A method for preparing a blade with uniform coating

By using clamping devices on the metal cutting insert to adjust the position and angle of the blade in the coating furnace, a uniform front and rear cutting surface coating is formed, which solves the problem of uneven coating thickness and improves the cutting performance and wear resistance of the blade sex.

CN118407045BActive Publication Date: 2024-11-22ZHUZHOU CEMENTED CARBIDE CUTTING TOOLS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410860094.3
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-06-28
Publication Date
2024-11-22
Estimated Expiration
2044-06-28

AI Technical Summary

Technical Problem

In the prior art, the coating thickness of the front and back of the metal cutting inserts is uneven, resulting in the impact of cutting performance and service life.

Method used

The first positioning and clamping device is used to clamp and position the coating blade to be coated, so that the bottom surface of the blade and the horizontal direction of the coating furnace form an angle α, and first a uniform first coating is formed on the front and rear blade surfaces; then a second positioning is used The clamping device forms an angle β in the bottom surface of the blade and the vertical direction of the coating furnace to form a second coating layer to ensure that the thickness of the two coating layers on the front and rear cutting surfaces is basically the same.

Benefits of technology

The coating thickness of the front and rear cutting surfaces is achieved uniformly and uniformly, reducing the tensile stress between the coatings, and improving the cutting performance and wear resistance of the blade.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118407045B_ABST
    Figure CN118407045B_ABST
Patent Text Reader

Abstract

The invention discloses a method for preparing a blade with uniform coating, which comprises the following steps: S1, assembling a blade to be coated onto a first positioning and clamping device; S2, sending the first positioning and clamping device and the blade to be coated into a coating furnace and adjusting them so that the bottom surface of the blade to be coated forms an angle α with the horizontal direction of the coating furnace; S3, starting the coating furnace to complete the preparation of a first coating on the blade to be coated; S4, taking out the first positioning and clamping device and the blade to be coated, cleaning the blade to be coated, and then assembling the blade to be coated onto a second positioning and clamping device; S5, sending the second positioning and clamping device and the blade to be coated into the coating furnace and adjusting them so that the bottom surface of the blade to be coated forms an angle β with the vertical direction of the coating furnace; S6, starting the coating furnace to complete the preparation of the second coating on the blade to be coated, which has the advantages of being stable and reliable, having uniform coating, and being able to significantly improve the cutting performance of the blade.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention mainly relates to the field of metal cutting tool forming, and in particular to a method for preparing a blade with uniform coating. Background Art

[0002] Metal cutting blades made of cemented carbide have large friction during cutting and are prone to built-up edge during cutting. They can only be used in working conditions with low cutting speed parameters and have a short service life. In the prior art, a coating process is usually used on the surface of cemented carbide blades, that is, a certain thickness of refractory compounds such as carbides, nitrides, oxides, etc. are coated to act as a protector, so that the surface of the cutting blade has the characteristics of high hardness, high wear resistance, high heat resistance, and low friction coefficient, and the built-up edge is eliminated, which can greatly improve the cutting performance and service life of the cutting blade.

[0003] However, in actual cutting applications, the amount of wear on the rake face and flank face of the cutting insert is different. Sometimes the rake face wears too much, resulting in the failure of the cutting edge, and sometimes the flank face wears too much, resulting in the failure of the cutting edge. There are two main reasons for the above problems: on the one hand, it is affected by the material properties of the workpiece; on the other hand, it is because the coating thickness on the rake face and flank face of the cutting insert is uneven.

[0004] In the prior art, the operation of preparing blade coating is usually to fix multiple groups of cutting blades using a positioning device, and then transfer the blades to a coating furnace for coating preparation. If it is necessary to prepare a multi-layer coating with different materials for each layer, the practice in the prior art is to change the coating material sprayed by the coating furnace and prepare the coating layer by layer. Since the coating material spray source of the physical coating furnace is located on the side wall of the coating furnace, the spray direction of the coating material is horizontal, and the front blade face and the back blade face of the coated blade are not on the same plane, and the front blade face and the back blade face have different angles with the spray direction of the coating material. When a certain layer of coating is prepared, the coating thickness on the front blade face and the back blade face is obviously uneven. If a multi-layer coating is prepared, the overall coating thickness difference of the front blade face and the back blade face is more obvious when completed, that is, the coating thickness of the front blade face and the back blade face is uneven, thereby affecting the cutting performance of the cutting blade. Summary of the invention

[0005] The technical problem to be solved by the present invention is to overcome the deficiencies of the prior art and provide a method for preparing a blade with a uniform coating which is stable and reliable, has a uniform coating and can significantly improve the cutting performance of the blade.

