A flexible conductive barrier film and its preparation method and application
The inorganic/organic composite film layer is formed through low-temperature plasma treatment and atomic layer deposition technology, and modified silver nanowires are used to solve the problems of insufficient compactness and bending resistance of high barrier films in the existing technology, and realize a flexible conductive barrier film High barrier properties and conductivity, suitable for flexible electronic product packaging.
Patent Information
- Application Number
- CN202410595564.8
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-05-14
- Publication Date
- 2024-10-22
- Estimated Expiration
- 2044-05-14
AI Technical Summary
The high-barrier films in the existing technology have insufficient compactness and bending resistance, making it difficult to meet the development needs of flexible electronic devices, and the inherent mechanical brittleness and conductivity of traditional transparent conductive oxide films limit their applications.
The polyethylene terephthalate film is treated with low-temperature argon/oxygen mixed plasma technology, and aluminum oxide and titanium dioxide films are alternately deposited using the atomic layer deposition method to form an inorganic/organic composite film layer, and the weather resistance of the barrier layer is improved through photocuring technology. properties and electrical conductivity, using modified silver nanowires to improve electrical conductivity.
A flexible conductive barrier film with excellent barrier properties and conductivity has been obtained. It has high interlayer peeling strength and is not easy to delaminate. It is suitable for packaging of flexible electronic products.
Smart Images

Figure CN118418556B_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of conductive films, and in particular to a flexible conductive barrier film and a preparation method and application thereof. Background Art
[0002] Water vapor, oxygen, carbon dioxide and other substances in nature can damage high-precision electronic components, causing electronic components to fail. In the prior art, high-barrier barrier films are used as packaging protective layers to protect high-precision electronic components and extend the service life of the components.
[0003] In the prior art, the preparation of high barrier films is mostly carried out by evaporation, chemical vapor deposition, magnetron sputtering and the like. The film density of the barrier film prepared by evaporation is poor, resulting in low barrier performance and failing to meet the requirements of high water barrier performance. The density of the film layer prepared by magnetron sputtering is lower than that of chemical vapor deposition, and a flat layer needs to be formed on the substrate before coating. Although chemical vapor deposition can produce high-density films, it has poor bending resistance and high cost, and is not suitable for the preparation of flexible barrier films. In order to improve the packaging life of high-precision electronic components and increase the feasibility of their application in electronic products, it is necessary to develop barrier films with better barrier properties, better flexibility, conductivity and thinner overall thickness.
[0004] In the existing technology, traditional transparent conductive oxide films represented by indium tin oxide (ITO) and fluorine-doped tin oxide (FTO) have limitations such as inherent mechanical brittleness, poor conductivity when deposited at low temperatures, lack of flexibility, and shortage of indium resources, making it difficult to meet the development needs of flexible electronic devices.
[0005] Prior art, such as Chinese patent application CN112927839A, discloses a flexible nanosilver conductive film and its preparation method and application, wherein a protective layer, an anti-scratch layer, an oxygen barrier layer, a nanosilver coating, a TPU substrate layer, a nanosilver coating, an oxygen barrier layer, an anti-scratch layer, and a protective layer are sequentially arranged on a modified TPU substrate from top to bottom, so that the obtained flexible nanosilver conductive film has excellent conductivity and light transmittance and low cost. However, since the barrier layer structure arranged in the prepared film is only composed of an organic layer, the thickness is relatively thick, and the barrier property needs to be improved, which limits the application of the material. Summary of the invention
[0006] The purpose of the present invention is to overcome the shortcomings of the prior art and provide a flexible conductive barrier film and a preparation method and application thereof. The flexible conductive barrier film has excellent barrier properties and conductivity, high interlayer peeling strength, is not easy to delaminate, and can be used in flexible packaging of electronic products.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] A method for preparing a flexible conductive barrier film comprises the following steps:
[0009] Step (1), washing the polyethylene terephthalate film with acetone, drying, and treating both sides of the dried polyethylene terephthalate film with a low-temperature argon / oxygen mixed plasma technology to obtain a base film; immersing the base film in aniline, taking out the base film with aniline attached after immersion, suspending it on the surface of an aniline / hydrochloric acid / ammonium persulfate mixed solution, reacting, and washing and drying after the reaction is completed to obtain an intermediate layer material;
[0010] Step (2), using an atomic layer deposition method to alternately deposit an aluminum oxide film and a titanium dioxide film on the side of the intermediate layer material that is not attached with polyaniline, and after the deposition, attaching a layer of polymethyl methacrylate through an inkjet printing system, and forming a polymethyl methacrylate film after photocuring, and repeating the deposition, inkjet printing, and photocuring operations three times to obtain a barrier layer / intermediate layer composite material;
[0011] Step (3), mixing polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate, and performing a first reaction. After the reaction is completed, 1,4-butanediol and 3-methyl-1,5-pentanediol are added. After the reaction is completed, pentaerythritol triacrylate and hydroxyethyl acrylate are added. After the reaction is completed, a third reaction is performed to obtain polyurethane acrylate.
[0012] Mixing and dissolving acrylic acid, tetramethylammonium chloride and p-hydroxyanisole to obtain an acrylic acid mixed solution, adding the acrylic acid mixed solution dropwise to the epoxy resin, and reacting after the addition is complete. After the reaction is complete, a modified epoxy resin is obtained;
[0013] Mixing modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and a photoinitiator under light-proof conditions to obtain an outer layer material, coating the outer layer material on the barrier layer surface of the barrier layer / intermediate layer composite material, and light curing to obtain an outer layer / barrier layer / intermediate layer composite material;
[0014] Step (4), mixing water, xylene and polyurethane acrylate uniformly, adding dodecylbenzene sulfonic acid and continuing to mix, adding aniline, dropping an aqueous solution of ammonium persulfate, reacting after the dropwise addition is complete, and drying after the reaction is complete to obtain modified polyurethane acrylate;
[0015] Isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile are mixed and reacted to obtain modified polyacrylate; the modified polyacrylate, modified polyurethane acrylate, and a photoinitiator are mixed under light-proof conditions to obtain a glue layer material;
[0016] Silver nanowires, 3-mercaptopropionic acid and water are mixed and stirred, centrifuged, filtered, washed and dried to obtain modified silver nanowires, the modified silver nanowires are mixed with isopropanol to obtain a modified silver nanowire / isopropanol mixed solution, the modified silver nanowire / isopropanol mixed solution is deposited on a substrate film layer to obtain a substrate film layer having a modified silver nanowire network on the surface, a glue layer material is coated on the side having the modified silver nanowire network on the substrate film layer having the modified silver nanowire network on the surface, an outer layer / barrier layer / middle layer composite material is covered, a side of the outer layer / barrier layer / middle layer composite material with polyaniline is brought into contact with the glue layer material, photocuring is performed, and the substrate film layer is peeled off to obtain a flexible conductive barrier film.
[0017] Preferably, in step (1), the conditions for the low-temperature argon / oxygen mixed plasma technology treatment are: plasma discharge power is 100-150W, and the treatment time is 400-600s.
[0018] Preferably, in step (1), the thickness of the base film is 40 μm, and the mass ratio of the base film to aniline is 1:10; the reaction conditions are: reacting at room temperature for 6-8 hours; and the thickness of the intermediate layer material is 45-50 μm.
[0019] Preferably, the aniline / hydrochloric acid / ammonium persulfate mixed solution is prepared by mixing aniline, 1 mol / L hydrochloric acid aqueous solution, and 0.36 mol / L ammonium persulfate aqueous solution. In the solute of the aniline / hydrochloric acid / ammonium persulfate mixed solution, the molar ratio of aniline, the solute hydrogen chloride in the 1 mol / L hydrochloric acid aqueous solution, and the solute ammonium persulfate in the 0.36 mol / L ammonium persulfate aqueous solution is 1:20:1.
