Flame-retardant low-melting-point polyester and preparation method and application thereof
By using methylpropylene glycol, terephthalic acid and DOPO-based phosphorus-based flame retardants in low-melting polyester for esterification and polycondensation reactions, combined with titanium-based catalysts, the melting point of polyester was successfully reduced and the flame-retardant properties were improved. It solves the problems of high melting point and insufficient flame retardant performance in the existing technology, expands the application scope and simplifies the preparation process.
Patent Information
- Application Number
- CN202410840410.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-06-27
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-06-27
AI Technical Summary
The melting point of existing low-melting point polyester is relatively high, which limits its application in fields with high flame retardant requirements, and it is difficult to effectively reduce the melting temperature while maintaining good flame retardant properties with existing technology.
Methyl propylene glycol, terephthalic acid and DOPO phosphorus-based flame retardants are used to perform esterification and polycondensation reactions, catalyzed by titanium-based catalysts, and reaction conditions are controlled to produce low-melting polyester with a melting point below 100°C.
It achieves a significant reduction in melting temperature and improvement in flame retardant properties, expands the application scope of polyester, and simplifies the preparation process, making it suitable for industrial applications.
Smart Images

Figure SMS_3 
Figure QLYQS_1
Abstract
Description
Technical Field
[0001] The invention relates to a flame-retardant low-melting-point polyester and a preparation method and application thereof, belonging to the technical field of new polymer materials. Background Art
[0002] Low melting point PET copolyester is a new functional PET polyester developed in recent years. It is a new type of PET copolyester prepared by copolymerization of single or multiple modified components. This PET copolyester has the characteristics of low crystallinity, low glass transition temperature and low melting point. It can meet the special requirements of some products used in specific scenarios. It is a green and environmentally friendly product that can replace traditional adhesives. It is mainly used in non-woven fabrics, filter screens, clothing interlinings, sofa fabrics, mattresses, automotive interior materials, bonded lines, thermal insulation sheets, shoe upper materials and other fields.
[0003] Due to the inherent flammability of polyester, the application of low-melting point polyester is limited in some fields with relatively high flame retardant requirements. Therefore, it is very necessary to develop a highly flame retardant and low-melting point polyester. According to the existing data, the melting temperature of low-melting point polyester is above 100°C, which limits its scope of use to a certain extent. For example, Chinese patent application CN115896976A discloses a regenerated low-melting polyester composite fiber with flame retardant function and a preparation method thereof, wherein the regenerated low-melting polyester with flame retardant function is composed of a terephthalic acid segment, an isophthalic acid segment, an ethylene glycol segment, a 2-methyl-1,3-propylene glycol segment, a diethylene glycol segment and a flame retardant segment; the flame retardant corresponding to the flame retardant segment is a diol series, specifically trans-cyclohexanediol isobutyl cage silsesquioxane, 1,2-propylene glycol isobutyl cage silsesquioxane, TMP dihydroxy isobutyl cage silsesquioxane or disilanol isobutyl cage silsesquioxane; however, the softening point of the low-melting polyester prepared by this patent is 120-150°C. Chinese patent application CN106757444A discloses a low melting point polyester fiber and a preparation method thereof, wherein the low melting point polyester is composed of terephthalic acid segments, isophthalic acid segments, ethylene glycol segments, diethylene glycol segments and molecular weight regulator end-capping groups, and the molecular weight distribution of the polymer is broadened by adding a molecular weight regulator, so that the flow temperature of the polyester melt is reduced, thereby improving the melting performance of the low melting point polyester, and the melting point of the low melting point polyester is between 100° C. and 180° C. It can be seen that the melting point of the polyester prepared in these prior arts is still relatively high.
[0004] Therefore, developing a flame-retardant low-melting point polyester and a preparation method thereof can effectively expand the application scope of polyester. Summary of the invention
[0005] The present invention aims at the deficiencies in the prior art and provides a flame-retardant low-melting polyester and a preparation method and application thereof. The flame-retardant low-melting polyester has a melting point of below 100°C and excellent flame retardant performance, and the preparation method is simple and suitable for industrial application.