[0006] In order to solve the above technical problems, the present invention adopts the following technical solutions:

[0007] A method for preparing a blade having a uniform coating comprises the following steps:

[0008] S1, assembling the blade to be coated onto a first positioning and clamping device;

[0009] S2, sending the first positioning clamping device and the blade to be coated into the coating furnace and adjusting them so that the bottom surface of the blade to be coated forms an angle α with the horizontal direction of the coating furnace;

[0010] S3, start the coating furnace to complete the preparation of the first coating on the blade to be coated;

[0011] S4, taking out the first positioning and clamping device and the blade to be coated, cleaning the blade to be coated, and then assembling the blade to be coated onto the second positioning and clamping device;

[0012] S5, sending the second positioning and clamping device and the blade to be coated into the coating furnace and adjusting them so that the bottom surface of the blade to be coated forms an angle β with the vertical direction of the coating furnace;

[0013] S6, starting the coating furnace to complete the preparation of the second coating on the blade to be coated;

[0014] The angle α and the angle β in steps S2 and S5 should satisfy: 0≤α≤30° and 0≤β≤30°, or satisfy: 60°≤α≤90° and 60°≤β≤90°, and should also satisfy: 0.8β≤α≤1.2β.

[0015] As a further improvement of the above technical solution:

[0016] The angle α and the angle β should satisfy: α=0, β=0.

[0017] In the step S4, before cleaning the blade to be coated, the cutting edge of the blade to be coated is subjected to jet treatment, using corundum particles with a particle size of 120 to 150 meshes and a jet time of 1 to 3 minutes.

[0018] In the step S3, a first coating is formed on both the rake face and the flank face of the insert to be coated, and in the step S6, a second coating is formed on both the rake face and the flank face of the insert to be coated.

[0019] The maximum total thickness of the coating on the front cutting edge is Y1, and the maximum total thickness of the coating on the rear cutting edge is Y2, which should satisfy the following: 0≤Y1 -Y2≤1µm.

[0020] The minimum total thickness of the coating on the front cutting edge is Y1', and the minimum total thickness of the coating on the rear cutting edge is Y2', which should satisfy the following conditions: 0≤Y1 -Y1'≤1µm, 0≤Y2-Y2'≤1µm.

[0021] The maximum thickness of the first coating on the front cutting edge is X1, the maximum thickness of the second coating is X2, the maximum thickness of the first coating on the rear cutting edge is X1', the maximum thickness of the second coating is X2', and they should satisfy: 1µm≤X1 - X2≤3µm, 1µm≤X2'- X1'≤3µm.

[0022] The maximum thickness of the first coating on the front cutting edge is X1, the maximum thickness of the second coating is X2, the maximum thickness of the first coating on the rear cutting edge is X1', the maximum thickness of the second coating is X2', and the following should be satisfied: 1µm≤X2 - X1≤3µm, 1µm≤X1'- X2'≤3µm.

[0023] The first positioning and clamping device and / or the second positioning and clamping device comprises a base plate capable of forming an incompletely covered coating on the rear cutting edge and a cover plate capable of forming an incompletely covered coating on the front cutting edge.