[0020] Preferably, in the step (2), the equipment used for the atomic layer deposition method is a BENEQ TFS500 thin film deposition system, the precursor materials are trimethylaluminum, titanium tetrachloride and distilled water at room temperature, the temperature of the thin film deposition is 80°C, the chamber pressure is 43Pa, the carrier gas is nitrogen, the carrier gas volume is 300mL / min, the thickness of the aluminum oxide film formed by a single deposition and the titanium dioxide film formed by a single deposition are both 5nm, and the number of alternating depositions is 6 times; the photocuring conditions are: photocuring for 30s in a nitrogen atmosphere and UV-LED ultraviolet light; the thickness of the polymethyl methacrylate film formed after a single inkjet printing and photocuring is 1μm.
[0021] Preferably, in step (3), the molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate and 2-hydroxyethyl acrylate is 1:1:1:0.4-0.5:0.3-0.4:0.1:0.1-0.3, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol; the first reaction conditions are: the first reaction is carried out in a nitrogen atmosphere at a temperature of 60-70°C for 3-4h; the second reaction conditions are: the second reaction is carried out at a temperature of 70-80°C for 1.5-2h; and the third reaction conditions are: the third reaction is carried out at a temperature of 70-80°C for 1-2h.
[0022] Preferably, in step (3), the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole and epoxy resin is 150-180:0.25-0.3:0.75-0.85:250-300; the dropping time of the acrylic acid mixed solution is 20-30 min; and the reaction conditions are: reacting at a temperature of 90-100° C. for 3-4 h.
[0023] Preferably, in step (3), the mass ratio of modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator is 10-20:30-40:50:2-3; the coating thickness of the outer layer material is 1-2 μm; and the photocuring conditions are: photocuring in a nitrogen atmosphere and UV-LED ultraviolet light for 2 minutes.
[0024] Preferably, in step (4), polyurethane acrylate is prepared in step (2), and the mass ratio of dodecylbenzenesulfonic acid, water, xylene, polyurethane acrylate, aniline, and ammonium persulfate aqueous solution is 40-45:50-60:85-100:16-25:10-40:100-110; the ammonium persulfate aqueous solution is 1.2 mol / L ammonium persulfate aqueous solution, and the dropwise addition time is 15-20 min; and the reaction conditions are: reaction at a temperature of 0-5°C for 6-8 h.
[0025] Preferably, in step (4), the mass ratio of isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile is 120-130:10-20:11.5-13:7.5-10:4-5:200:0.15-0.2; the reaction conditions are: react at a temperature of 65-75°C for 18-24h; and the mass ratio of modified polyacrylate, modified polyurethane acrylate, and photoinitiator is 5-10:90-95:1.
[0026] Preferably, in step (4), the mass ratio of silver nanowires, 3-mercaptopropionic acid and water is 1:1:300, and the stirring time is 12 hours. The coating thickness of the adhesive layer material is 5-6 μm. The light curing conditions are: light curing in a nitrogen atmosphere and UV-LED ultraviolet light for 30-40 seconds.
[0027] Preferably, in the step (4), the deposition operation comprises: depositing the modified silver nanowire / isopropanol mixed solution on the substrate film layer by spin coating, and drying at 80-90° C. for 10-20 min; the spin coating parameters of the spin coating method are: slow spin coating speed of 400 r / min, time of 6 s, fast spin coating speed of 3500 r / min, time of 20 s, and the number of spin coating deposition is 4 times.
[0028] Preferably, the mass ratio of the modified silver nanowires to isopropanol is 1:220-260.
[0029] Furthermore, the substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm.
[0030] Preferably, a flexible conductive barrier film is prepared by the method for preparing a flexible conductive barrier film as described above.
[0031] Preferably, an application of the flexible conductive barrier film as described above is provided.
[0032] Compared with the prior art, the present invention has the following beneficial effects:
[0033] The present invention modifies the PET film by low-temperature plasma treatment, thereby increasing the surface area of the PET film and increasing polar groups such as hydroxyl groups on the film surface, thereby increasing the bonding performance between the obtained modified base film and other film layers; and polymerizing aniline on one side of the modified base film by chemical oxidation polymerization, so that the obtained polyaniline layer and the modified base film can have an excellent bonding effect without adding an adhesive.
[0034] Atomic layer deposition (ALD) technology is a preparation technology that controls the growth of thin films at the atomic scale. It has the advantages of preparing highly dense structures and precisely controllable film thickness. It can also precisely control the thickness and uniformity of the film on a large-area substrate, and can be used in the preparation of ultra-high barrier films. The present invention uses an atomic layer deposition method to alternately deposit inorganic film layers and organic film layers on the side of the modified base film without polyaniline, so that the obtained inorganic / organic composite film layer has excellent adhesion to the modified base film, and because the inorganic film layer in the inorganic / organic composite film layer is formed by combining an aluminum oxide film and a titanium dioxide film to form a multilayer structure, this structure can reduce the continuous diffusion path of water vapor in the film, thereby reducing the water vapor transmission rate, and the composite use of the aluminum oxide film and the titanium dioxide film can further improve the chemical stability and barrier properties of the inorganic film layer; the insertion of the organic film layer into the inorganic film layer can prevent defects from growing through the inorganic layer, and provide a flat surface for subsequent inorganic film layer deposition, which can further increase the barrier properties of the composite film layer, and at the same time increase the flexibility of the inorganic / organic composite film layer, so that the obtained barrier layer has high barrier properties while maintaining good softness.
[0035] The present invention modifies the epoxy resin to have double bonds, and can achieve photocuring by adding a photoinitiator. The epoxy resin is mixed and modified with polyurethane acrylate to improve the heat resistance and weather resistance of the polyurethane acrylate, while maintaining good softness. The epoxy resin is used as an outer layer material and coated on the side of the barrier layer to which polyaniline is not attached. After photocuring, the barrier layer can be protected and the weather resistance of the barrier layer can be improved.
[0036] In the present invention, polyaniline is synthesized in polyurethane acrylic resin to make the obtained modified polyurethane acrylate have conductivity. By adding modified polyacrylate having carboxyl groups and siloxane segments into the modified polyurethane acrylate, on the one hand, the conductivity of polyaniline can be improved, and on the other hand, the siloxane segments of the modified polyacrylate can improve the softness of the adhesive layer material and reduce the influence of polar groups on the flexibility of the adhesive layer material. In addition, the carboxyl groups in the modified polyacrylate can enhance the bonding performance of the adhesive layer material and improve the bonding between the adhesive layer material and the adjacent layer material.
[0037] The present invention uses 3-mercaptopropionic acid to modify the surface of silver nanowires, thereby improving the dispersibility of the silver nanowires. At the same time, due to the interaction between the modified silver nanowires and the carboxyl groups in the adhesive layer material, the silver nanowires are tightly compounded with the adhesive layer material and are not easy to peel off. At the same time, the adhesive layer material also protects the silver nanowires and is not easily affected by external forces to damage the conductive properties of the film. After the various layers of materials are compounded and photocured, a flexible conductive barrier film is obtained. Since the use of adhesive is reduced and the overall thickness of the film is reduced, the flexible conductive barrier film is more flexible and has excellent barrier properties and conductivity, and can be applied to flexible packaging of electronic products. BRIEF DESCRIPTION OF THE DRAWINGS
[0038] Figure 1 is a flow chart of a method for preparing a flexible conductive barrier film in the present invention;
[0039] Figure 2 It is a schematic diagram of the structure of the flexible conductive barrier film prepared in the present invention;
[0040] Figure 3 It is a line graph of interlayer peeling strength of the flexible conductive barrier films prepared in Examples 1-5 and Comparative Examples 1-3 of the present invention in a comprehensive performance test;
[0041] In the figure:
[0042] 1. Outer layer; 2. Barrier layer; 3. Base film; 4. Polyaniline layer; 5. Middle layer; 6. Adhesive layer; 7. Modified silver nanowire network layer. DETAILED DESCRIPTION
[0043] The technical solutions in the embodiments of the present invention will be clearly and completely described below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of the present invention.
