibers: using a coupling agent to pretreat the surface of the long glass fibers; S2. Dispersion of long glass fibers: the maleic anhydride grafted polypropylene I and the long glass fibers are uniformly mixed according to a certain proportion, and then heated to a molten state and maintained for 1-3 hours; S3, impregnation of long glass fibers: adding the polyacrylamide to the molten system of step S2, mixing and maintaining for 2-10 seconds; S4, extrusion molding: the molten system obtained in step S3 is mixed evenly with the maleic anhydride grafted polypropylene II, the stearic acid glyceryl ester, the silane coupling agent and the polyethylene wax, and then put into an extruder for extrusion molding, cooling and pelletizing.

7. The preparation method according to claim 6, characterized in that: In step S1, the specific process of preprocessing is: S11, cleaning and drying the long glass fibers; S12, soaking the long glass fiber treated in step S11 in a 10%-15% potassium permanganate solution under ultrasonic vibration for 30-60 minutes; S13. Under ultrasonic vibration conditions, immerse the long glass fiber treated in step S12 in a silane coupling agent solution for 30-60 minutes.

8. The preparation method according to claim 7, characterized in that: The silane coupling agent solution is composed of the following components in weight percentage: Ethoxysilane 25%, anhydrous ethanol 69%, purified water 6%.

9. The preparation method according to claim 6, characterized in that: In step S4, the extruder is a twin-screw extruder, the processing temperature of the twin-screw extruder is 280°C to 300°C, the main engine speed is 350rpm to 500rpm, and the vacuum degree is ≥0.08MPa; the temperature of the infiltration mold is 290°C to 310°C.

10. The preparation method according to claim 9, characterized in that: The processing temperature of the twin-screw extruder is 290°C, the main engine speed is 450rpm, and the vacuum degree is 0.08MPa; The temperature of the infiltration head used during infiltration was 300°C.