[0024] Compared with the prior art, the advantages of the present invention are:

[0025] The method for preparing a blade with uniform coating of the present invention comprises the following steps: using a first positioning and clamping device to clamp and position the blade to be coated, so that the position and angle of the blade to be coated in the coating furnace can be adjusted, so that the bottom surface of the blade to be coated forms an angle α with the horizontal direction of the coating furnace, and firstly, a uniform first coating is formed on the rake face and the flank face. Since the angles between the rake face and the flank face and the horizontal coating spraying direction are different, the thickness of the first coating on the rake face and the flank face is also different (the thickness of the first coating on the rake face is X1, and the thickness of the first coating on the flank face is X1'). Then, using a second positioning and clamping device to clamp and position the blade to be coated, so that the bottom surface of the blade to be coated forms an angle β with the vertical direction of the coating furnace, and a second coating is formed on the rake face and the flank face. The thickness of the second coating alone on the rake face and the flank face is also different (the thickness of the second coating on the rake face is X2, and the thickness of the first coating on the flank face is X2'). Since the angles α and β satisfy: 0≤α≤30° And 0≤β≤30°, or satisfying: 60°≤α≤90° and 60°≤β≤90°, and satisfying 0.8β≤α≤1.2β (that is, the values ​​of α and β are relatively close, which is equivalent to the position interchange of the front cutting edge 11 and the back cutting edge 12 during the two coating preparations), the overall thickness of the two coating layers on the front cutting edge (X1+X2) and the overall thickness of the two coating layers on the back cutting edge (X1'+X2') can be achieved to be basically the same, and because when preparing the first coating, the bottom surface of the blade to be coated and the horizontal direction of the coating furnace have an angle α, the particle density of the same number of coating particles ejected from the coating furnace and deposited on the front cutting edge and the back cutting edge is reduced, and when the first coating thickness reaches the set value, the first coating thickness on the front cutting edge is more uniform, and the first coating thickness on the back cutting edge is also more uniform. Similarly, the second coating thickness on the front cutting edge is more uniform, and the second coating thickness on the back cutting edge is also more uniform. Therefore, the overall coating thickness at various locations on the front cutting edge is more uniform, and the overall coating thickness at various locations on the back cutting edge is also more uniform. This eliminates the problem of uneven coating thickness caused by the different angles between the front cutting edge, the back cutting edge and the coating spraying direction in the prior art. Finally, the coating formed on the front cutting edge is more uniform and stable, and the coating formed on the back cutting edge is also more uniform and stable. At the same time, the coating thickness of the front cutting edge and the back cutting edge can also be kept uniform and consistent. The tensile and compressive stresses between the blade coatings are small, and different coatings can be combined. The prepared blade coating has good impact resistance and wear resistance, thereby improving the cutting performance of the blade. BRIEF DESCRIPTION OF THE DRAWINGS

[0026] Figure 1 is a schematic diagram of a coating device used in the method for preparing a blade with a uniform coating according to the present invention;

[0027] Figure 2 is a schematic diagram of a first positioning and clamping device of the method for preparing a blade with a uniform coating according to the present invention;

[0028] Figure 3 is a schematic diagram of a second positioning and clamping device of the method for preparing a blade with a uniform coating according to the present invention;

[0029] Figure 4 is a schematic diagram of preparing a first coating layer in the method for preparing a blade with a uniform coating layer according to the present invention;

[0030] Figure 5 is a schematic diagram of a first coating (enlarged) prepared by the method for preparing a blade with a uniform coating according to the present invention;

[0031] Figure 6 is a schematic diagram of preparing a second coating layer in the method for preparing a blade with a uniform coating layer according to the present invention;

[0032] Figure 7 is a schematic diagram of a first coating (enlarged) prepared by the method for preparing a blade with a uniform coating according to the present invention;

[0033] Figure 8 It is a schematic diagram of the method for preparing a blade with a uniform coating according to the present invention for preparing a blade with a completely covered coating on the front and rear blade surfaces;

[0034] Fig. 9 yes Figure 8 Enlarged view of point A in the middle;

[0035] Fig.10 It is a schematic diagram of the method for preparing a blade with a uniform coating according to the present invention for preparing a blade with an incomplete coating on the front and rear blade surfaces;

[0036] Fig.11 The present invention is a schematic diagram of a base plate and a cover plate of a coating device used in the method for preparing a blade with a uniform coating.