[0044] Example 1
[0045] This embodiment discloses a method for preparing a flexible conductive barrier film, comprising the following steps:
[0046] Step (1), washing the polyethylene terephthalate film with acetone, drying it at 60°C for 3h, treating both sides of the dried polyethylene terephthalate film with low-temperature argon / oxygen mixed plasma technology, wherein the plasma discharge power is 100W and the treatment time is 600s, and after the treatment, a base film is obtained; immersing the base film in aniline, wherein the mass ratio of the base film to the aniline is 1:10, after the immersion, taking out the base film attached with aniline, suspending it on the surface of a mixed solution of aniline / hydrochloric acid / ammonium persulfate, reacting it at room temperature for 6h, and after the reaction is completed, adding water 6 times the mass of the base film for washing, and drying it at 50°C for 10h to obtain an intermediate layer material; one side of the intermediate layer material is attached with polyaniline;
[0047] The thickness of the base film is 40 μm, and the thickness of the intermediate layer material is 45 μm; the aniline / hydrochloric acid / ammonium persulfate mixed solution is prepared by mixing aniline, 1 mol / L hydrochloric acid aqueous solution, and 0.36 mol / L ammonium persulfate aqueous solution, and in the solute of the aniline / hydrochloric acid / ammonium persulfate mixed solution, the molar ratio of aniline, the solute hydrogen chloride in the 1 mol / L hydrochloric acid aqueous solution, and the solute ammonium persulfate in the 0.36 mol / L ammonium persulfate aqueous solution is 1:20:1;
[0048] Step (2), using an atomic layer deposition method to alternately deposit an aluminum oxide film and a titanium dioxide film on the side of the intermediate layer material not attached with polyaniline, wherein the thickness of the aluminum oxide film and the titanium dioxide film formed by a single deposition are both 5 nm, and the number of alternating depositions is 6 times. After the deposition is completed, a layer of polymethyl methacrylate is attached by an inkjet printing system, and a polymethyl methacrylate film is formed after photocuring for 30 seconds in a nitrogen atmosphere and UV-LED ultraviolet light. The thickness of the polymethyl methacrylate film formed after a single inkjet printing and photocuring is 1 μm. The deposition, inkjet printing, and photocuring operations are repeated three times to obtain a barrier layer / intermediate layer composite material;
[0049] The equipment used for the atomic layer deposition method is the BENEQ TFS500 thin film deposition system. The precursor materials are trimethylaluminum, titanium tetrachloride and distilled water at room temperature. The film deposition temperature is 80°C, the chamber pressure is 43Pa, the carrier gas is nitrogen, and the carrier gas volume is 300mL / min.
[0050] Step (3), polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate are mixed, and the mixture is reacted for a first time at 60° C. in a nitrogen atmosphere for 4 hours. After the reaction, 1,4-butanediol and 3-methyl-1,5-pentanediol are added, and the mixture is reacted for a second time at 70° C. for 2 hours. After the reaction, pentaerythritol triacrylate and hydroxyethyl acrylate are added, and the mixture is reacted for a third time at 70° C. for 2 hours. After the reaction, polyurethane acrylate is obtained;
[0051] The molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate, and 2-hydroxyethyl acrylate is 1:1:1:0.5:0.3:0.1:0.3, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol;
[0052] Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin for 20 minutes. After the addition is completed, the mixture is reacted at 100° C. for 3 hours. After the reaction is completed, a modified epoxy resin is obtained;
[0053] Wherein, the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole and epoxy resin is 150:0.25:0.75:250;
[0054] Modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator are mixed in a mass ratio of 10:40:50:2 under light-proof conditions to obtain an outer layer material, and the outer layer material is coated on the barrier layer surface of the barrier layer / intermediate layer composite material, the coating thickness of the outer layer material is 1 μm, and the outer layer material is photocured for 2 minutes under UV-LED ultraviolet light in a nitrogen atmosphere to obtain an outer layer / barrier layer / intermediate layer composite material;
[0055] Step (4), mixing water, xylene and polyurethane acrylate uniformly, adding dodecylbenzene sulfonic acid and continuing mixing for 15 minutes, adding aniline, and dripping 1.2 mol / L ammonium persulfate aqueous solution for 15 minutes. After the dripping is completed, reacting at 0°C for 8 hours. After the reaction is completed, drying at 50°C for 24 hours to obtain modified polyurethane acrylate;
[0056] The polyurethane acrylate is prepared in step (2), and the mass ratio of dodecylbenzenesulfonic acid, water, xylene, polyurethane acrylate, aniline, and 1.2 mol / L ammonium persulfate aqueous solution is 40:50:85:16:10:100;
[0057] Isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile are mixed in a mass ratio of 120:10:11.5:7.5:4:200:0.15, and reacted at 65°C for 24 hours. After the reaction, modified polyacrylate is obtained; modified polyacrylate, modified polyurethane acrylate, and photoinitiator are mixed in a mass ratio of 5:95:1 under light-proof conditions to obtain a glue layer material;
[0058] Silver nanowires, 3-mercaptopropionic acid, and water were mixed and stirred at a mass ratio of 1:1:300 for 12 h, centrifuged, filtered, washed with water 6 times the mass of the silver nanowires, and dried at 60°C for 12 h to obtain modified silver nanowires. The modified silver nanowires were mixed with isopropanol at a mass ratio of 1:220 to obtain a modified silver nanowire / isopropanol mixed solution. The modified silver nanowire / isopropanol mixed solution was deposited on a substrate film layer by spin coating, and dried at 80°C for 20 min to obtain A substrate film layer having a modified silver nanowire network on its surface is coated with a glue layer material on one side of the substrate film layer having the modified silver nanowire network on its surface, wherein the coating thickness of the glue layer material is 5 μm, and an outer layer / barrier layer / intermediate layer composite material is covered, so that the side of the outer layer / barrier layer / intermediate layer composite material with polyaniline attached is in contact with the glue layer material, and the composite material is photocured in a nitrogen atmosphere and UV-LED ultraviolet light for 30 seconds, and the substrate film layer is peeled off to obtain a flexible conductive barrier film;
[0059] The substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm. The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
[0060] Example 2
[0061] This embodiment discloses a method for preparing a flexible conductive barrier film, comprising the following steps:
[0062] Step (1), washing the polyethylene terephthalate film with acetone, drying it at 50°C for 5h, treating both sides of the dried polyethylene terephthalate film with low-temperature argon / oxygen mixed plasma technology, wherein the plasma discharge power is 120W and the treatment time is 450s, and obtaining a base film after treatment; immersing the base film in aniline, wherein the mass ratio of the base film to the aniline is 1:10, after immersion, taking out the base film attached with aniline, suspending it on the surface of a mixed solution of aniline / hydrochloric acid / ammonium persulfate, reacting it at room temperature for 6h, and after the reaction is completed, adding water 8 times the mass of the base film for washing, and drying it at 45°C for 11h to obtain an intermediate layer material; wherein one side of the intermediate layer material is attached with polyaniline;
[0063] The thickness of the base film is 40 μm, and the thickness of the intermediate layer material is 46 μm; the aniline / hydrochloric acid / ammonium persulfate mixed solution is prepared by mixing aniline, 1 mol / L hydrochloric acid aqueous solution, and 0.36 mol / L ammonium persulfate aqueous solution, and in the solute of the aniline / hydrochloric acid / ammonium persulfate mixed solution, the molar ratio of aniline, the solute hydrogen chloride in the 1 mol / L hydrochloric acid aqueous solution, and the solute ammonium persulfate in the 0.36 mol / L ammonium persulfate aqueous solution is 1:20:1;
[0064] Step (2), preparation of the barrier layer / intermediate layer composite material is the same as in Example 1;