[0006] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing a flame-retardant low-melting polyester, the preparation method comprising: using methyl propylene glycol, terephthalic acid and DOPO-type phosphorus flame retardant as raw materials, carrying out esterification reaction and polycondensation reaction to obtain the low-melting polyester.
[0007] Furthermore, the DOPO type phosphorus flame retardant is: .
[0008] Furthermore, the esterification reaction and polycondensation reaction are carried out under the action of a catalyst, and the catalyst is a titanium-based catalyst.
[0009] Furthermore, the catalyst is one or more of tetrabutyl titanate, tetraethyl titanate, tetra-n-propyl titanate, tetraisopropyl titanate or tetraisooctyl titanate.
[0010] Furthermore, the amount of the catalyst is 0.01-0.5% of the total mass of the terephthalic acid and DOPO phosphorus flame retardant powders;
[0011] During the esterification reaction, the amount of the catalyst added is 40% to 60% of the total amount of the catalyst;
[0012] During the polycondensation reaction, the amount of the catalyst added is 40% to 60% of the total amount of the catalyst.
[0013] Further, the molar ratio of the total moles of the terephthalic acid and DOPO-based phosphorus flame retardant to the methylpropylene glycol is 1:(1.2-1.8);
[0014] The molar ratio of the terephthalic acid to the DOPO type phosphorus flame retardant is 1:(0.012-0.085).
[0015] Furthermore, the temperature of the esterification reaction is 230-240° C., and the pressure of the esterification reaction is 240-260 KPa.
[0016] Furthermore, the temperature of the polycondensation reaction is 260-280° C., the system pressure of the polycondensation reaction is below 100 Pa, and the time of the polycondensation reaction is 160-200 min.
[0017] The invention also discloses a flame retardant low-melting polyester, which is prepared by the preparation method of the invention.
[0018] The invention also discloses an application of flame-retardant low-melting polyester, wherein the low-melting polyester is applied to the technical fields of non-woven fabrics, filter screens, clothing adhesive linings, sofa fabrics, mattresses, automobile interior materials, bonded yarns, thermal insulation flakes, and shoe upper materials.
[0019] The beneficial effects of the present invention are:
[0020] The preparation method of the present invention uses methylpropanediol, terephthalic acid and DOPO phosphorus flame retardant as raw materials. The polyester prepared by esterification reaction and polycondensation reaction has a lower melting temperature (melting temperature is below 100°C) and good flame retardant performance (LOI can reach 33%), which can effectively expand the application field of polyester. The polyester has a lower melting temperature, so it has more convenient processing performance and is more convenient to use in the application process of non-woven fabrics, filter screens, clothing adhesive linings, sofa fabrics, mattresses, automotive interior materials, Bondi lines, thermal insulation flakes, shoe upper materials and other technical fields.
[0021] In the preparation method of the present invention, the methyl group on the side chain of the methyl propanediol participating in the reaction is an asymmetric structure, which will disrupt the regularity of the polymer chain during the polymerization process, making the polyester difficult to crystallize and the molecular chain easier to move, so the required melting temperature is much lower than that of normal polyester; after adding the flame retardant, since the side chain of the DOPO phosphorus-based flame retardant increases the steric hindrance effect, the internal repulsive force is further increased, and the required melting temperature will be further reduced. Therefore, the polyester prepared by the preparation method of the present invention has a lower melting point temperature and better flame retardant properties.
[0022] The raw materials used in the preparation method of the present invention can all be purchased on the market, the operation process is simple, the required equipment is of the same type as the current conventional polyester preparation equipment and does not require modification, so it is very suitable for industrial application. DETAILED DESCRIPTION
[0023] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0024] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0025] A method for preparing flame-retardant low-melting polyester comprises the following steps: using methyl propylene glycol, terephthalic acid and DOPO phosphorus flame retardant as raw materials, carrying out esterification reaction and polycondensation reaction to obtain the low-melting polyester.
[0026] Specifically, the DOPO type phosphorus flame retardant is: .
[0027] Specifically, the esterification reaction and polycondensation reaction are carried out under the action of a catalyst, and the catalyst is a titanium-based catalyst.
