A polyimide-based carbon membrane for CO2 / N2 separation and a preparation method thereof

By introducing -CF3 groups into the polyimide molecular chain and performing pyrolysis treatment, the problem of low CO2 penetration of the carbon membrane is solved, efficient CO2 capture is achieved, and a method for CO2/N2 separation is provided. High-performance polyimide-based carbon membrane.

CN118371130BActive Publication Date: 2024-10-01GUANGDONG TECHNION ISRAEL INST OF TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410807755.6
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-21
Publication Date
2024-10-01
Estimated Expiration
2044-06-21

AI Technical Summary

Technical Problem

Existing carbon membranes have low CO2 penetration during the CO2/N2 separation process, resulting in low separation efficiency.

Method used

By introducing -CF3 groups into the polyimide molecular chain, the stacking density of the molecular chain is reduced and small molecular gases are decomposed during the pyrolysis process to create pores to increase the CO2 flux of the carbon membrane. Heat treatment at 500~1000℃ is used. Preparation of polyimide-based carbon membrane through decomposition process.

Benefits of technology

It significantly increases the CO2 permeation flux and achieves efficient CO2 capture. It has excellent performance and is suitable for the field of CO2 capture.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118371130B_ABST
    Figure CN118371130B_ABST
Patent Text Reader

Abstract

One for CO 2 / N 2 Polyimide-based carbon membrane for separation and preparation method thereof, belonging to CO 2 In the field of capture technology, it overcomes the carbon membrane CO 2 The present invention is used for CO 2 / N 2 The preparation method of the isolated polyimide-based carbon membrane comprises: step 1, mixing a diamine monomer, a dianhydride monomer and an organic solvent to obtain a mixed solution, reacting to obtain a polyamic acid solution; at least part of the diamine monomer and / or at least part of the dianhydride monomer contains CF 3 ; Step 2, mixing the polyamic acid solution with a dehydrating agent and a catalyst, reacting to obtain polyimide; Step 3, using the polyimide obtained in Step 2 to prepare a polyimide precursor film; Step 4, pyrolyzing the polyimide precursor film at 500-1000°C to obtain a polyimide-based carbon film. The carbon film of the present invention has ultra-high CO 2 Flux, which can achieve CO 2 Efficient capture.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of CO2 capture, and in particular relates to a polyimide-based carbon membrane for CO2 / N2 separation and a preparation method thereof. Background Art

[0002] With the rapid development of the global economy, humanity's demand for energy has increased dramatically, particularly for fossil fuels such as oil, coal, and natural gas. However, the combustion of fossil fuels leads to the production of large amounts of greenhouse gases. CO2, as a major greenhouse gas, exacerbates global climate change, contributing to rising sea levels and melting polar ice caps. To directly and effectively reduce carbon emissions, the implementation of CO2 capture technology is crucial.

[0003] Traditional gas separation technologies, such as pressure swing adsorption and cryogenic separation, suffer from drawbacks such as high cost, high energy consumption, and complex production processes. In recent years, membrane gas separation technologies, offering low cost, low energy consumption, and safe and simple operation, have garnered widespread attention. Among these technologies, carbon molecular sieve membranes (referred to as carbon membranes) have attracted significant attention due to their advanced, highly selective, nanoscale ultrafine pore structure, high thermal and chemical stability, corrosion resistance, and gas separation performance exceeding the Robeson upper limit.

[0004] Carbon membranes are generally produced by pyrolysis of polymer membranes, but the carbon membranes produced by pyrolysis of existing polymer membranes such as polysulfone, homophenyl or biphenyl polyimide membranes have low CO2 permeation during use. Summary of the Invention

[0005] Therefore, the technical problem to be solved by the present invention is to overcome the defect of low CO2 permeability of carbon membranes in the prior art, thereby providing a polyimide-based carbon membrane for CO2 / N2 separation and a preparation method thereof.

[0006] To this end, the present invention provides the following technical solutions.