[0037] The symbols in the figure represent:

[0038] 1. Blade to be coated; 11. Rake face; 12. Flank face; 13. Blade bottom surface; 2. First positioning and clamping device; 3. Second positioning and clamping device; 51. First coating layer; 52. Second coating layer; 6. Chassis; 61. Side recess; 7. Cover plate; 71. Top recess; 8. Coating furnace; 81. Side wall of coating furnace. DETAILED DESCRIPTION

[0039] The present invention will be further described in detail below with reference to the accompanying drawings and specific embodiments.

[0040] In the description of the present invention, it should be noted that terms such as "center", "up", "down", "horizontal", "inside", "outside", "top", and "bottom" indicating directions or positional relationships are based on the directions or positional relationships shown in the accompanying drawings. They are only for the convenience of describing the present invention and simplifying the description, and do not indicate or imply that the device or element referred to must have a specific direction, be constructed and operated in a specific direction. Therefore, they should not be understood as limitations on the present invention.

[0041] Figures 1 to 11 The coating device used in the method for preparing a blade with a uniform coating of the present invention is shown. The device mainly includes a coating furnace 8, a first positioning and clamping device 2 and a second positioning and clamping device 3. The method for preparing a blade with a uniform coating of the present invention includes the following steps:

[0042] S1, assembling the blade to be coated 1 onto the first positioning and clamping device 2;

[0043] S2, sending the first positioning and clamping device 2 and the blade to be coated 1 into the coating furnace and adjusting them so that the blade bottom surface 13 of the blade to be coated 1 forms an angle α with the horizontal direction of the coating furnace;

[0044] S3, start the coating furnace to complete the preparation of the first coating 51 of the blade to be coated 1;

[0045] S4, taking out the first positioning and clamping device 2 and the blade to be coated 1, cleaning the blade to be coated 1, and then assembling the blade to be coated 1 onto the second positioning and clamping device 3;

[0046] S5, sending the second positioning and clamping device 3 and the blade to be coated 1 into the coating furnace and adjusting them so that the blade bottom surface 13 of the blade to be coated 1 forms an angle β with the vertical direction of the coating furnace;

[0047] S6, starting the coating furnace to complete the preparation of the second coating 52 on the blade to be coated 1;

[0048] The angle α and the angle β in steps S2 and S5 should satisfy: 0≤α≤30° and 0≤β≤30°, and should also satisfy: 0.8β≤α≤1.2β.

[0049] The method for preparing a blade with a uniform coating of the present invention firstly adopts a first positioning and clamping device 2 to clamp and position the blade 1 to be coated, so that the position and angle of the blade 1 to be coated in the coating furnace 8 can be adjusted, so that the blade bottom surface 13 of the blade 1 to be coated forms an angle α with the horizontal direction of the coating furnace 8, and firstly forms a uniform first coating 51 on the rake face 11 and the flank face 12. Since the angles between the rake face 11 and the flank face 12 and the horizontal coating spraying direction are different, the thickness of the first coating 51 formed on the rake face 11 and the flank face 12 is different. The thickness of the first coating on the front blade surface is X1, and the thickness of the first coating on the back blade surface is X1'. Then, the second positioning and clamping device 3 is used to clamp and position the blade 1 to be coated, so that the bottom surface 13 of the blade 1 to be coated forms an angle β with the vertical direction of the coating furnace 8, and the second coating 52 is formed on the front blade surface 11 and the back blade surface 12. Based on the same reason as above, the thickness of the second coating 52 on the front blade surface 11 and the back blade surface 12 is also different (the thickness of the second coating on the front blade surface is X2, and the thickness of the first coating on the back blade surface is X2' ), since the angle α and the angle β satisfy 0.8β≤α≤1.2β (i.e., the values ​​of α and β are relatively close, which is equivalent to the position exchange of the front cutting edge 11 and the back cutting edge 12 during the two coating preparations), the overall thickness (X1+X2) of the two layers of coating on the front cutting edge 11 can be substantially the same as the overall thickness (X1'+X2') of the two layers of coating on the back cutting edge 12, and since when preparing the first coating 51, the blade bottom surface 13 of the blade to be coated 1 has an angle α with the horizontal direction of the coating furnace 8, 0≤α≤30°, therefore, compared with the prior art , the particle density of the same number of coating particles ejected from the coating furnace 8 and deposited on the front cutting edge 11 and the back cutting edge 12 is reduced. When the thickness of the first coating 51 reaches the set value, the thickness of the first coating 51 on the front cutting edge 11 is more uniform, and the thickness of the first coating 51 on the back cutting edge 12 is also more uniform. Similarly, the thickness of the second coating 52 on the front cutting edge 11 is more uniform, and the thickness of the second coating 52 on the back cutting edge 12 is also more uniform. Therefore, the overall thickness of the coating at various locations on the front cutting edge 11 is more uniform, and the overall thickness of the coating at various locations on the back cutting edge 12 is also more uniform. Thereby, the problem of uneven coating thickness caused by the different angles between the front cutting surface 11 and the back cutting surface 12 and the coating spraying direction in the prior art is eliminated. Finally, the coating formed on the front cutting surface 11 is more uniform and stable, and the coating formed on the back cutting surface 12 is also more uniform and stable. At the same time, the coating thickness of the front cutting surface 11 and the back cutting surface 12 can also be kept uniform and consistent, the tensile and compressive stresses between the blade coatings are small, and different coatings can be combined. The prepared blade coating has good impact resistance and wear resistance, thereby improving the cutting performance of the blade.