[0028] Specifically, the catalyst is one or more of tetrabutyl titanate, tetraethyl titanate, tetra-n-propyl titanate, tetraisopropyl titanate or tetraisooctyl titanate.
[0029] Specifically, the amount of the catalyst is 0.01-0.5% of the total mass of the terephthalic acid and DOPO phosphorus flame retardant powders;
[0030] During the esterification reaction, the amount of the catalyst added is 40% to 60% of the total amount of the catalyst;
[0031] During the polycondensation reaction, the amount of the catalyst added is 40% to 60% of the total amount of the catalyst.
[0032] Because the esterification process will produce water, water will cause the titanium catalyst to hydrolyze. If all the catalysts used in the entire preparation process are added in the esterification reaction, the catalyst may be hydrolyzed, resulting in insufficient catalyst for the polycondensation reaction. Therefore, adding the catalyst in batches is more conducive to ensuring the smooth progress of the esterification reaction and the polycondensation reaction.
[0033] Specifically, the molar ratio of the total molar number of the terephthalic acid and the DOPO type phosphorus flame retardant to the methyl propylene glycol is 1: (1.2-1.8);
[0034] The molar ratio of the terephthalic acid to the DOPO type phosphorus flame retardant is 1:(0.012-0.085).
[0035] Specifically, the temperature of the esterification reaction is 230-240° C., and the pressure of the esterification reaction is 240-260 KPa.
[0036] Specifically, the temperature of the polycondensation reaction is 260-280° C., the system pressure of the polycondensation reaction is below 100 Pa, and the time of the polycondensation reaction is 160-200 min.
[0037] More specifically, in the embodiment of the present invention, a 20L polymerization reactor is used to prepare polyester, and the preparation process is a two-reactor process: the first reactor is an esterification reactor, and the second reactor is a polycondensation reactor; after the esterification reaction is completed, the material is transferred to the polycondensation reactor for reaction. The specific preparation process is as follows:
[0038] (1) Beating
[0039] Open the polymerization reactor and replace the air in the reactor with nitrogen. Then add appropriate amounts of terephthalic acid, methyl propylene glycol, DOPO-type phosphorus flame retardant and catalyst into the polymerization reactor. After stirring for ten minutes, the materials are evenly mixed and wait for the next reaction.
[0040] (2) Esterification reaction
[0041] The initial reaction pressure is set to 100KPa, the reaction temperature is 230-240℃, and the esterification reaction pressure is controlled to be 240-260KPa. During the reaction, the water in the reaction system is separated by a distillation tower. When the esterification water output reaches 80% of the theoretical value, the pressure is slowly reduced until it drops to normal pressure. When the water output is no higher than 95% of the theoretical value, the esterification reaction is considered to be completed. In the specific implementation process, it is found that the esterification reaction time is 120-160min (the esterification time is the time required from the beginning of water output to the end of the esterification reaction).
[0042] (3) Polycondensation reaction
[0043] After the esterification reaction is completed, the material is transferred to a polycondensation reactor, the temperature of the polycondensation reactor is set to 260-280°C, vacuum is slowly evacuated, and high vacuum is maintained for 30 minutes. Finally, the pressure of the reactor is maintained below 100 Pa, and the reaction is stirred for 160-200 minutes. The material is discharged when the stirring torque increases to 7N.m-30N.m (15Hz) to obtain the melting point polyester.
[0044] More specifically, a heat stabilizer is added during the polycondensation reaction, and the heat stabilizer is any one of trimethyl phosphite, triphenyl phosphate, and triphenyl phosphite.
[0045] Example 1
[0046] A method for preparing a flame-retardant low-melting polyester, the preparation method comprising:
[0047] 3900 g of terephthalic acid, 100 g of DOPO-based phosphorus flame retardant, and 2568 g of methyl propylene glycol were added into a polymerization reactor that had been substituted with nitrogen, and then 0.2 g of tetraethyl titanate catalyst was added and stirred evenly.