[0007] In a first aspect, the present invention provides a method for preparing a polyimide-based carbon membrane for CO2 / N2 separation, comprising the following steps:

[0008] Step 1: mixing a diamine monomer, a dianhydride monomer and an organic solvent to obtain a mixed solution, reacting to obtain a polyamic acid solution; at least part of the diamine monomer and / or at least part of the dianhydride monomer contains -CF3;

[0009] Step 2: mixing the polyamic acid solution with a dehydrating agent and a catalyst, and reacting the mixture to obtain polyimide;

[0010] Step 3, preparing a polyimide precursor film using the polyimide prepared in step 2;

[0011] Step 4: pyrolyzing the polyimide precursor film at 500-1000° C. to obtain a polyimide-based carbon film;

[0012] The diamine monomer containing -CF3 is the first diamine monomer;

[0013] The first diamine monomer is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane (6FAP), 2,2-bis[4-(4-aminophenoxyphenyl)]hexafluoropropane (HFBAPP), 2,2'-bis(trifluoromethyl)diaminobiphenyl (TFDB), 4,4'-oxybis[3-(trifluoromethyl)aniline (6FODA), N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide) ( AB-TFMB), 2,2-bis(4-aminophenyl)hexafluoropropane (FA), N,N'-[[2,2,2-trifluoro-1-(trifluoromethyl)ethylidene]bis(6-hydroxy-3,1-phenylene)]bis[3-aminobenzamide] (M-6FDAP), and N,N'-[[2,2,2-trifluoro-1-(trifluoromethyl)ethylidene]bis(6-hydroxy-3,1-phenylene)]bis[4-aminobenzamide] (P-6FDAP).

[0014] The diamine monomer not containing -CF3 is the second diamine monomer;

[0015] The second diamine monomer is a combination of one or more of 2,4,6-trimethyl-1,3-phenylenediamine (DAM), 1,4-bis(4-aminophenoxy)benzene (TPE-Q), 4,4'-bis(4-aminophenoxy)biphenyl (BAPB), p-phenylenediamine (p-PDA), 1,6-hexanediamine (HMDA), 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid (2,2'-DCB), 2,2-bis(4-hydroxy-3-aminophenyl)propane (BAP), 3,3'-dihydroxybenzidine (HAB), 9,9-bis(3-amino-4-hydroxyphenyl)fluorene (BisAHPF), and 4,4'-diaminodiphenyl ether (ODA).

[0016] Optionally, step 4 is performed by pyrolysis at 600-800°C.

[0017] Optionally, the organic solvent in step 1 is N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), m-cresol (m-Cresol) or dimethyl sulfoxide (DMSO).

[0018] Furthermore, step 1 satisfies at least one of the following conditions:

[0019] (1) The molar ratio of the diamine monomer to the dianhydride monomer is 1:(1-1.05);

[0020] (2) The solid content of the mixed solution is 10-30 wt%;

[0021] (3) The reaction temperature in step 1 is 0-30°C;

[0022] (4) The reaction time in step 1 is 24 to 48 hours;

[0023] (5) Stirring is continued during the reaction in step 1. Preferably, the stirring rate is 50 to 600 rpm.

[0024] Further, the dianhydride monomer containing -CF3 is the first dianhydride monomer;

[0025] The first dianhydride monomer is a combination of one or more of hexafluorodianhydride (6FDA), N-[4-[4-[(1,3-dioxy-2-benzofuran-5-carbonyl)amino]-2-(trifluoromethyl)phenyl]-3-(trifluoromethyl)phenyl]-1,3-dioxy-2-benzofuran-5-carboxamide (TA-TFMB), 9,9-bis(trifluoromethyl)-2,3,6,7-oxanthene tetracarboxylic dianhydride (6FCDA) and bisphenol AF dianhydride (BPADA).

[0026] Further, the dianhydride monomer not containing -CF3 is the second dianhydride monomer;

[0027] The second dianhydride monomer is a combination of one or more of 3,3'4,4'-benzophenonetetracarboxylic dianhydride (BTDA), pyromellitic dianhydride (PMDA), and 3,3,4,4-diphenylsulfonetetracarboxylic dianhydride (DSDA).

[0028] Furthermore, step 2 satisfies at least one of the following conditions:

[0029] (1) The dehydrating agent includes at least one of trifluoroacetic anhydride, acetic anhydride, acetyl chloride, thionyl chloride and dicyclohexylcarboximide;

[0030] (2) The catalyst comprises at least one of pyridine, triethylamine and 3-methylpyridine;

[0031] (3) The volume of the dehydrating agent is 880 to 950 times the total molar amount of the diamine monomer, where the volume unit is ml and the molar amount unit is mol;

[0032] (4) The volume amount of the catalyst is 90 to 120 times the total molar amount of the diamine monomer, where the volume unit is ml and the molar amount unit is mol;

[0033] (5) The reaction temperature in step 2 is 0-30°C;

[0034] (6) The reaction time in step 2 is 24 to 48 hours;

[0035] (7) Stirring is continued during the reaction in step 2. Preferably, the stirring rate is 100 to 600 rpm.

