A chlorinated paraffin / graphene composite material and its preparation method and application

By loading chlorinated paraffin on the surface of graphene and utilizing the alkylation reaction of octa(aminophenyltrioxysilane) and the layered structure of graphene, the thermal stability and corrosion of chlorinated paraffin during extreme pressure friction are solved. problem, improves extreme pressure anti-wear performance and thermal stability, and reduces the risk of metal corrosion.

CN118389193BActive Publication Date: 2024-10-01ANHUI XINGXIN MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410290658.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-03-14
Publication Date
2024-10-01
Estimated Expiration
2044-03-14

AI Technical Summary

Technical Problem

Chlorinated paraffin has poor thermal stability during extreme pressure friction, causing metal surface corrosion, and its anti-wear and extreme pressure properties need to be improved.

Method used

Graphene and chlorinated paraffin are connected through octa(aminophenyltrioxysilane), so that the chlorinated paraffin is loaded on the surface of graphene. The alkylation reaction is used to improve the thermal stability of the chlorinated paraffin, and through the layering of graphene The structure and extreme pressure anti-wear effect of chlorinated paraffin enhance the extreme pressure anti-wear performance, while improving the dispersion of graphene and preventing HCl corrosion.

Benefits of technology

Significantly improves the extreme pressure anti-wear performance and thermal stability of chlorinated paraffin/graphene composite materials, reduces corrosion of metals, enhances dispersion in base oil, and effectively prevents corrosion of metals by HCl.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004740584420000051
    Figure BDA0004740584420000051
  • Figure BDA0004740584420000061
    Figure BDA0004740584420000061
Patent Text Reader

Abstract

The present invention discloses a chlorinated paraffin / graphene composite material, comprising: connecting graphene and chlorinated paraffin through octa(aminophenyltrioxysilane) so that the chlorinated paraffin is loaded on the surface of the graphene. The present invention also discloses a method for preparing the above-mentioned chlorinated paraffin / graphene composite material, comprising the following steps: S1, mixing octa(aminophenyltrioxysilane), a catalyst, an acid binding agent, and an organic solvent, adding chlorinated paraffin, reacting to obtain an intermediate; S2, mixing the intermediate with a dispersion of graphite oxide, heating and reacting to obtain a chlorinated paraffin / graphene composite material. The present invention also discloses the application of the above-mentioned chlorinated paraffin / graphene composite material in an extreme pressure anti-wear agent. The present invention also discloses a lubricating oil. The present invention has good extreme pressure and anti-wear properties, good thermal stability, and low corrosion to metals.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of chlorinated paraffin, and in particular to a chlorinated paraffin / graphene composite material and a preparation method and application thereof. Background Art

[0002] Chlorinated paraffin is an organic substance, a chlorinated derivative of paraffin hydrocarbons. It has the advantages of low volatility, flame retardancy, good electrical insulation, and low price. It can be used as an extreme pressure anti-wear agent, flame retardant, and auxiliary plasticizer for polyvinyl chloride.

[0003] The chlorine atoms on chlorinated paraffin are most active when they are at the end of aliphatic hydrocarbons, and have the best extreme pressure and anti-wear properties; when the chlorine atoms are in the middle of the carbon chain, they are less active. When chlorinated paraffin is used as an extreme pressure and anti-wear agent, the C-Cl chemical bond breaks to generate chlorine atoms or HCl, which react with the metal surface of the friction pair to form a FeCl2 or FeCl3 protective film, showing anti-wear and extreme pressure effects. Because a lot of heat is generated during extreme pressure friction, and chlorinated paraffin has poor thermal stability, a large amount of HCl will be generated at high temperatures, which can easily cause large-scale corrosion on the metal surface, and the anti-wear and extreme pressure properties of chlorinated paraffin still need to be improved. Summary of the invention

[0004] Based on the technical problems existing in the background technology, the present invention proposes a chlorinated paraffin / graphene composite material, which has good extreme pressure and anti-wear properties, good thermal stability, and low corrosion to metals.

[0005] The invention provides a chlorinated paraffin / graphene composite material, which comprises: connecting graphene and chlorinated paraffin through octa(aminophenyltrioxysilane) so that the chlorinated paraffin is loaded on the surface of the graphene.