[0065] Step (3), polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate are mixed, and the mixture is reacted for a first time at 65° C. in a nitrogen atmosphere for 3.5 hours. After the reaction is completed, 1,4-butanediol and 3-methyl-1,5-pentanediol are added, and the mixture is reacted for a second time at 75° C. for 1.8 hours. After the reaction is completed, pentaerythritol triacrylate and hydroxyethyl acrylate are added, and the mixture is reacted for a third time at 70° C. for 2 hours. After the reaction is completed, polyurethane acrylate is obtained;
[0066] The molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate, and 2-hydroxyethyl acrylate is 1:1:1:0.42:0.32:0.1:0.15, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol;
[0067] Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin for 20 minutes. After the addition is completed, the mixture is reacted at 95° C. for 3.5 hours. After the reaction is completed, a modified epoxy resin is obtained;
[0068] Among them, the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole, and epoxy resin is 155:0.26:0.78:260;
[0069] Modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator are mixed in a mass ratio of 12:32:50:2.5 under light-proof conditions to obtain an outer layer material, and the outer layer material is coated on the barrier layer surface of the barrier layer / middle layer composite material, the coating thickness of the outer layer material is 1 μm, and the outer layer material is photocured for 2 minutes under UV-LED ultraviolet light in a nitrogen atmosphere to obtain an outer layer / barrier layer / middle layer composite material;
[0070] Step (4), mixing water, xylene and polyurethane acrylate uniformly, adding dodecylbenzene sulfonic acid and continuing mixing for 15 minutes, adding aniline, and dripping 1.2 mol / L ammonium persulfate aqueous solution for 20 minutes. After the dripping is completed, reacting at 2°C for 7 hours. After the reaction is completed, drying at 60°C for 18 hours to obtain modified polyurethane acrylate;
[0071] The polyurethane acrylate is prepared in step (2), and the mass ratio of dodecylbenzene sulfonic acid, water, xylene, polyurethane acrylate, aniline, and 1.2 mol / L ammonium persulfate aqueous solution is 41:52:90:18:20:102;
[0072] Isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile are mixed in a mass ratio of 123:12:12:8.5:4.2:200:0.16, and reacted at 65°C for 24 hours. After the reaction, modified polyacrylate is obtained; modified polyacrylate, modified polyurethane acrylate, and photoinitiator are mixed in a mass ratio of 6:94:1 under light-proof conditions to obtain a glue layer material;
[0073] Silver nanowires, 3-mercaptopropionic acid, and water were mixed and stirred at a mass ratio of 1:1:300 for 12 hours, centrifuged, filtered, washed with water 7 times the mass of the silver nanowires, and dried at 55°C for 14 hours to obtain modified silver nanowires. The modified silver nanowires were mixed with isopropanol at a mass ratio of 1:230 to obtain a modified silver nanowire / isopropanol mixed solution. The modified silver nanowire / isopropanol mixed solution was deposited on a substrate film layer by spin coating, and dried at 85°C for 15 minutes to obtain A substrate film layer having a modified silver nanowire network on its surface is coated with a glue layer material on one side of the substrate film layer having the modified silver nanowire network on its surface, wherein the coating thickness of the glue layer material is 5 μm, and an outer layer / barrier layer / intermediate layer composite material is covered, so that the side of the outer layer / barrier layer / intermediate layer composite material with polyaniline attached is in contact with the glue layer material, and the composite material is photocured in a nitrogen atmosphere under UV-LED ultraviolet light for 35 seconds, and the substrate film layer is peeled off to obtain a flexible conductive barrier film;
[0074] The substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm. The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
[0075] Example 3
[0076] This embodiment discloses a method for preparing a flexible conductive barrier film, comprising the following steps:
[0077] Step (1), washing the polyethylene terephthalate film with acetone, drying it at 55°C for 4 hours, treating both sides of the dried polyethylene terephthalate film with low-temperature argon / oxygen mixed plasma technology, the plasma discharge power is 130W, the treatment time is 500s, and after the treatment, a base film is obtained; immersing the base film in aniline, the mass ratio of the base film to the aniline is 1:10, after the immersion, taking out the base film attached with aniline, suspending it on the surface of a mixed solution of aniline / hydrochloric acid / ammonium persulfate, reacting it at room temperature for 7 hours, after the reaction is completed, adding water 7 times the mass of the base film for washing, and drying it at 45°C for 11 hours to obtain an intermediate layer material; one side of the intermediate layer material is attached with polyaniline;
[0078] The thickness of the base film is 40 μm, and the thickness of the intermediate layer material is 47 μm; the aniline / hydrochloric acid / ammonium persulfate mixed solution is prepared by mixing aniline, 1 mol / L hydrochloric acid aqueous solution, and 0.36 mol / L ammonium persulfate aqueous solution, and in the solute of the aniline / hydrochloric acid / ammonium persulfate mixed solution, the molar ratio of aniline, the solute hydrogen chloride in the 1 mol / L hydrochloric acid aqueous solution, and the solute ammonium persulfate in the 0.36 mol / L ammonium persulfate aqueous solution is 1:20:1;
[0079] Step (2), preparation of the barrier layer / intermediate layer composite material is the same as in Example 1;
[0080] Step (3), polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate are mixed, and the mixture is reacted for a first time at 65° C. in a nitrogen atmosphere for 3.5 hours. After the reaction is completed, 1,4-butanediol and 3-methyl-1,5-pentanediol are added, and the mixture is reacted for a second time at 75° C. for 1.8 hours. After the reaction is completed, pentaerythritol triacrylate and hydroxyethyl acrylate are added, and the mixture is reacted for a third time at 75° C. for 1.5 hours. After the reaction is completed, polyurethane acrylate is obtained;
[0081] The molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate, and 2-hydroxyethyl acrylate is 1:1:1:0.45:0.35:0.1:0.2, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol;
[0082] Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin for 25 minutes. After the addition is completed, the mixture is reacted at 95° C. for 3.5 hours. After the reaction is completed, a modified epoxy resin is obtained;
[0083] Among them, the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole, and epoxy resin is 165:0.28:0.8:270;
[0084] Modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator are mixed in a mass ratio of 15:35:50:2.5 under light-proof conditions to obtain an outer layer material, and the outer layer material is coated on the barrier layer surface of the barrier layer / intermediate layer composite material, the coating thickness of the outer layer material is 1 μm, and the outer layer material is photocured for 2 minutes under UV-LED ultraviolet light in a nitrogen atmosphere to obtain an outer layer / barrier layer / intermediate layer composite material;
[0085] Step (4), mixing water, xylene and polyurethane acrylate uniformly, adding dodecylbenzene sulfonic acid and continuing mixing for 18 minutes, adding aniline, and dripping 1.2 mol / L ammonium persulfate aqueous solution for 18 minutes. After the dripping is completed, reacting at 2°C for 7 hours. After the reaction is completed, drying at 55°C for 21 hours to obtain modified polyurethane acrylate;
[0086] The polyurethane acrylate is prepared in step (2), and the mass ratio of dodecylbenzenesulfonic acid, water, xylene, polyurethane acrylate, aniline, and 1.2 mol / L ammonium persulfate aqueous solution is 42:55:95:20:25:105;
[0087] Isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile are mixed in a mass ratio of 125:15:12.2:9:4.5:200:0.18, and reacted at 70°C for 21 hours. After the reaction, modified polyacrylate is obtained; modified polyacrylate, modified polyurethane acrylate, and photoinitiator are mixed in a mass ratio of 7:93:1 under light-proof conditions to obtain a glue layer material;
[0088] Silver nanowires, 3-mercaptopropionic acid, and water were mixed and stirred at a mass ratio of 1:1:300 for 12 hours, centrifuged, filtered, washed with water 7 times the mass of the silver nanowires, and dried at 55°C for 14 hours to obtain modified silver nanowires. The modified silver nanowires were mixed with isopropanol at a mass ratio of 1:240 to obtain a modified silver nanowire / isopropanol mixed solution. The modified silver nanowire / isopropanol mixed solution was deposited on a substrate film layer by spin coating, and dried at 85°C for 15 minutes to obtain A substrate film layer having a modified silver nanowire network on its surface is coated with a glue layer material on one side of the substrate film layer having the modified silver nanowire network on its surface, wherein the coating thickness of the glue layer material is 6 μm, and an outer layer / barrier layer / intermediate layer composite material is covered, so that the side of the outer layer / barrier layer / intermediate layer composite material with polyaniline attached is in contact with the glue layer material, and the composite material is photocured in a nitrogen atmosphere under UV-LED ultraviolet light for 35 seconds, and the substrate film layer is peeled off to obtain a flexible conductive barrier film;