[0036] Furthermore, step 4 satisfies at least one of the following conditions:

[0037] (1) Pyrolysis in an argon atmosphere;

[0038] Preferably, the flow rate of argon is 100 to 1000 mL / min;

[0039] (2) The pyrolysis process includes heating the temperature from room temperature to 15°C below the final temperature at a rate of 2-5°C / min, then heating the temperature to a final temperature of 600-800°C at a rate of 0.25-1°C / min, and maintaining the temperature for 30-150 minutes. Exemplarily, the final carbonization temperature is 650°C, 700°C, or 750°C. Reducing the heating rate near the final temperature can prevent defects in the prepared polyimide-based carbon film.

[0040] In a possible embodiment, the diamine monomer includes 2,4,6-trimethyl-1,3-phenylenediamine and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide), the molar ratio of 2,4,6-trimethyl-1,3-phenylenediamine and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide) is 3:2~1:1, and the dianhydride monomer is hexafluorodianhydride.

[0041] In a possible embodiment, the diamine monomer is N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide), and the dianhydride monomer is hexafluorodianhydride.

[0042] In a possible embodiment, the diamine monomer includes 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide), the molar ratio of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide) is 3:2~1:1, and the dianhydride monomer is hexafluorodianhydride.

[0043] In a possible embodiment, the diamine monomer includes 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 2,2-bis(4-hydroxy-3-aminophenyl)propane, the molar ratio of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and 2,2-bis(4-hydroxy-3-aminophenyl)propane is 3:2~1:1, and the dianhydride monomer is 3,3'4,4'-benzophenonetetracarboxylic dianhydride.

[0044] In a second aspect, the present invention provides a polyimide-based carbon membrane prepared according to the method for preparing the polyimide-based carbon membrane for CO2 / N2 separation.

[0045] Optionally, the first diamine monomer accounts for 1% to 99% of the total molar amount of the diamine monomers. Exemplarily, the first diamine monomer accounts for 30%, 40%, 50%, 60% or 70% of the total molar amount of the diamine monomers.

[0046] Optionally, the first dianhydride monomer accounts for 1% to 100% of the total molar amount of the dianhydride monomers. Exemplarily, the first dianhydride monomer accounts for 30%, 40%, 50%, 60% or 70% of the total molar amount of the dianhydride monomers.

[0047] Furthermore, step 1 includes: adding a diamine monomer to an organic solvent and stirring to dissolve; then adding a dianhydride monomer, reacting to obtain a polyamic acid solution; further, adding the diamine monomer to an organic solvent and stirring to dissolve at 0~30℃; optionally, the stirring and dissolving time is 40~120min.

[0048] During the entire process of polyimide preparation, the temperature of the reaction system must be maintained at 0-30°C.

[0049] Furthermore, step 2 also includes recrystallizing the polyimide.

[0050] Furthermore, step 3 includes: stirring and dissolving the polyimide obtained in step 2 in a solvent to obtain a polyimide casting solution; casting the polyimide casting solution into a film, vacuum degassing, drying, and cooling to obtain a polyimide precursor film.

[0051] Optionally, the temperature conditions for stirring and dissolving the polyimide in the solvent are 20 to 60° C.; the dissolving and stirring time is 12 to 48 hours; and the dissolving and stirring speed is 100 to 1000 rpm.

[0052] Optionally, the solvent used to dissolve the polyimide is N,N-dimethylacetamide (DMAc), N,N-dimethylformamide (DMF), N-methylpyrrolidone (NMP), m-cresol (m-Cresol), dimethyl sulfoxide (DMSO), chloroform, or tetrahydrofuran (THF).

[0053] Optionally, the solid content of the polyimide casting solution is 5-20 wt %, and illustratively, it can be 5 wt %, 8 wt %, 10 wt %, 15 wt %, or 20 wt %.

[0054] Optionally, the temperature condition for vacuum degassing is 20-50° C.; and the time for vacuum degassing is 3-8 hours.

[0055] Optionally, the drying temperature is 60-120° C., and the drying time is 24-72 hours.