[0006] Preferably, the chlorine content of the chlorinated paraffin is 42-52 wt%.

[0007] The average molecular weight of chlorinated paraffin-42 is 594.81, and the average molecular weight of chlorinated paraffin-52 is 419.09.

[0008] The present invention also provides a method for preparing the above-mentioned chlorinated paraffin / graphene composite material, comprising the following steps:

[0009] S1, octa(aminophenyltrioxysilane), a catalyst, an acid-binding agent, and an organic solvent are mixed, and chlorinated paraffin is added to react to obtain an intermediate;

[0010] S2. Evenly mix the intermediate and the dispersion of graphite oxide, and heat to react to obtain a chlorinated paraffin / graphene composite material.

[0011] The present invention uses the amino group on octa(aminophenyltrioxysilane) to react with some C-Cl bonds on chlorinated paraffin to undergo an alkylation reaction, connects octa(aminophenyltrioxysilane) to the chlorinated paraffin, improves the thermal stability of the chlorinated paraffin, and reduces the active Cl on the chlorinated paraffin, thereby avoiding the generation of a large amount of HCl during extreme pressure friction, thereby avoiding corrosion of the metal;

[0012] In addition, the remaining amino groups on octa(aminophenyltrioxysilane) react with active groups (such as carboxyl, epoxy, etc.) on graphene oxide, thereby loading octa(aminophenyltrioxysilane) and chlorinated paraffin on the graphene surface; octa(aminophenyltrioxysilane) is a nanoparticle and is approximately cage-shaped, which can achieve rolling friction, and combined with the layered structure of graphene and the extreme pressure and anti-wear effect of chlorinated paraffin, its extreme pressure and anti-wear performance can be greatly improved; and the dispersibility of graphene in base oil can be improved, and the introduction of graphene can further prevent HCl from corroding metals.

[0013] Preferably, in S1, the acid binding agent is pyridine.

[0014] Preferably, in S1, the organic solvent is tetrahydrofuran.

[0015] Preferably, in S1, the catalyst is benzyltriethylammonium chloride.

[0016] Preferably, in S1, the molar ratio of octa(aminophenyltrioxysilane) to chlorinated paraffin is 1:1-2.

[0017] Preferably, in S1, the molar ratio of chlorinated paraffin to acid binding agent is 1:0.4-0.5.

[0018] Preferably, in S1, the molar ratio of chlorinated paraffin to catalyst is 1:0.002-0.003.

[0019] Preferably, in S1, the reflux reaction is carried out for 10-12 hours.

[0020] Preferably, in S2, the weight ratio of the intermediate to graphene oxide is 1:0.5-1.

[0021] Preferably, in S2, the temperature is heated to 50-60°C and the reaction is carried out for 3-4 hours.

[0022] In the above S1, after the reaction is completed, water is added to precipitate, the solid is washed, and dried to obtain an intermediate.

[0023] In the above S2, after the reaction is completed, centrifugation, washing and drying are performed to obtain the chlorinated paraffin / graphene composite material.

[0024] The present invention also proposes the application of the chlorinated paraffin / graphene composite material in an extreme pressure anti-wear agent.

[0025] The present invention also proposes a lubricating oil, the raw materials of which include: base oil and extreme pressure anti-wear agent, wherein the extreme pressure anti-wear agent is the above-mentioned chlorinated paraffin / graphene composite material.

[0026] Preferably, the content of the extreme pressure antiwear agent is 1-1.5 wt %.

[0027] The above-mentioned base oil may be base oil 150N, 500N or the like.

[0028] The lubricating oil may also contain: corrosion inhibitors, antioxidants, rust inhibitors, etc.

[0029] Beneficial effects:

[0030] The present invention loads octa(aminophenyltrioxysilane) and chlorinated paraffin on the surface of graphene, and the three cooperate with each other to greatly improve the extreme pressure and anti-wear performance of the graphene; and can also improve the thermal stability of the chlorinated paraffin, improve the dispersibility of the graphene in the base oil, and reduce the corrosion of the chlorinated paraffin to the metal. DETAILED DESCRIPTION

[0031] The technical solutions of the present invention are described in detail below through specific embodiments. However, it should be clearly stated that these embodiments are for illustration only and are not to be construed as limiting the scope of the present invention.