[0050] like Figure 2 , Figure 4 and Figure 5As shown, the first positioning and clamping device 2 is used to clamp and position the blade 1 to be coated to prepare the first coating 51: a plurality of coating spraying devices are arranged on the side wall 81 of the coating furnace to spray the coating material horizontally. Figure 2 When the first positioning and clamping device 2 is in state B, C, and D, it meets the requirement of the present application that "the blade bottom surface 13 of the blade to be coated 1 forms an angle α with the horizontal direction of the coating furnace 8", such as Figure 4 , 5 As shown in the figure (the arrow in the figure represents the coating spraying direction), after the preparation of the first coating 51 is completed, the thickness of the first coating 51 on the front cutting edge 11 is X1, and the thickness of the first coating on the back cutting edge 12 is X1'. Moreover, since an angle α satisfying 0≤α≤30° is provided (α=13° in this embodiment), the particle density of the same number of coating particles sprayed by the coating spraying device and deposited on the front cutting edge 11 and the back cutting edge 12 is reduced. When the thickness of the first coating 51 reaches the set value, the thickness of the first coating 51 on the front cutting edge 11 is more uniform, and the thickness of the first coating 51 on the back cutting edge 12 is also more uniform.

[0051] like Figure 3 , Figure 6 and Figure 7 As shown, the second positioning and clamping device 3 is used to clamp and position the blade to be coated 1 that has been prepared with the first coating 51 to prepare the second coating 52: Figure 3 When the second positioning and clamping device 3 is in state E, F, and G, it meets the requirement of the present application that "the blade bottom surface 13 of the blade to be coated 1 forms an angle β with the horizontal direction of the coating furnace 8", such as Figure 6 , 7 As shown in the figure (the arrow in the figure represents the coating spraying direction), after the preparation of the second coating 52 is completed, the thickness of the second coating 52 on the front cutting edge 11 is X2, and the thickness of the second coating on the back cutting edge 12 is X2'. Since the values ​​of α and β are relatively close, it is equivalent to the front cutting edge 11 and the back cutting edge 12 being exchanged in the two coating preparations (see Figure 4 and Figure 6 The position of the front cutting edge 11 and the back cutting edge 12 can achieve that the overall thickness (X1+X2) of the two coating layers on the front cutting edge 11 is substantially the same as the overall thickness (X1'+X2') of the two coating layers on the back cutting edge 12; and because an angle β satisfying 0≤β≤30° is provided (β=13° in the present embodiment), the particle density of the same number of coating particles sprayed by the coating spraying device and deposited on the front cutting edge 11 and the back cutting edge 12 is reduced, and when the thickness of the second coating layer 52 reaches a set value, the thickness of the second coating layer 52 on the front cutting edge 11 is more uniform, and the thickness of the second coating layer 52 on the back cutting edge 12 is also more uniform.

[0052] In addition to this embodiment, the angle α and the angle β may also be set to satisfy 60°≤α≤90°, 60°≤β≤90°, and the above technical effects may also be achieved.