[0056] The technical solution of the present invention has the following advantages:

[0057] 1. The preparation method of the polyimide-based carbon membrane for CO2 / N2 separation of the present invention comprises the following steps: step 1, mixing a diamine monomer, a dianhydride monomer and an organic solvent to obtain a mixed solution, reacting to obtain a polyamic acid solution; at least part of the diamine monomer and / or at least part of the dianhydride monomer contains -CF3; step 2, mixing the polyamic acid solution with a dehydrating agent and a catalyst, reacting to obtain a polyimide; step 3, using the polyimide obtained in step 2 to prepare a polyimide precursor film; step 4, mixing the polyimide The amine precursor film is pyrolyzed at 500-1000° C. to obtain a polyimide-based carbon film; the diamine monomer containing -CF3 is the first diamine monomer; the first diamine monomer is 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 2,2-bis[4-(4-aminophenoxybenzene)]hexafluoropropane, 2,2'-bis(trifluoromethyl)diaminobiphenyl, 4,4'-oxybis[3-(trifluoromethyl)aniline, N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4 ,4'-diyl)bis(4-aminobenzamide), 2,2-bis(4-aminophenyl)hexafluoropropane, N,N'-[[2,2,2-trifluoro-1-(trifluoromethyl)ethylidene]bis(6-hydroxy-3,1-phenylene)]bis[3-aminobenzamide] and N,N'-[[2,2,2-trifluoro-1-(trifluoromethyl)ethylidene]bis(6-hydroxy-3,1-phenylene)]bis[4-aminobenzamide]; the diamine monomer not containing -CF3 is the first Diamine monomer; the second diamine monomer is a combination of one or more of 2,4,6-trimethyl-1,3-phenylenediamine, 1,4-bis(4-aminophenoxy)benzene, 4,4'-bis(4-aminophenoxy)biphenyl, p-phenylenediamine, 1,6-hexanediamine, 4,4'-diaminobiphenyl-2,2'-dicarboxylic acid, 2,2-bis(4-hydroxy-3-aminophenyl)propane, 3,3'-dihydroxybenzidine, 9,9-bis(3-amino-4-hydroxyphenyl)fluorene, and 4,4'-diaminodiphenyl ether.

[0058] Starting from the structural design of the precursor, the present invention introduces a -CF3 group with a large spatial volume and easy to decompose into the polyimide molecular chain, reduces the packing density of the polyimide molecular chain, and increases its free volume fraction. At the same time, the -CF3 group decomposes to produce small molecular gas during the pyrolysis and carbonization process, which plays a role in pore formation, thereby preparing a carbon membrane with high CO2 flux, solving the problem of low permeation flux of the carbon membrane, and achieving the purpose of efficiently capturing CO2.

[0059] The preparation method of the present invention is easy to scale up and has good repeatability. The obtained polyimide-based carbon membrane has excellent performance and can be used in the field of CO2 capture, providing a new idea for the preparation of carbon dioxide membrane separation materials. BRIEF DESCRIPTION OF THE DRAWINGS

[0060] In order to more clearly illustrate the specific embodiments of the present invention or the technical solutions in the prior art, the following briefly introduces the drawings required for use in the specific embodiments or the description of the prior art. Obviously, the drawings described below are some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative work.

[0061] Figure 1 is the polyimide in Example 1 1 H NMR spectra;

[0062] Figure 2 is the polyimide in Example 1 19 F NMR spectrum;

[0063] Figure 3 IR spectra of 6FDA, AB-TFMB and the prepared polyimide in Example 1;

[0064] Figure 4 are photos of the polyimide-based carbon membranes prepared in Examples 1, 2, and 3;

[0065] Figure 5 The carbonization procedure of the polyimide-based carbon membrane in Examples 1, 2, and 3 is as follows;

[0066] Figure 6 Surface electron microscopy images of the polyimide-based carbon films in Examples 1, 2, and 3;

[0067] Figure 7 : Electron microscope images of the cross sections of the polyimide-based carbon membranes in Examples 1, 2, and 3;

[0068] Figure 8 is the X-ray diffraction pattern of the polyimide-based carbon film in Examples 1, 2, and 3;

[0069] Figure 9The thermal weight loss curves of the polyimide-based carbon membranes in Examples 1, 2, and 3;

[0070] Figure 10 The mechanical properties of the polyimide-based carbon membranes in Examples 1, 2, and 3;

[0071] Figure 11 This is a graph evaluating the CO2 / N2 separation performance of the polyimide-based carbon membrane in Examples 1, 2, and 3;

[0072] Figure 12 IR spectra of the polyimide-based carbon films in Examples 1, 2, and 3. DETAILED DESCRIPTION

[0073] The following examples are provided for a better understanding of the present invention and are not intended to limit the best mode of implementation. They do not limit the content and scope of protection of the present invention. Any product identical or similar to the present invention obtained by anyone under the guidance of the present invention or by combining the features of the present invention with other prior arts shall fall within the scope of protection of the present invention.