[0048] Nitrogen was introduced into the polymerization reactor, the initial pressure was set to 100 kPa, the esterification reaction temperature was 230 °C, the pressure of the esterification reaction was controlled to 260 kPa, and the water output of the esterification reaction was recorded. When the water output reached 80% of the theoretical value, the pressure was slowly reduced. When the water output reached 95% of the theoretical value, the esterification reaction was completed. The esterification reaction time was recorded as 160 min.
[0049] Then the material is transferred to a polycondensation reactor, and 2 g of a heat stabilizer trimethyl phosphite is added, and then 0.2 g of a catalyst tetraethyl titanate is added, the polycondensation reaction temperature is set to 260°C, and vacuuming is started slowly. After about 30 minutes, the polycondensation reactor is kept in a high vacuum state, the reactor pressure is set to less than 100 Pa, and the low-melting point polyester is obtained after 200 minutes of reaction.
[0050] Example 2
[0051] A method for preparing a flame-retardant low-melting polyester, the preparation method comprising:
[0052] 3800 g of terephthalic acid, 200 g of DOPO type phosphorus flame retardant, and 3802 g of methyl propylene glycol were added into a polymerization reactor which had been replaced with nitrogen, and then 8 g of tetrabutyl titanate catalyst was added and stirred evenly.
[0053] Nitrogen was introduced into the polymerization reactor, the initial pressure was set to 100 kPa, the esterification reaction temperature was 240 °C, the pressure of the esterification reaction was controlled to 240 kPa, and the water output of the esterification reaction was recorded. When the water output reached 80% of the theoretical value, the pressure was slowly reduced. When the water output reached 95% of the theoretical value, the esterification reaction was completed. The esterification reaction time was recorded as 120 min.
[0054] Then the material is transferred to a polycondensation reactor, and 2 g of triphenyl phosphate as a heat stabilizer is added, and then 12 g of tetrabutyl titanate as a catalyst is added, the polycondensation reaction temperature is set to 280°C, and vacuuming is started slowly. After about 30 minutes, the polycondensation reactor is kept in a high vacuum state, the reactor pressure is set to less than 100 Pa, and the low-melting point polyester is obtained after 160 minutes of reaction.
[0055] Example 3
[0056] A method for preparing a flame-retardant low-melting polyester, the preparation method comprising:
[0057] 3600 g of terephthalic acid, 400 g of DOPO-based phosphorus flame retardant, and 2673 g of methyl propylene glycol were added into a polymerization reactor that had been substituted with nitrogen, and then 0.48 g of tetrabutyl titanate catalyst was added and stirred evenly.
[0058] Nitrogen was introduced into the polymerization reactor, the initial pressure was set to 100 kPa, the esterification reaction temperature was set to 240 °C, and the pressure of the esterification reaction was controlled to 250 kPa; the water output of the esterification reaction was recorded, and when the water output reached 80% of the theoretical value, the pressure was slowly reduced, and when the water output reached 95% of the theoretical value, the esterification reaction was completed, and the esterification reaction time was recorded as 150 min.
[0059] Then the material was transferred to a polycondensation reactor, and 2 g of triphenyl phosphite as a heat stabilizer was added, and 0.32 g of tetrabutyl titanate as a catalyst was added. The polycondensation reaction temperature was set to 275°C, and vacuum was slowly drawn. After about 30 minutes, the polycondensation reactor was kept in a high vacuum state, and the reactor pressure was set to less than 100 Pa. After 180 minutes of reaction, the material was discharged to obtain the low-melting point polyester.
[0060] Example 4
[0061] A method for preparing a flame-retardant low-melting polyester, the preparation method comprising:
[0062] 3400 g of terephthalic acid, 600 g of DOPO-based phosphorus flame retardant, and 2599 g of methyl propylene glycol were added into a polymerization reactor that had been replaced with nitrogen, and then 0.4 g of tetrabutyl titanate catalyst was added and stirred evenly.
[0063] Nitrogen was introduced into the polymerization reactor, the initial pressure was set to 100 kPa, the esterification reaction temperature was 240 °C, and the pressure of the esterification reaction was controlled to 260 kPa; the water output of the esterification reaction was recorded, and when the water output reached 80% of the theoretical value, the pressure was slowly reduced, and when the water output reached 95% of the theoretical value, the esterification reaction was completed, and the esterification reaction time was recorded as 150 min.