[0053] If the angle α and the angle β are set to α=0 and β=0, under the premise that the space of the coating preparation area inside the coating furnace 8 is limited, the number of blades prepared by a single coating can be maximized, and the difficulty of positioning the blades and the positioning clamping device is reduced, thereby greatly improving the blade production efficiency. Moreover, through two coating preparations, the overall thickness of the coating on the front cutting edge 11 and the back cutting edge 12 can be basically the same, and the coating is uniform and stable.

[0054] In this embodiment, in step S4, before cleaning the blade 1 to be coated, the edge of the blade 1 to be coated is subjected to jet treatment, using corundum particles with a particle size of 120-150 meshes and a jet time of 1-3 minutes.

[0055] In this embodiment, in step S3 , a first coating 51 is formed on both the rake face 11 and the flank face 12 of the insert 1 to be coated, and in step S6 , a second coating 52 is formed on both the rake face 11 and the flank face 12 of the insert 1 to be coated.

[0056] In order to ensure the coating performance, the maximum total thickness of the coating on the front cutting edge 11 is Y1, the maximum total thickness of the coating on the rear cutting edge 12 is Y2, the minimum total thickness of the coating on the front cutting edge 11 is Y1', and the minimum total thickness of the coating on the rear cutting edge 12 is Y2', which should satisfy: 0≤Y1 -Y2≤1µm, 0≤Y1 -Y1'≤1µm, 0≤Y2-Y2'≤1µm. In this embodiment, Y1 =Y2=5µm, Y1'=4.9µm, and Y2'=4.9µm.

[0057] In this embodiment, the thickness of the first coating 51 on the front cutting edge 11 is X1, the thickness of the second coating 52 is X2, the thickness of the first coating 51 on the rear cutting edge 12 is X1', and the thickness of the second coating 52 is X2'. In order to ensure the coating performance, the following conditions should be met: 1µm≤X1 - X2≤3µm, 1µm≤X2'- X1'≤3µm. In this embodiment, X1=3µm, X2=2µm, X2'=3µm, and X1'=2µm.

[0058] In addition to the above embodiments, the thickness of the first coating 51 on the front cutting edge 11 is X1, the thickness of the second coating 52 is X2, the thickness of the first coating 51 on the rear cutting edge 12 is X1', the thickness of the second coating 52 is X2', and the following conditions should be satisfied: 1µm≤X2 -X1≤3µm, 1µm≤X1'- X2'≤3µm.

[0059] In the coating device used in the method for preparing a blade with uniform coating in this embodiment, the first positioning and clamping device 2 may be magnetic or may be a hook to fix the blade 1 to be coated.

[0060] In this embodiment, the first positioning and clamping device 2 and the second positioning and clamping device 3 include a chassis 6 that can form an incomplete coating on the back face 12 and a cover plate 7 that can form an incomplete coating on the front face 11. The chassis 6 is provided with a side recess 61, and the cover plate 7 is provided with a top recess 71. The incomplete coating can be formed on the back face 12 of the blade to be coated 1 by installing the blade to be coated 1 in the chassis 6, and the cover plate 7 is covered on the front face 11 of the blade to be coated 1 to form an incomplete coating on the front face 11. Both the first coating 51 and the second coating 52 can be set as incomplete coatings.

[0061] In addition to this embodiment, it can also be configured that the first positioning and clamping device 2 includes a base plate 6 that can form an incomplete coating coverage on the back cutting edge 12 and a cover plate 7 that can form an incomplete coating coverage on the front cutting edge 11, or the second positioning and clamping device 3 includes a base plate 6 that can form an incomplete coating coverage on the back cutting edge 12 and a cover plate 7 that can form an incomplete coating coverage on the front cutting edge 11.

[0062] In this embodiment, in order to facilitate the control of the spraying direction of the coating material and to prepare an incompletely covered coating, the coating furnace 8 is a physical coating furnace.