[0074] If no specific experimental steps or conditions are specified in the examples, the conventional experimental steps or conditions described in the literature in this field can be used. If the manufacturer of the reagents or instruments is not specified, they are all commercially available conventional reagents.

[0075] Example 1

[0076] This embodiment provides a method for preparing a polyimide-based carbon membrane for CO2 / N2 separation, comprising the following steps:

[0077] Step 1: Weigh 3.61g DAM (2,4,6-trimethyl-1,3-phenylenediamine, 0.024mol) and 8.94g AB-TFMB (0.016mol) into a 250mL three-necked flask. Add 121.28g NMP to the flask and introduce Ar. Maintain the reaction temperature at 25°C and stir at 200 rpm for 90 minutes. Then, add 17.77g 6FDA (0.040mol). After the additions are complete, continue the reaction at the same stirring speed and temperature for 24 hours to obtain a transparent, viscous polyamic acid solution.

[0078] Step 2: Add 36 ml of acetic anhydride and 4 ml of 3-methylpyridine to the polyamic acid solution, maintain the reaction temperature at 25° C., and stir at a stirring rate of 400 rpm for 24 hours to obtain a transparent and viscous polyimide solution.

[0079] The polyimide solution was poured into methanol for recrystallization, filtered and dried.

[0080] Step 3: Add the dried polyimide into DMF at 25° C. and stir at 400 rpm for 24 hours to prepare a polyimide casting solution with a solid content of 8 wt %.

[0081] The polyimide casting liquid was poured into a clean flat-bottomed Petri dish to form a film, and then placed in a vacuum oven and vacuumed and degassed at 30°C for 4 hours; the Petri dish was taken out, transferred to an oven, and dried at a constant temperature of 80°C for 48 hours, and a polyimide precursor film was obtained after natural cooling.

[0082] Step 4: Place the polyimide precursor film in a carbonization furnace and perform high-temperature pyrolysis in a 500 mL / min Ar atmosphere. Figure 5 As shown in the figure, the temperature was first increased to 585°C at a heating rate of 3°C / min; then the temperature was increased to 600°C at a heating rate of 0.25°C / min and kept warm for 60 minutes; finally, the temperature was naturally cooled to room temperature to obtain a polyimide-based carbon film, and the thickness of the polyimide-based carbon film was about 100 μm.

[0083] Figure 1 、 Figure 2 are respectively the polyimide of this embodiment 1 H NMR spectra and 19 F NMR spectrum; Figure 3 IR spectra of 6FDA, AB-TFMB and the prepared polyimide (PI) in this example. Figure 1-Figure 3 It shows that polyimide was successfully prepared in this embodiment.

[0084] from Figure 4 、 Figure 6 、 Figure 7 It can be seen from the figure that the surface of the polyimide-based carbon membrane is smooth and dense.

[0085] Example 2

[0086] The preparation method of the polyimide-based carbon membrane for CO2 / N2 separation in this embodiment is essentially the same as that in Example 1, except that the final carbonization temperature is different. Specifically, step 4 involves placing the polyimide precursor membrane in a carbonization furnace and performing high-temperature pyrolysis in a 500 mL / min Ar atmosphere. The temperature is first raised to 685°C at a heating rate of 3°C / min; then raised to 700°C at a heating rate of 0.25°C / min and held at that temperature for 60 minutes; and finally, naturally cooled to room temperature to obtain the polyimide-based carbon membrane.

[0087] Example 3

[0088] The preparation method of the polyimide-based carbon membrane for CO2 / N2 separation in this embodiment is essentially the same as that in Example 1, except that the final carbonization temperature is different. Specifically, step 4 involves placing the polyimide precursor membrane in a carbonization furnace and performing high-temperature pyrolysis in a 500 mL / min Ar atmosphere. The temperature is first raised to 785°C at a heating rate of 3°C / min; then raised to 800°C at a heating rate of 0.25°C / min and held at that temperature for 60 minutes; and finally, naturally cooled to room temperature to obtain the polyimide-based carbon membrane.

[0089] Figure 12 The infrared spectra of the carbon films prepared in Examples 1 to 3 are shown in FIG. Figure 12 It can be seen that 1311 cm -1 and 1103cm -1 The CF peak at 30° disappears, indicating that during the carbonization process, -CF3 in the polyimide molecular chain decomposes to produce small molecular gas and disappears.