[0032] Example 1

[0033] A chlorinated paraffin / graphene composite material comprises: connecting graphene and chlorinated paraffin via octa(aminophenyltrioxysilane) so that the chlorinated paraffin is loaded on the surface of the graphene.

[0034] The preparation method of the above-mentioned chlorinated paraffin / graphene composite material comprises the following steps:

[0035] S1. Mix 1mmol of octa(aminophenyltrioxysilane), 0.003mmol of benzyltriethylammonium chloride, 0.5mmol of pyridine and 500ml of tetrahydrofuran, add dropwise 1mmol of chlorinated paraffin with a chlorine content of 52wt% within 30min, reflux for 10h, add water for precipitation, wash the solid, and dry under reduced pressure at 50°C to obtain an intermediate;

[0036] S2. Mix 1 g of the intermediate and 1 g of an ethanol dispersion of graphite oxide, heat to 50° C., stir to react for 4 h, centrifuge, wash the solid, and dry under reduced pressure at 50° C. to obtain a chlorinated paraffin / graphene composite material.

[0037] Example 2

[0038] A chlorinated paraffin / graphene composite material comprises: connecting graphene and chlorinated paraffin via octa(aminophenyltrioxysilane) so that the chlorinated paraffin is loaded on the surface of the graphene.

[0039] The preparation method of the above-mentioned chlorinated paraffin / graphene composite material comprises the following steps:

[0040] S1. Mix 1mmol of octa(aminophenyltrioxysilane), 0.004mmol of benzyltriethylammonium chloride, 0.8mmol of pyridine and 500ml of tetrahydrofuran, add dropwise 2mmol of chlorinated paraffin with a chlorine content of 42wt% within 30min, reflux for 12h, add water for precipitation, wash the solid, and dry under reduced pressure at 50°C to obtain an intermediate;

[0041] S2. Mix 1 g of the intermediate with 0.5 g of an ethanol dispersion of graphite oxide, heat to 60° C., stir to react for 3 h, centrifuge, wash the solid, and dry under reduced pressure at 50° C. to obtain a chlorinated paraffin / graphene composite material.

[0042] Example 3

[0043] A chlorinated paraffin / graphene composite material comprises: connecting graphene and chlorinated paraffin via octa(aminophenyltrioxysilane) so that the chlorinated paraffin is loaded on the surface of the graphene.

[0044] The preparation method of the above-mentioned chlorinated paraffin / graphene composite material comprises the following steps:

[0045] S1. Mix 1mmol of octa(aminophenyltrioxysilane), 0.003mmol of benzyltriethylammonium chloride, 0.6mmol of pyridine and 500ml of tetrahydrofuran, add dropwise 1.5mmol of chlorinated paraffin with a chlorine content of 42wt% within 30min, reflux for 10-12h, add water for precipitation, wash the solid, and dry under reduced pressure at 50°C to obtain an intermediate;

[0046] S2. Mix 1 g of the intermediate with 0.7 g of an ethanol dispersion of graphite oxide, heat to 55° C., stir to react for 3.5 h, centrifuge, wash the solid, and dry under reduced pressure at 50° C. to obtain a chlorinated paraffin / graphene composite material.

[0047] Comparative Example 1

[0048] The invention discloses an extreme pressure anti-wear agent, which is a chlorinated paraffin with a chlorine content of 42 wt%.

[0049] Comparative Example 2

[0050] An extreme pressure anti-wear agent is composed of chlorinated paraffin with a chlorine content of 42wt% and octa(aminophenyltrioxysilane) in a molar ratio of 1.5:1.

[0051] Comparative Example 3

[0052] An extreme pressure anti-wear agent consists of chlorinated paraffin with a chlorine content of 42wt% and graphene oxide in a weight ratio of 1:0.7.