[0064] Then the material is transferred to a polycondensation reactor, and 2 g of triphenyl phosphite as a heat stabilizer is added, and then 0.4 g of tetrabutyl titanate as a catalyst is added, the polycondensation reaction temperature is set to 270°C, and vacuuming is started slowly. After about 30 minutes, the polycondensation reactor is kept in a high vacuum state, the reactor pressure is set to less than 100 Pa, and the low-melting point polyester is obtained after 180 minutes of reaction.
[0065] Comparative Example 1
[0066] The polyester was prepared by the same method as in Example 4, except that the dosage ratio of the DOPO type phosphorus flame retardant was increased. The specific preparation process is as follows:
[0067] 3200 g of terephthalic acid, 800 g of DOPO-based phosphorus flame retardant, and 2599 g of methyl propylene glycol were added into a polymerization reactor that had been replaced with nitrogen, and then 0.4 g of tetrabutyl titanate catalyst was added and stirred evenly.
[0068] Nitrogen was introduced into the polymerization reactor, the initial pressure was set to 100 kPa, the esterification reaction temperature was 240 °C, and the pressure of the esterification reaction was controlled to 260 kPa; the water output of the esterification reaction was recorded, and when the water output reached 80% of the theoretical value, the pressure was slowly reduced, and when the water output reached 95% of the theoretical value, the esterification reaction was completed, and the esterification reaction time was recorded as 150 min.
[0069] Then the material was transferred to the polycondensation reactor, and 2g of triphenyl phosphite as a heat stabilizer was added, and then 0.4g of catalyst was added. The polycondensation reaction temperature was set to 270°C, and vacuum was slowly drawn. After about 30 minutes, the polycondensation reactor was kept in a high vacuum state, the reactor pressure was set to less than 100 Pa, and the material was discharged after 180 minutes of reaction.
[0070] Comparative Example 2
[0071] The polyester was prepared by the same method as in Example 4, except that no DOPO type phosphorus flame retardant was added. The specific preparation process is as follows:
[0072] 4000 g of terephthalic acid and 2599 g of methyl propylene glycol were added into a polymerization reaction kettle which had been replaced with nitrogen, and then 0.4 g of tetrabutyl titanate catalyst was added and stirred evenly.
[0073] Nitrogen was introduced into the polymerization reactor, the initial pressure was set to 100 kPa, the esterification reaction temperature was 240 °C, and the pressure of the esterification reaction was controlled to 260 kPa; the water output of the esterification reaction was recorded, and when the water output reached 80% of the theoretical value, the pressure was slowly reduced, and when the water output reached 95% of the theoretical value, the esterification reaction was completed, and the esterification reaction time was recorded as 150 min.
[0074] Then the material was transferred to the polycondensation reactor, and 2g of triphenyl phosphite as a heat stabilizer was added, and 0.4g of tetrabutyl titanate as a catalyst was added. The polycondensation reaction temperature was set to 270°C, and vacuum was slowly drawn. After about 30 minutes, the polycondensation reactor was kept in a high vacuum state, the reactor pressure was set to less than 100 Pa, and the material was discharged after 180 minutes of reaction.
[0075] Comparative Example 3
[0076] The polyester was prepared by the same method as in Example 4, except that the tetrabutyl titanate catalyst was replaced with antimony ethylene glycol. The specific preparation process is as follows:
[0077] 3400 g of terephthalic acid, 600 g of DOPO type phosphorus flame retardant and 2599 g of methyl propylene glycol were added into a polymerization reactor which had been replaced with nitrogen, and then 0.4 g of catalyst antimony ethylene glycol was added and stirred evenly.
[0078] Nitrogen was introduced into the polymerization reactor, the initial pressure was set to 100 kPa, the esterification reaction temperature was 240 °C, and the pressure of the esterification reaction was controlled to 260 kPa; the water output of the esterification reaction was recorded, and when the water output reached 80% of the theoretical value, the pressure was slowly reduced, and when the water output reached 95% of the theoretical value, the esterification reaction was completed, and the esterification reaction time was recorded as 150 min.