[0090] Example 4

[0091] This embodiment provides a method for preparing a polyimide-based carbon membrane for CO2 / N2 separation, comprising the following steps:

[0092] Step 1: Weigh 22.34 g of AB-TFMB (0.04 mol) into a 250 mL three-necked flask. Add 160.44 g of NMP and introduce Ar into the flask. Maintain the reaction temperature at 25°C and stir at 200 rpm for 90 minutes. Then, add 17.77 g of 6FDA (0.040 mol). After the addition of the ingredients, continue the reaction at the same stirring speed and temperature for 24 hours to obtain a transparent, viscous polyamic acid solution.

[0093] Step 2: Add 36 ml of acetic anhydride and 4 ml of 3-methylpyridine to the polyamic acid solution, maintain the reaction temperature at 25° C., and stir at a stirring rate of 300 rpm for 36 hours to obtain a transparent and viscous polyimide solution.

[0094] The polyimide solution was poured into methanol for recrystallization, filtered and dried.

[0095] Step 3: Add the dried polyimide into DMF at 40° C. and stir at a rate of 500 rpm for 48 hours to prepare a polyimide casting solution with a solid content of 8 wt %.

[0096] The polyimide casting liquid was poured into a clean flat-bottomed Petri dish to form a film, and then placed in a vacuum oven and vacuumed and degassed at 30°C for 4 hours; the Petri dish was taken out, transferred to an oven, and dried at a constant temperature of 80°C for 48 hours, and a polyimide precursor film was obtained after natural cooling.

[0097] Step 4: Place the polyimide precursor film in a carbonization furnace and perform high-temperature pyrolysis in a 500 mL / min Ar atmosphere. First, heat the film to 785°C at a rate of 3°C / min; then increase the temperature to 800°C at a rate of 0.25°C / min and maintain for 60 minutes. Finally, cool the film naturally to room temperature to obtain the polyimide-based carbon film.

[0098] Example 5

[0099] This embodiment provides a method for preparing a polyimide-based carbon membrane for CO2 / N2 separation, comprising the following steps:

[0100] Step 1. Weigh 7.32 g of 6FAP (2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 0.02 mol) and 11.17 g of AB-TFMB (0.02 mol) into a 250 mL three-necked flask. Add 145.04 g of NMP to the flask and introduce Ar. Maintain the reaction temperature at 25°C and stir at 200 rpm for 90 minutes. Then, add 17.77 g of 6FDA (0.040 mol). After the additions are complete, maintain the stirring speed and temperature and continue the reaction for 24 hours to obtain a transparent, viscous polyamic acid solution.

[0101] Step 2: Add 36 ml of acetic anhydride and 4 ml of 3-methylpyridine to the polyamic acid solution, maintain the reaction temperature at 25° C., and stir at a stirring rate of 500 rpm for 24 hours to obtain a transparent and viscous polyimide solution.

[0102] The polyimide solution was poured into methanol for recrystallization, filtered and dried.

[0103] Step 3: Add the dried polyimide into DMF at 55° C. and stir at 600 rpm for 48 hours to prepare a polyimide casting solution with a solid content of 8 wt %.

[0104] The polyimide casting liquid was poured into a clean flat-bottomed Petri dish to form a film, and then placed in a vacuum oven and vacuumed and degassed at 60°C for 4 hours; the Petri dish was taken out, transferred to an oven, and dried at a constant temperature of 80°C for 48 hours, and a polyimide precursor film was obtained after natural cooling.

[0105] Step 4: Place the polyimide precursor film in a carbonization furnace and perform high-temperature pyrolysis in a 500 mL / min Ar atmosphere. First, heat the film to 785°C at a rate of 3°C / min; then increase the temperature to 800°C at a rate of 0.25°C / min and maintain for 60 minutes. Finally, cool the film naturally to room temperature to obtain the polyimide-based carbon film.

[0106] Example 6

[0107] This embodiment provides a method for preparing a polyimide-based carbon membrane for CO2 / N2 separation, comprising the following steps:

[0108] Step 1. Weigh 7.32 g of 6FAP (2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane, 0.02 mol) and 5.17 g of BAP (0.02 mol) into a 250 mL three-necked flask. Add 101.52 g of NMP to the flask and introduce Ar. Maintain the reaction temperature at 25°C and stir at 200 rpm for 90 minutes. Then, add 12.89 g of BTDA (0.040 mol). After the addition of the ingredients, continue the reaction at the same stirring speed and temperature for 24 hours to obtain a transparent, viscous polyamic acid solution.