[0053] Comparative Example 4

[0054] An extreme pressure anti-wear agent consists of chlorinated paraffin with a chlorine content of 42wt%, octa(aminophenyltrioxysilane) and graphene oxide, wherein the weight ratio of the total weight of the chlorinated paraffin and octa(aminophenyltrioxysilane) to the graphene oxide is 1:0.7, and the molar ratio of the chlorinated paraffin and octa(aminophenyltrioxysilane) is 1.5:1.

[0055] The products of Examples 1-3 and Comparative Examples 1-4 were used as extreme pressure anti-wear agents to prepare lubricating oils. The raw materials of the lubricating oils were recorded as follows by weight percentage: base oil 150N 99wt%, extreme pressure anti-wear agent 1wt%. The properties of the lubricating oils of each group were tested, and the results are shown in Table 1.

[0056] The friction and wear properties and extreme pressure properties of the oil samples were tested using a four-ball friction tester. Each group of lubricating oil was dripped into the ball-disc contact area and tested according to GB / T12583-1998. The wear spot diameter test conditions were room temperature, a rotation speed of 1450r / min, and a test time of 30min; the friction coefficient test conditions were 500N. All test balls were GCr15 bearing steel balls with a diameter of 12.7mm and a Rockwell hardness of HRC59-61.

[0057] The corrosion resistance of lubricating oil was tested according to SH / T 0195. The storage condition was 100℃ for 8h and the test sample was 45# steel.

[0058] Table 1 Test results

[0059]

[0060]

[0061] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.

Claims

1. An extreme pressure anti-wear agent, characterized in that: The extreme pressure anti-wear agent is a chlorinated paraffin / graphene composite material, which comprises: connecting graphene and chlorinated paraffin through octa(aminophenyltrioxysilane) so that the chlorinated paraffin is loaded on the surface of the graphene; The preparation method of the extreme pressure anti-wear agent comprises the following steps: S1, octa(aminophenyltrioxysilane), a catalyst, an acid-binding agent, and an organic solvent are mixed, chlorinated paraffin is added, and a reflux reaction is performed to obtain an intermediate; S2, mixing the intermediate with an ethanol dispersion of graphite oxide, heating and reacting to obtain a chlorinated paraffin / graphene composite material; In S1, the molar ratio of octa(aminophenyltrioxysilane) to chlorinated paraffin is 1:1-2.

2. The chlorinated paraffin / graphene composite material according to claim 1, characterized in that: The chlorine content of chlorinated paraffin is 42-52 wt%.

3. A method for preparing the extreme pressure anti-wear agent as claimed in claim 1 or 2, characterized in that: The steps include: S1, octa(aminophenyltrioxysilane), a catalyst, an acid-binding agent, and an organic solvent are mixed, chlorinated paraffin is added, and a reflux reaction is performed to obtain an intermediate; S2. Evenly mix the intermediate with an ethanol dispersion of graphite oxide, and heat to react to obtain a chlorinated paraffin / graphene composite material.

4. The method for preparing the extreme pressure anti-wear agent according to claim 3, characterized in that: In S1, the acid binding agent is pyridine.

5. The method for preparing the extreme pressure anti-wear agent according to claim 3, characterized in that: In S1, the organic solvent is tetrahydrofuran.

6. The method for preparing the extreme pressure anti-wear agent according to claim 3, characterized in that: In S1, the catalyst is benzyltriethylammonium chloride.

7. The method for preparing the extreme pressure anti-wear agent according to claim 3, characterized in that: In S1, the molar ratio of chlorinated paraffin to acid binding agent is 1:0.4-0.

5.

8. The method for preparing the extreme pressure anti-wear agent according to claim 3, characterized in that: In S1, the molar ratio of chlorinated paraffin to catalyst is 1:0.002-0.

003.

9. The method for preparing the extreme pressure anti-wear agent according to claim 3, characterized in that: In S1, the reaction is refluxed for 10-12 h.

10. The method for preparing the extreme pressure anti-wear agent according to claim 3, characterized in that: In S2, the weight ratio of the intermediate to graphene oxide is 1:0.5-1.

11. The method for preparing the extreme pressure anti-wear agent according to claim 3, characterized in that: In S2, heat to 50-60°C and react for 3-4 hours.

12. A lubricating oil, characterized in that: The raw materials include: base oil and the extreme pressure anti-wear agent according to claim 1 or 2.