[0089] The substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm. The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
[0090] Example 4
[0091] This embodiment discloses a method for preparing a flexible conductive barrier film, comprising the following steps:
[0092] Step (1), washing the polyethylene terephthalate film with acetone, drying it at 60°C for 3h, treating both sides of the dried polyethylene terephthalate film with low-temperature argon / oxygen mixed plasma technology, wherein the plasma discharge power is 140W and the treatment time is 550s, and after the treatment, a base film is obtained; immersing the base film in aniline, wherein the mass ratio of the base film to the aniline is 1:10, after the immersion, taking out the base film attached with aniline, suspending it on the surface of a mixed solution of aniline / hydrochloric acid / ammonium persulfate, reacting it at room temperature for 7.5h, and after the reaction is completed, adding water 6 times the mass of the base film for washing, and drying it at 45°C for 11h to obtain an intermediate layer material; wherein one side of the intermediate layer material is attached with polyaniline;
[0093] The thickness of the base film is 40 μm, and the thickness of the intermediate layer material is 48 μm; the aniline / hydrochloric acid / ammonium persulfate mixed solution is prepared by mixing aniline, 1 mol / L hydrochloric acid aqueous solution, and 0.36 mol / L ammonium persulfate aqueous solution, and in the solute of the aniline / hydrochloric acid / ammonium persulfate mixed solution, the molar ratio of aniline, the solute hydrogen chloride in the 1 mol / L hydrochloric acid aqueous solution, and the solute ammonium persulfate in the 0.36 mol / L ammonium persulfate aqueous solution is 1:20:1;
[0094] Step (2), preparation of the barrier layer / intermediate layer composite material is the same as in Example 1;
[0095] Step (3), polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate are mixed, and the mixture is reacted for a first time at 68° C. in a nitrogen atmosphere for 3 hours. After the reaction is completed, 1,4-butanediol and 3-methyl-1,5-pentanediol are added, and the mixture is reacted for a second time at 75° C. for 1.8 hours. After the reaction is completed, pentaerythritol triacrylate and hydroxyethyl acrylate are added, and the mixture is reacted for a third time at 80° C. for 1 hour. After the reaction is completed, polyurethane acrylate is obtained;
[0096] The molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate, and 2-hydroxyethyl acrylate is 1:1:1:0.48:0.38:0.1:0.25, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol;
[0097] Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin for 30 minutes. After the addition is completed, the mixture is reacted at 100° C. for 3 hours. After the reaction is completed, a modified epoxy resin is obtained;
[0098] Among them, the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole, and epoxy resin is 170:0.29:0.82:285;
[0099] Modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator are mixed in a mass ratio of 18:38:50:2.8 under light-proof conditions to obtain an outer layer material, and the outer layer material is coated on the barrier layer surface of the barrier layer / intermediate layer composite material, the coating thickness of the outer layer material is 2 μm, and the outer layer material is photocured for 2 minutes under UV-LED ultraviolet light in a nitrogen atmosphere to obtain an outer layer / barrier layer / intermediate layer composite material;
[0100] Step (4), mixing water, xylene and polyurethane acrylate evenly, adding dodecylbenzene sulfonic acid and continuing mixing for 20 minutes, adding aniline, and dripping 1.2 mol / L ammonium persulfate aqueous solution for 15 minutes. After the dripping is completed, reacting at 4°C for 7 hours. After the reaction is completed, drying at 60°C for 18 hours to obtain modified polyurethane acrylate;
[0101] The polyurethane acrylate is prepared in step (2), and the mass ratio of dodecylbenzenesulfonic acid, water, xylene, polyurethane acrylate, aniline, and 1.2 mol / L ammonium persulfate aqueous solution is 44:58:98:22:35:108;
[0102] Isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile are mixed in a mass ratio of 128:18:12.6:9.5:4.8:200:0.19, and reacted at 72°C for 20 hours. After the reaction, modified polyacrylate is obtained; modified polyacrylate, modified polyurethane acrylate, and photoinitiator are mixed in a mass ratio of 8:92:1 under light-proof conditions to obtain a glue layer material;
[0103] Silver nanowires, 3-mercaptopropionic acid, and water were mixed and stirred at a mass ratio of 1:1:300 for 12 h, centrifuged, filtered, washed with water 6 times the mass of the silver nanowires, and dried at 60°C for 12 h to obtain modified silver nanowires. The modified silver nanowires were mixed with isopropanol at a mass ratio of 1:250 to obtain a modified silver nanowire / isopropanol mixed solution. The modified silver nanowire / isopropanol mixed solution was deposited on a substrate film layer by spin coating, and dried at 80°C for 20 min to obtain A substrate film layer having a modified silver nanowire network on its surface is coated with a glue layer material on one side of the substrate film layer having the modified silver nanowire network on its surface, wherein the coating thickness of the glue layer material is 6 μm, and an outer layer / barrier layer / intermediate layer composite material is covered, so that the side of the outer layer / barrier layer / intermediate layer composite material with polyaniline attached is in contact with the glue layer material, and the composite material is photocured in a nitrogen atmosphere under UV-LED ultraviolet light for 38 seconds, and the substrate film layer is peeled off to obtain a flexible conductive barrier film;
[0104] The substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm. The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
[0105] Example 5
[0106] This embodiment discloses a method for preparing a flexible conductive barrier film, comprising the following steps:
[0107] Step (1), washing the polyethylene terephthalate film with acetone, drying it at 50°C for 5h, treating both sides of the dried polyethylene terephthalate film with low-temperature argon / oxygen mixed plasma technology, wherein the plasma discharge power is 150W and the treatment time is 400s, and after the treatment, a base film is obtained; immersing the base film in aniline, wherein the mass ratio of the base film to the aniline is 1:10, after the immersion, taking out the base film attached with aniline, suspending it on the surface of a mixed solution of aniline / hydrochloric acid / ammonium persulfate, reacting it at room temperature for 8h, and after the reaction is completed, adding water 8 times the mass of the base film for washing, and drying it at 40°C for 12h to obtain an intermediate layer material; wherein one side of the intermediate layer material is attached with polyaniline;
[0108] The thickness of the base film is 40 μm, and the thickness of the intermediate layer material is 50 μm; the aniline / hydrochloric acid / ammonium persulfate mixed solution is prepared by mixing aniline, 1 mol / L hydrochloric acid aqueous solution, and 0.36 mol / L ammonium persulfate aqueous solution, and in the solute of the aniline / hydrochloric acid / ammonium persulfate mixed solution, the molar ratio of aniline, the solute hydrogen chloride in the 1 mol / L hydrochloric acid aqueous solution, and the solute ammonium persulfate in the 0.36 mol / L ammonium persulfate aqueous solution is 1:20:1;
[0109] Step (2), preparation of the barrier layer / intermediate layer composite material is the same as in Example 1;
[0110] Step (3), polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate are mixed, and the mixture is reacted for a first time at 70° C. in a nitrogen atmosphere for 3 hours. After the reaction is completed, 1,4-butanediol and 3-methyl-1,5-pentanediol are added, and the mixture is reacted for a second time at 80° C. for 1.5 hours. After the reaction is completed, pentaerythritol triacrylate and hydroxyethyl acrylate are added, and the mixture is reacted for a third time at 80° C. for 1 hour. After the reaction is completed, polyurethane acrylate is obtained;