[0109] Step 2: Add 36 ml of acetic anhydride and 4 ml of 3-methylpyridine to the polyamic acid solution. Maintain the reaction temperature at 25° C. and stir at 500 rpm for 24 hours to obtain a transparent and viscous polyimide solution.

[0110] The polyimide solution was poured into methanol for recrystallization, filtered and dried.

[0111] Step 3: Add the dried polyimide into DMF at 55° C. and stir at 600 rpm for 48 hours to prepare a polyimide casting solution with a solid content of 8 wt %.

[0112] The polyimide casting liquid was poured into a clean flat-bottomed Petri dish to form a film, and then placed in a vacuum oven and vacuumed and degassed at 60°C for 4 hours; the Petri dish was taken out, transferred to an oven, and dried at a constant temperature of 80°C for 48 hours, and a polyimide precursor film was obtained after natural cooling.

[0113] Step 4: Place the polyimide precursor film in a carbonization furnace and perform high-temperature pyrolysis in a 500 mL / min Ar atmosphere. First, heat the film to 785°C at a rate of 3°C / min; then increase the temperature to 800°C at a rate of 0.25°C / min and maintain for 60 minutes. Finally, cool the film naturally to room temperature to obtain the polyimide-based carbon film.

[0114] Comparative Example 1

[0115] The preparation method of the polyimide-based carbon membrane in this comparative example is basically the same as that in Example 1, except that AB-TFMB is not added in step 1, and all 0.04 mol of diamine monomer is DAM.

[0116] Test example

[0117] 1. The thermal stability of the polyimide precursor film prepared in Example 1 was tested by heating the film from room temperature to 900° C. at a rate of 5° C. / min. The test results are shown in Table 1.

[0118] Table 1 Polyimide precursor film structure and performance parameters

[0119]

[0120] As can be seen from Table 1, the glass transition temperature of the polyimide precursor film of the present invention is 374.8° C., which has high thermal stability; the carbon residue rate at 900° C. is 52.5%, which shows that it is an excellent carbon film precursor.

[0121] 2. The thermal stability of the polyimide-based carbon membranes prepared in Examples 1, 2, and 3 was tested by heating the temperature from room temperature to 900°C at a rate of 5°C / min. The test results are shown in Table 2. Figure 9 .Depend on Figure 9 It can be seen that the polyimide-based carbon membrane of the present invention has high thermal stability.

[0122] 3. XRD test was performed on the polyimide-based carbon films prepared in Examples 1, 2, and 3: the scanning range of 2θ was from 5° to 70°, and the scanning rate was 0.05 s -1 , test results see Figure 8 .Depend on Figure 8 It can be seen that with the increase of carbonization temperature, the interlayer spacing between carbon layers gradually decreases.

[0123] 4. The gas separation performance of the polyimide-based carbon membrane was tested using the constant pressure variable volume method. The test process was as follows: the polyimide-based carbon membrane was installed in a laboratory stainless steel flat membrane module with an effective area of ​​1.77 cm 2 A 10 vol% CO2 / 90 vol% N2 mixture was selected as the feed gas and fed into the membrane permeation system. Argon was used as the purge gas and fed into the permeation line. The feed gas flow rate was controlled at 100 NmL / min, and the purge gas flow rate was controlled at 20 NmL / min. The feed pressure was set to 2 bar. After stabilization for 30 minutes, the test system was ready for measurement. The gas composition on the permeate side was measured by gas chromatography.

[0124] Polyimide-based carbon membrane i Gas permeability P i (Unit is Barrer, 1 Barrer = 1×10 -10 cm 3 (STP) cm cm -2 s -1 cmHg -1 ) is calculated according to formula (1), and CO2 / N2 selectivity is calculated according to formula (2):

[0125] Formula (1)

[0126] Formula (2)

[0127] Among them, Q i for i Gas permeate flow rate, cm 3 (STP) h -1 ; L is the thickness of the polyimide-based carbon membrane, cm; A is the effective area of ​​the membrane, cm 2 ; Δ p i For the feed side and the permeate side i The partial pressure difference of the gases, cmHg. x 、 y The feed side and the permeate side i 、 j The concentrations of the two gases. STP stands for standard temperature and pressure, which is the state of one atmosphere at 0°C.

[0128] The test results are shown in Table 2.

[0129] Table 2 Gas separation performance of polyimide-based carbon membranes

[0130]

[0131] From Table 2 and Figure 11 As can be seen in the figure, the polyimide-based carbon membrane of the present invention has an ultra-high CO2 permeation flux exceeding 6000 barrers. In addition, its gas separation performance far exceeds the latest 2019 upper bound, demonstrating its excellent CO2 capture capacity.