[0079] Then the material was transferred to the polycondensation reactor, and 2g of triphenyl phosphite as a heat stabilizer was added, and then 0.4g of ethylene glycol antimony catalyst was added. The polycondensation reaction temperature was set to 270°C, and vacuum was slowly drawn. After about 30 minutes, the polycondensation reactor was kept in a high vacuum state, the reactor pressure was set to less than 100 Pa, and the material was discharged after 180 minutes of reaction.
[0080] Comparative Example 4
[0081] The polyester was prepared by the same method as in Example 4, except that the polycondensation reaction temperature was increased. The polycondensation reaction temperature in this comparative example 4 was 290° C. The specific preparation process was as follows:
[0082] 3400 g of terephthalic acid, 600 g of DOPO-based phosphorus flame retardant, and 2599 g of methyl propylene glycol were added into a polymerization reactor that had been replaced with nitrogen, and then 0.4 g of tetrabutyl titanate catalyst was added and stirred evenly.
[0083] Nitrogen was introduced into the polymerization reactor, and the initial pressure was set to 100 kPa, the esterification reaction temperature was 240 °C, and the esterification reaction pressure was 260 kPa; the water output of the esterification reaction was recorded, and when the water output reached 80% of the theoretical value, the pressure was slowly reduced, and when the water output reached 95% of the theoretical value, the esterification reaction was completed, and the esterification reaction time was recorded as 150 min.
[0084] Then the material was transferred to the polycondensation reactor, and 2g of triphenyl phosphite as a heat stabilizer was added, and 0.4g of tetrabutyl titanate as a catalyst was added. The polycondensation reaction temperature was set to 290°C, and vacuum was slowly drawn. After about 30 minutes, the polycondensation reactor was kept in a high vacuum state, the reactor pressure was set to less than 100 Pa, and the material was discharged after 180 minutes of reaction.
[0085] The polyesters prepared in the above examples and comparative examples were subjected to performance tests, and the test methods involved were:
[0086] (1) Intrinsic viscosity: According to GB / T14190-2017, the viscosity of polyester chips was tested with a ratio of phenol to tetrachloroethane of 1:1 and an Ubbelohde viscometer was used for the test at 25°C.
[0087] (2) Limiting oxygen index (LOI): The limiting oxygen index of polyester was tested in accordance with GB / T2406.2-2009. The specimens were cut into 15 cm long strips and the damaged length of the strips was recorded in the oxygen concentration range of 22%-35%.
[0088] (3) Vertical burning (UL-94): According to ASTM D3801 test standard, sample size is 130 mm × 13 mm × 3 mm.
[0089] (4) Microscopic melting point test: The polyester slices are cut into thin slices and placed under a microscope. The temperature is first quickly raised to 80°C, and then the heating rate is 1°C / min. The melting process of the slices with temperature is observed under the microscope and the melting temperature is recorded.
[0090] The relevant performance test results are shown in Table 1.
[0091] Table 1 Performance test results
[0092]
[0093] Note: In Table 1, t1 is the afterburning time after the first combustion when measuring the vertical combustion performance; t2 is the afterburning time after the second combustion when measuring the vertical combustion performance.
[0094] From the above table data, it can be seen that the intrinsic viscosity of the polyesters prepared by the preparation method of the present invention in Examples 1 to 4 is not less than 0.7 dl / g, the flame retardant effect is relatively good, and the melting temperature is lower than 100° C. Therefore, the polyester prepared by the preparation method of the present invention has a lower melting point temperature and better flame retardant performance.
[0095] From the comparison of the experimental results of Example 4 and Comparative Example 1, it can be seen that if the amount of DOPO-type phosphorus-based flame retardant used is too much, the discharge state is relatively thin, and the tested intrinsic viscosity does not reach the normal resin viscosity. This is because when the content of the added flame retardant is large, the group on the side chain of the flame retardant has a large steric hindrance effect. When the added amount reaches a certain level, it is difficult for the polymer to continue to undergo polymerization reaction under the current existing conditions, resulting in low viscosity and failure to form a qualified product.