[0111] The molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate and 2-hydroxyethyl acrylate is 1:1:1:0.4:0.4:0.1:0.1, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol;
[0112] Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin for 30 minutes. After the addition is completed, the mixture is reacted at 90° C. for 4 hours. After the reaction is completed, a modified epoxy resin is obtained;
[0113] Wherein, the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole and epoxy resin is 180:0.3:0.85:300;
[0114] Modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator are mixed in a mass ratio of 20:30:50:3 under light-proof conditions to obtain an outer layer material, and the outer layer material is coated on the barrier layer surface of the barrier layer / intermediate layer composite material, the coating thickness of the outer layer material is 2 μm, and the outer layer material is photocured for 2 minutes under UV-LED ultraviolet light in a nitrogen atmosphere to obtain an outer layer / barrier layer / intermediate layer composite material;
[0115] Step (4), mixing water, xylene and polyurethane acrylate evenly, adding dodecylbenzene sulfonic acid and continuing mixing for 20 minutes, adding aniline, and dripping 1.2 mol / L ammonium persulfate aqueous solution for 20 minutes. After the dripping is completed, reacting at 5°C for 6 hours. After the reaction is completed, drying at 60°C for 18 hours to obtain modified polyurethane acrylate;
[0116] The polyurethane acrylate is prepared in step (2), and the mass ratio of dodecylbenzenesulfonic acid, water, xylene, polyurethane acrylate, aniline, and 1.2 mol / L ammonium persulfate aqueous solution is 45:60:100:25:40:110;
[0117] Isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile are mixed in a mass ratio of 130:20:13:10:5:200:0.2, and reacted at 75°C for 18 hours. After the reaction, modified polyacrylate is obtained; modified polyacrylate, modified polyurethane acrylate, and photoinitiator are mixed in a mass ratio of 10:90:1 under light-proof conditions to obtain a glue layer material;
[0118] Silver nanowires, 3-mercaptopropionic acid, and water were mixed and stirred at a mass ratio of 1:1:300 for 12 h, centrifuged, filtered, washed with water 8 times the mass of the silver nanowires, and dried at 50°C for 16 h to obtain modified silver nanowires. The modified silver nanowires were mixed with isopropanol at a mass ratio of 1:260 to obtain a modified silver nanowire / isopropanol mixed solution. The modified silver nanowire / isopropanol mixed solution was deposited on a substrate film layer by spin coating, and dried at 90°C for 10 min to obtain A substrate film layer having a modified silver nanowire network on its surface is coated with a glue layer material on one side of the substrate film layer having the modified silver nanowire network on its surface, wherein the coating thickness of the glue layer material is 6 μm, and an outer layer / barrier layer / intermediate layer composite material is covered, so that the side of the outer layer / barrier layer / intermediate layer composite material with polyaniline attached is in contact with the glue layer material, and the composite material is photocured in a nitrogen atmosphere and UV-LED ultraviolet light for 40 seconds, and the substrate film layer is peeled off to obtain a flexible conductive barrier film;
[0119] The substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm. The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
[0120] Comparative Example 1
[0121] This comparative example discloses a method for preparing a flexible conductive barrier film, comprising the following steps:
[0122] Step (1), washing the polyethylene terephthalate film with acetone, drying it at 60°C for 3h, treating both sides of the dried polyethylene terephthalate film with low-temperature argon / oxygen mixed plasma technology, wherein the plasma discharge power is 100W and the treatment time is 600s, and after the treatment, a base film is obtained; immersing the base film in aniline, wherein the mass ratio of the base film to the aniline is 1:10, after the immersion, taking out the base film attached with aniline, suspending it on the surface of a mixed solution of aniline / hydrochloric acid / ammonium persulfate, reacting it at room temperature for 6h, and after the reaction is completed, adding water 6 times the mass of the base film for washing, and drying it at 50°C for 10h to obtain an intermediate layer material; one side of the intermediate layer material is attached with polyaniline;
[0123] The thickness of the base film is 40 μm, and the thickness of the intermediate layer material is 45 μm; the aniline / hydrochloric acid / ammonium persulfate mixed solution is prepared by mixing aniline, 1 mol / L hydrochloric acid aqueous solution, and 0.36 mol / L ammonium persulfate aqueous solution, and in the solute of the aniline / hydrochloric acid / ammonium persulfate mixed solution, the molar ratio of aniline, the solute hydrogen chloride in the 1 mol / L hydrochloric acid aqueous solution, and the solute ammonium persulfate in the 0.36 mol / L ammonium persulfate aqueous solution is 1:20:1;
[0124] Step (2), polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate are mixed, and the mixture is reacted for a first time at 60° C. in a nitrogen atmosphere for 4 hours. After the reaction is completed, 1,4-butanediol and 3-methyl-1,5-pentanediol are added, and the mixture is reacted for a second time at 70° C. for 2 hours. After the reaction is completed, pentaerythritol triacrylate and hydroxyethyl acrylate are added, and the mixture is reacted for a third time at 70° C. for 2 hours. After the reaction is completed, polyurethane acrylate is obtained;
[0125] The molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate, and 2-hydroxyethyl acrylate is 1:1:1:0.5:0.3:0.1:0.3, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol;
[0126] Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin for 20 minutes. After the addition is completed, the mixture is reacted at 100° C. for 3 hours. After the reaction is completed, a modified epoxy resin is obtained;
[0127] Wherein, the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole and epoxy resin is 150:0.25:0.75:250;
[0128] Modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator are mixed in a mass ratio of 10:40:50:2 under light-proof conditions to obtain an outer layer material, and the outer layer material is coated on the side of the middle layer material to which polyaniline is not attached, with a coating thickness of 1 μm. The outer layer material is photocured for 2 minutes under UV-LED ultraviolet light in a nitrogen atmosphere to obtain an outer layer / middle layer composite material;
[0129] Step (3), mixing water, xylene and polyurethane acrylate evenly, adding dodecylbenzene sulfonic acid and continuing mixing for 15 minutes, adding aniline, and dripping 1.2 mol / L ammonium persulfate aqueous solution for 15 minutes. After the dripping is completed, reacting at 0°C for 8 hours. After the reaction is completed, drying at 50°C for 24 hours to obtain modified polyurethane acrylate;
[0130] The polyurethane acrylate is prepared in step (2), and the mass ratio of dodecylbenzenesulfonic acid, water, xylene, polyurethane acrylate, aniline, and 1.2 mol / L ammonium persulfate aqueous solution is 40:50:85:16:10:100;
[0131] Isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile are mixed in a mass ratio of 120:10:11.5:7.5:4:200:0.15, and reacted at 65°C for 24 hours. After the reaction, modified polyacrylate is obtained; modified polyacrylate, modified polyurethane acrylate, and photoinitiator are mixed in a mass ratio of 5:95:1 under light-proof conditions to obtain a glue layer material;
[0132] Silver nanowires, 3-mercaptopropionic acid and water were mixed and stirred at a mass ratio of 1:1:300 for 12 hours, centrifuged, filtered, washed with water 6 times the mass of the silver nanowires, and dried at 60°C for 12 hours to obtain modified silver nanowires. The modified silver nanowires were mixed with isopropanol at a mass ratio of 1:220 to obtain a modified silver nanowire / isopropanol mixed solution. The modified silver nanowire / isopropanol mixed solution was deposited on a substrate film layer by spin coating, and dried at 80°C for 20 minutes to obtain a substrate film layer having a modified silver nanowire network on the surface. A glue layer material was coated on one side of the substrate film layer having the modified silver nanowire network on the surface of the substrate film layer having the modified silver nanowire network. The coating thickness of the glue layer material was 5 μm. An outer layer / middle layer composite material was covered so that the side of the outer layer / middle layer composite material with polyaniline was in contact with the glue layer material. The composite material was photocured for 30 seconds under UV-LED ultraviolet light in a nitrogen atmosphere, and the substrate film layer was peeled off to obtain a flexible conductive barrier film.