[0132] The gas separation performance of the unpyrolyzed and carbonized polyimide precursor membrane of Example 1 was tested using the above method. Since the polyimide precursor membrane was very dense, the CO2 permeation flux was very low and could not be measured by the testing machine.

[0133] 3. The mechanical properties of polyimide-based carbon film were tested using a nanoindenter. The test results are shown in Figure 10 .Depend on Figure 10 It can be seen that the polyimide-based carbon membrane of the present invention has high mechanical strength, which is conducive to its promotion and application in industry.

[0134] Obviously, the above embodiments are merely examples for clarity of explanation and are not intended to limit the implementation methods. Those skilled in the art will appreciate that other variations or modifications can be made based on the above description. It is not necessary and impossible to enumerate all implementation methods here. Obvious variations or modifications arising therefrom remain within the scope of protection of the present invention.

Claims

1. A method for preparing a polyimide-based carbon membrane for CO2 / N2 separation, characterized in that: The following steps are involved: Step 1, mixing a diamine monomer, a dianhydride monomer and an organic solvent to obtain a mixed solution, and reacting to obtain a polyamic acid solution; Step 2, mixing the polyamic acid solution with a dehydrating agent and a catalyst, and reacting to obtain polyimide; Step 3, preparing a polyimide precursor film using the polyimide prepared in step 2; Step 4, pyrolyzing the polyimide precursor film to obtain a polyimide-based carbon film; The diamine monomer is a combination of 2,4,6-trimethyl-1,3-phenylenediamine and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide); or The diamine monomer is N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide); or The diamine monomer is a combination of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide); The dianhydride monomer is hexafluorodianhydride; The pyrolysis comprises: firstly heating from room temperature to 15°C below the final temperature at a rate of 2-5°C / min, then heating to a final temperature of 600-800°C at a rate of 0.25-1°C / min, and keeping the temperature for 30-150min; The reaction temperature in step 1 is 0-30°C, and the reaction temperature in step 2 is 0-30°C.

2. The method for preparing a polyimide-based carbon membrane for CO2 / N2 separation according to claim 1, characterized in that: The step 1 satisfies at least one of the following conditions: (1) The molar ratio of the diamine monomer to the dianhydride monomer is 1:(1-1.05); (2) The solid content of the mixed solution is 10-30 wt%; (3) The reaction time in step 1 is 24 to 48 hours; (4) Continue stirring during the reaction in step 1.

3. The method for preparing a polyimide-based carbon membrane for CO2 / N2 separation according to claim 1, characterized in that: The step 2 satisfies at least one of the following conditions: (1) The dehydrating agent includes at least one of trifluoroacetic anhydride, acetic anhydride, acetyl chloride, thionyl chloride and dicyclohexylcarbocyanine; (2) The catalyst comprises at least one of pyridine, triethylamine and 3-methylpyridine; (3) The volume amount of the dehydrating agent is 880 to 950 times the total molar amount of the diamine monomer, wherein the volume unit is ml and the molar amount unit is mol; (4) The volume amount of the catalyst is 90 to 120 times the total molar amount of the diamine monomer, where the volume unit is ml and the molar amount unit is mol; (5) The reaction time in step 2 is 24 to 48 hours; (6) Continue stirring during the reaction in step 2.

4. The method for preparing a polyimide-based carbon membrane for CO2 / N2 separation according to claim 1 or 2, characterized in that: The step 4 is to perform pyrolysis in an argon atmosphere.

5. The method for preparing a polyimide-based carbon membrane for CO2 / N2 separation according to claim 1, characterized in that: The diamine monomer is a combination of 2,4,6-trimethyl-1,3-phenylenediamine and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide), and the molar ratio of 2,4,6-trimethyl-1,3-phenylenediamine to N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide) is 3:2~1:

1.

6. The method for preparing a polyimide-based carbon membrane for CO2 / N2 separation according to claim 1, characterized in that: The diamine monomer is a combination of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane and N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide), and the molar ratio of 2,2-bis(3-amino-4-hydroxyphenyl)hexafluoropropane to N,N'-(2,2'-bis(trifluoromethyl)-[1,1'-biphenyl]-4,4'-diyl)bis(4-aminobenzamide) is 3:2-1:

1.

7. A polyimide-based carbon membrane for CO2 / N2 separation, characterized in that: It is prepared according to the method for preparing a polyimide-based carbon membrane for CO2 / N2 separation according to any one of claims 1-6.