[0063] Although the present invention has been disclosed as above with preferred embodiments, it is not intended to limit the present invention. Any technician familiar with the art can make many possible changes and modifications to the technical solution of the present invention by using the technical content disclosed above without departing from the scope of the technical solution of the present invention, or modify it into an equivalent embodiment of equivalent changes. Therefore, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention should fall within the scope of protection of the technical solution of the present invention.

Claims

1. A method for preparing a blade having a uniform coating, characterized in that: The following steps are involved: S1, assembling the blade to be coated (1) onto a first positioning and clamping device (2); S2, sending the first positioning clamping device (2) and the blade to be coated (1) into the coating furnace and adjusting them so that the blade bottom surface (13) of the blade to be coated (1) forms an angle α with the horizontal direction of the coating furnace; S3, starting the coating furnace to complete the preparation of the first coating (51) on the blade to be coated (1); S4, taking out the first positioning and clamping device (2) and the blade to be coated (1), cleaning the blade to be coated (1), and then assembling the blade to be coated (1) onto the second positioning and clamping device (3); S5, sending the second positioning clamping device (3) and the blade to be coated (1) into the coating furnace and adjusting them so that the blade bottom surface (13) of the blade to be coated (1) forms an angle β with the vertical direction of the coating furnace; S6, starting the coating furnace to complete the preparation of the second coating (52) on the blade to be coated (1); The angle α and the angle β in steps S2 and S5 should satisfy: 0≤α≤30° and 0≤β≤30°, or satisfy: 60°≤α≤90° and 60°≤β≤90°, and should also satisfy: 0.8β≤α≤1.2β.

2. The method for preparing a blade having a uniform coating according to claim 1, characterized in that: The angle α and the angle β satisfy: α=0, β=0.

3. The method for preparing a blade with a uniform coating according to claim 1 or 2, characterized in that: In the step S4, before cleaning the blade to be coated (1), the cutting edge of the blade to be coated (1) is subjected to jet treatment, using corundum particles with a particle size of 120 to 150 meshes and a jetting time of 1 to 3 minutes.

4. The method for preparing a blade with a uniform coating according to claim 1 or 2, characterized in that: In the step S3, a first coating (51) is formed on both the front cutting surface (11) and the rear cutting surface (12) of the blade to be coated (1), and in the step S6, a second coating (52) is formed on both the front cutting surface (11) and the rear cutting surface (12) of the blade to be coated (1).

5. The method for preparing a blade with a uniform coating according to claim 4, characterized in that: The maximum total thickness of the coating on the front cutting edge (11) is Y1, and the maximum total thickness of the coating on the rear cutting edge (12) is Y2, which should satisfy: 0≤Y1-Y2≤1µm.

6. The method for preparing a blade with a uniform coating according to claim 5, characterized in that: The minimum total thickness of the coating on the front cutting edge (11) is Y1', and the minimum total thickness of the coating on the rear cutting edge (12) is Y2', which should satisfy the following conditions: 0≤Y1-Y1'≤1µm, 0≤Y2-Y2'≤1µm.

7. The method for preparing a blade having a uniform coating according to claim 6, characterized in that: The maximum thickness of the first coating (51) on the front cutting edge (11) is X1, the maximum thickness of the second coating (52) is X2, the maximum thickness of the first coating (51) on the rear cutting edge (12) is X1', the maximum thickness of the second coating (52) is X2', and the following conditions are satisfied: 1µm≤X1 - X2≤3µm, 1µm≤X2'- X1'≤3µm.

8. The method for preparing a blade having a uniform coating according to claim 6, characterized in that: The maximum thickness of the first coating (51) on the front cutting edge (11) is X1, the maximum thickness of the second coating (52) is X2, the maximum thickness of the first coating (51) on the rear cutting edge (12) is X1', the maximum thickness of the second coating (52) is X2', and the following conditions are satisfied: 1µm≤X2 - X1≤3µm, 1µm≤X1'- X2'≤3µm.

9. The method for preparing a blade with a uniform coating according to claim 1 or 2, characterized in that: The first positioning and clamping device (2) and / or the second positioning and clamping device (3) comprises a base plate (6) capable of forming a back cutting edge (12) that is not completely covered with a coating, and a cover plate (7) capable of forming a front cutting edge (11) that is not completely covered with a coating.