[0133] The substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm. The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
[0134] Comparative Example 2
[0135] This comparative example discloses a method for preparing a flexible conductive barrier film, comprising the following steps:
[0136] Step (1), washing the polyethylene terephthalate film with acetone, drying at 60°C for 3h, and subjecting both sides of the dried polyethylene terephthalate film to low-temperature argon / oxygen mixed plasma treatment, wherein the plasma discharge power is 100W and the treatment time is 600s, and after the treatment, an intermediate layer material is obtained;
[0137] Among them, the thickness of the middle layer material is 40μm;
[0138] Step (2), preparation of the barrier layer / intermediate layer composite material is the same as in Example 1;
[0139] Step (3), polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate are mixed, and the mixture is reacted for a first time at 60° C. in a nitrogen atmosphere for 4 hours. After the reaction, 1,4-butanediol and 3-methyl-1,5-pentanediol are added, and the mixture is reacted for a second time at 70° C. for 2 hours. After the reaction, pentaerythritol triacrylate and hydroxyethyl acrylate are added, and the mixture is reacted for a third time at 70° C. for 2 hours. After the reaction, polyurethane acrylate is obtained;
[0140] The molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate, and 2-hydroxyethyl acrylate is 1:1:1:0.5:0.3:0.1:0.3, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol;
[0141] Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin for 20 minutes. After the addition is completed, the mixture is reacted at 100° C. for 3 hours. After the reaction is completed, a modified epoxy resin is obtained;
[0142] Wherein, the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole and epoxy resin is 150:0.25:0.75:250;
[0143] Modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator are mixed in a mass ratio of 10:40:50:2 under light-proof conditions to obtain an outer layer material, and the outer layer material is coated on the barrier layer surface of the barrier layer / intermediate layer composite material, the coating thickness of the outer layer material is 1 μm, and the outer layer material is photocured for 2 minutes under UV-LED ultraviolet light in a nitrogen atmosphere to obtain an outer layer / barrier layer / intermediate layer composite material;
[0144] Step (4), mixing isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile in a mass ratio of 120:10:11.5:7.5:4:200:0.15, reacting at 65°C for 24 hours, and obtaining a modified polyacrylate after the reaction; mixing the modified polyacrylate, polyurethane acrylate, and a photoinitiator in a mass ratio of 5:95:1 under light-proof conditions to obtain a glue layer material; wherein the polyurethane acrylate is obtained in step (2);
[0145] Silver nanowires, 3-mercaptopropionic acid, and water were mixed and stirred at a mass ratio of 1:1:300 for 12 h, centrifuged, filtered, washed with water 6 times the mass of the silver nanowires, and dried at 60°C for 12 h to obtain modified silver nanowires. The modified silver nanowires were mixed with isopropanol at a mass ratio of 1:220 to obtain a modified silver nanowire / isopropanol mixed solution. The modified silver nanowire / isopropanol mixed solution was deposited on the substrate film layer by spin coating, and dried at 80°C for 20 min to obtain a surface A substrate film layer having a modified silver nanowire network, coating a glue layer material on the side of the substrate film layer having the modified silver nanowire network on the surface, wherein the coating thickness of the glue layer material is 5 μm, and covering the outer layer / barrier layer / intermediate layer composite material, so that the side of the outer layer / barrier layer / intermediate layer composite material not attached with the outer layer / barrier layer is in contact with the glue layer material, light curing for 30 seconds in a nitrogen atmosphere and UV-LED ultraviolet light, peeling off the substrate film layer, and obtaining a flexible conductive barrier film;
[0146] The substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm. The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
[0147] Comparative Example 3
[0148] This comparative example discloses a method for preparing a flexible conductive barrier film, comprising the following steps:
[0149] Step (1), washing the polyethylene terephthalate film with acetone, drying it at 60°C for 3h, treating both sides of the dried polyethylene terephthalate film with low-temperature argon / oxygen mixed plasma technology, wherein the plasma discharge power is 100W and the treatment time is 600s, and after the treatment, a base film is obtained; immersing the base film in aniline, wherein the mass ratio of the base film to the aniline is 1:10, after the immersion, taking out the base film attached with aniline, suspending it on the surface of a mixed solution of aniline / hydrochloric acid / ammonium persulfate, reacting it at room temperature for 6h, and after the reaction is completed, adding water 6 times the mass of the base film for washing, and drying it at 50°C for 10h to obtain an intermediate layer material; one side of the intermediate layer material is attached with polyaniline;
[0150] Step (2), preparation of the barrier layer / intermediate layer composite material is the same as in Example 1;
[0151] The thickness of the base film is 40 μm, and the thickness of the intermediate layer material is 45 μm; the aniline / hydrochloric acid / ammonium persulfate mixed solution is prepared by mixing aniline, 1 mol / L hydrochloric acid aqueous solution, and 0.36 mol / L ammonium persulfate aqueous solution, and in the solute of the aniline / hydrochloric acid / ammonium persulfate mixed solution, the molar ratio of aniline, the solute hydrogen chloride in the 1 mol / L hydrochloric acid aqueous solution, and the solute ammonium persulfate in the 0.36 mol / L ammonium persulfate aqueous solution is 1:20:1;
[0152] Step (3), polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate, and dibutyltin dilaurate are mixed, and the mixture is reacted for a first time at 60° C. in a nitrogen atmosphere for 4 hours. After the reaction, 1,4-butanediol and 3-methyl-1,5-pentanediol are added, and the mixture is reacted for a second time at 70° C. for 2 hours. After the reaction, pentaerythritol triacrylate and hydroxyethyl acrylate are added, and the mixture is reacted for a third time at 70° C. for 2 hours. After the reaction, polyurethane acrylate is obtained;
[0153] The molar ratio of polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate, and 2-hydroxyethyl acrylate is 1:1:1:0.5:0.3:0.1:0.3, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol;
[0154] Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin for 20 minutes. After the addition is completed, the mixture is reacted at 100° C. for 3 hours. After the reaction is completed, a modified epoxy resin is obtained;
[0155] Wherein, the mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole and epoxy resin is 150:0.25:0.75:250;
[0156] Modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator are mixed in a mass ratio of 10:40:50:2 under light-proof conditions to obtain an outer layer material, and the outer layer material is coated on the barrier layer surface of the barrier layer / intermediate layer composite material, the coating thickness of the outer layer material is 1 μm, and the outer layer material is photocured for 2 minutes under UV-LED ultraviolet light in a nitrogen atmosphere to obtain an outer layer / barrier layer / intermediate layer composite material;
[0157] Step (4), mixing water, xylene and polyurethane acrylate uniformly, adding dodecylbenzene sulfonic acid and continuing mixing for 15 minutes, adding aniline, and dripping 1.2 mol / L ammonium persulfate aqueous solution for 15 minutes. After the dripping is completed, reacting at 0°C for 8 hours. After the reaction is completed, drying at 50°C for 24 hours to obtain modified polyurethane acrylate; the modified polyurethane acrylate and the photoinitiator are mixed in a mass ratio of 100:1 under light-proof conditions to obtain a glue layer material;
[0158] The polyurethane acrylate is prepared in step (2), and the mass ratio of dodecylbenzenesulfonic acid, water, xylene, polyurethane acrylate, aniline, and 1.2 mol / L ammonium persulfate aqueous solution is 40:50:85:16:10:100;