[0096] From the comparison of the experimental results of Example 4 and Comparative Example 2, it can be seen that after adding the DOPO type phosphorus-based flame retardant in Example 4, the melting temperature is lower, because the methyl group on the side chain of the methyl propanediol participating in the reaction is an asymmetric structure, which will disrupt the regularity of the polymer chain during the polymerization process, making the polyester difficult to crystallize and the molecular chain easier to move, so the required melting temperature is much lower than that of normal polyester; after adding the flame retardant, since the side chain of the DOPO type phosphorus-based flame retardant increases the steric hindrance effect, the internal repulsive force is further increased, and the required melting temperature will be further reduced. Therefore, under the synergistic effect of methyl propanediol and DOPO type phosphorus-based flame retardant, the polyester prepared by the preparation method of the present invention has a lower melting point temperature and better flame retardant properties.
[0097] From the comparison of the experimental results of Example 4 and Comparative Example 3, it can be seen that if an antimony-based catalyst is used in the preparation process of the polyester, the viscosity of the discharged product cannot meet the requirements of normal products, indicating that the catalytic efficiency of the antimony-based catalyst for the flame-retardant low-melting point polyester is low and it is difficult to meet the polymerization requirements. The use of the titanium-based catalyst of the present invention is more conducive to the production and processing of polyester.
[0098] From the comparison of the experimental results of Example 4 and Comparative Example 4, it can be seen that: if the polymerization reaction temperature is increased, the final polymer viscosity does not meet the normal product requirements, and the polymer color is grayish yellow, indicating that the polymer is degraded at a higher polymerization temperature. This is because in the polymerization reaction at high temperature, the chain growth reaction is accompanied by the degradation of the molecular chain, and as the temperature increases, the degradation reaction occurs violently, resulting in the viscosity failing to meet the normal standard. Therefore, the temperature of the condensation reaction is controlled at 260-280°C, which is more conducive to obtaining qualified products.
[0099] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0100] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A method for preparing a flame retardant low melting point polyester, It is characterized in that The preparation method comprises: using methyl propylene glycol, terephthalic acid and DOPO type phosphorus flame retardant as raw materials, carrying out esterification reaction and polycondensation reaction to obtain the low melting point polyester; the DOPO type phosphorus flame retardant is: ; The esterification reaction and polycondensation reaction are carried out under the action of a catalyst, and the catalyst is a titanium-based catalyst; The molar ratio of the total molar number of the terephthalic acid and the DOPO type phosphorus flame retardant to the methyl propylene glycol is 1: (1.2-1.8); The molar ratio of terephthalic acid to DOPO phosphorus flame retardant is 1: (0.012-0.085); The temperature of the polycondensation reaction is 260-280° C., the system pressure of the polycondensation reaction is below 100 Pa, and the time of the polycondensation reaction is 160-200 min.
2. A method for preparing a flame retardant low melting point polyester according to claim 1, It is characterized in that The catalyst is one or more of tetrabutyl titanate, tetraethyl titanate, tetra-n-propyl titanate, tetraisopropyl titanate or tetraisooctyl titanate.
3. A method for preparing a flame retardant low melting point polyester according to claim 1, It is characterized in that The amount of the catalyst is 0.01-0.5% of the total mass of the terephthalic acid and DOPO phosphorus flame retardant powders; During the esterification reaction, the amount of the catalyst added is 40% to 60% of the total amount of the catalyst; During the polycondensation reaction, the amount of the catalyst added is 40% to 60% of the total amount of the catalyst.
4. A method for preparing a flame retardant low melting point polyester according to claim 1, It is characterized in that The temperature of the esterification reaction is 230-240° C., and the pressure of the esterification reaction is 240-260 KPa.
5. A flame retardant low melting point polyester, It is characterized in that The low melting point polyester is prepared according to the preparation method according to any one of claims 1 to 4.
6. Use of a flame retardant low melting point polyester according to claim 5, It is characterized in that The low melting point polyester is applied to the technical fields of non-woven fabrics, filter screens, clothing adhesive linings, sofa fabrics, mattresses, automotive interior materials, bonded yarns, thermal insulation flakes, and shoe upper materials.