[0159] Silver nanowires, 3-mercaptopropionic acid, and water were mixed and stirred at a mass ratio of 1:1:300 for 12 h, centrifuged, filtered, washed with water 6 times the mass of the silver nanowires, and dried at 60°C for 12 h to obtain modified silver nanowires. The modified silver nanowires were mixed with isopropanol at a mass ratio of 1:220 to obtain a modified silver nanowire / isopropanol mixed solution. The modified silver nanowire / isopropanol mixed solution was deposited on a substrate film layer by spin coating, and dried at 80°C for 20 min to obtain A substrate film layer having a modified silver nanowire network on its surface is coated with a glue layer material on one side of the substrate film layer having the modified silver nanowire network on its surface, wherein the coating thickness of the glue layer material is 5 μm, and an outer layer / barrier layer / intermediate layer composite material is covered, so that the side of the outer layer / barrier layer / intermediate layer composite material with polyaniline attached is in contact with the glue layer material, and the composite material is photocured in a nitrogen atmosphere and UV-LED ultraviolet light for 30 seconds, and the substrate film layer is peeled off to obtain a flexible conductive barrier film;
[0160] The substrate film layer is a polyethylene terephthalate film with a thickness of 150 μm. The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
[0161] In the above embodiments and comparative examples: aniline is from Shanghai Aladdin Biochemical Technology Co., Ltd., item number A112125, CAS number: 62-53-3; hydrochloric acid aqueous solution is from Shanghai Yuanye Biotechnology Co., Ltd., item number B62243, model hydrogen chloride standard solution; ammonium persulfate is from Nanjing Chemical Reagent Co., Ltd., CAS number: 7727-54-0; trimethylaluminum is from Hubei Taihechang Biotechnology Co., Ltd., CAS number: 75-24-1; titanium tetrachloride is from Hubei Xinghengye Technology Co., Ltd., CAS number: 7550-45-0; polymethyl methacrylate is from Yongkuan Chemical Co., Ltd., item number FP6731, CAS number: 9011-14-7; polycarbonate diol is from Hubei Maidehao Chemical Co., Ltd., product name Ube Eternacoll PH-100; isophorone diisocyanate comes from Shandong New Kinetic Energy Chemical Co., Ltd., CAS number: 4098-71-9; hexamethylene diisocyanate comes from Jinan Hongyao Chemical Co., Ltd., CAS number: 822-06-0; dibutyltin dilaurate comes from Maoming Xiongda Chemical Co., Ltd., CAS number: 77-58-7; 1,4-butanediol comes from Shandong Huibang New Materials Technology Co., Ltd., CAS number: 110-63-4; 3-methyl-1,5-pentanediol comes from Jiangsu Youlixin Chemical Co., Ltd., CAS number: 4457-71-0; pentaerythritol triacrylate comes from Hubei Xingyan New Materials Technology Co., Ltd., CAS number: : 3524-68-3; hydroxyethyl acrylate comes from Shandong Chuangying Chemical Co., Ltd., CAS number: 818-61-1; acrylic acid comes from Shandong Mingyue Chemical Co., Ltd., CAS number: 79-10-7; tetramethylammonium chloride comes from Jinan Yuyi Chemical Co., Ltd., CAS number: 75-57-0; p-Hydroxyanisole comes from Shandong Xinghai Chemical Co., Ltd., CAS number: 150-76-5; epoxy resin comes from Jiaozuo Xinjing Technology Co., Ltd., product name epoxy resin UVR-6103; trimethylolpropane trimethacrylate comes from Jinan Yuyi Chemical Co., Ltd., CAS number: 3290-92-4; photoinitiator comes from Nanjing Milan New Materials Co., Ltd., product name photoinitiator 184, CAS number: 94 7-19-3; xylene comes from Chengdu Zhongsheng Jinhong Chemical Co., Ltd.; dodecylbenzene sulfonic acid comes from Shandong Runyue Chemical Co., Ltd., CAS number: 27176-87-0; isooctyl acrylate comes from Shanghai Nanmu Chemical Co., Ltd., CAS number: 29590-42-9; β-carboxyethyl acrylate comes from Zhongshan Dixin Chemical Co., Ltd., CAS number: 24615-84-7; vinyl trimethoxysilane comes from Shandong Yuanjin New Materials Co., Ltd., product name silane coupling agent A171, CAS number: 2768-02-7; ethyl acetate comes from Shandong Huayu Chemical Technology Co., Ltd., CAS number: 141-78-6; butanone comes from Zibo Jinshuo Chemical Co., Ltd., CAS number: 78-93-3;Azobisisobutyronitrile comes from Jinan Sibet Chemical Co., Ltd., CAS No.: 78-67-1; silver nanowires come from Beijing Zhongke Keyou Technology Co., Ltd., with an average diameter of 40nm and an average length of 35μm; 3-mercaptopropionic acid comes from Shandong Guohua Chemical Co., Ltd., CAS No.: 107-96-0; isopropanol comes from Wuxi Jingke Chemical Co., Ltd., CAS No.: 67-63-0. ;
[0162] Test example
[0163] (1) Comprehensive performance test
[0164] The comprehensive properties of the flexible conductive barrier films prepared in Examples 1-5 and Comparative Examples 1-3 were tested. The specific test results are shown in Table 1:
[0165] Table 1
[0166] ;
[0167] The tests of the indicators in Table 1 are based on the following standards: water vapor transmission rate is measured by GB / T21529-2008 "Electrolytic sensor method for determination of water vapor transmission rate of plastic films and sheets"; sheet resistance is measured with reference to GB / T 26598-2011 "Specification for transparent conductive films for optical instruments", among which, the instrument used for the bending operation is an electric bending instrument with a curvature radius of 5 mm and a bending frequency of 30 min. -1 The interlayer peel strength is measured with reference to GBT2792-2014 "Test method for peel strength of adhesive tape".
[0168] It can be seen from the test results in Table 1 that the flexible conductive barrier film prepared in the present invention has excellent barrier properties and electrical conductivity, and has high interlayer peeling strength and is not easy to delaminate.
[0169] The present invention modifies the PET film by low-temperature plasma treatment, thereby increasing the surface area of the PET film and increasing polar groups such as hydroxyl groups on the film surface, thereby increasing the bonding performance between the obtained modified base film and other film layers; and polymerizing aniline on one side of the modified base film by chemical oxidation polymerization, so that the obtained polyaniline layer and the modified base film can have an excellent bonding effect without adding an adhesive. By alternately depositing inorganic film layers and organic film layers on the side of the modified base film without polyaniline by atomic layer deposition, the obtained inorganic / organic composite film layer has excellent adhesion to the modified base film, and because the inorganic film layer in the inorganic / organic composite film layer is formed by combining aluminum oxide film and titanium dioxide film to form a multilayer structure, this structure can reduce the continuous diffusion path of water vapor in the film, thereby reducing the water vapor permeability, and the composite use of aluminum oxide film and titanium dioxide film can further improve the chemical stability and barrier properties of the inorganic film layer; the insertion of the organic film layer into the inorganic film layer can prevent defects from growing through the inorganic layer, and provide a smooth surface for subsequent inorganic film layer deposition, which can further increase the barrier properties of the composite film layer, while increasing the flexibility of the inorganic / organic composite film layer, and the obtained barrier layer has high barrier properties while maintaining good softness.
[0170] The present invention modifies the epoxy resin to have double bonds, and can achieve photocuring by adding a photoinitiator. The epoxy resin is mixed and modified with polyurethane acrylate to improve the heat resistance and weather resistance of the polyurethane acrylate, while maintaining good softness. The epoxy resin is used as an outer layer material and coated on the side of the barrier layer to which polyaniline is not attached. After photocuring, the barrier layer can be protected and the weather resistance of the barrier layer can be improved.
[0171] In the present invention, polyaniline is synthesized in polyurethane acrylic resin to make the obtained modified polyurethane acrylate have conductivity. By adding modified polyacrylate having carboxyl groups and siloxane segments into the modified polyurethane acrylate, on the one hand, the conductivity of polyaniline can be improved, and on the other hand, the siloxane segments of the modified polyacrylate can improve the softness of the adhesive layer material and reduce the influence of polar groups on the flexibility of the adhesive layer material. In addition, the carboxyl groups in the modified polyacrylate can enhance the bonding performance of the adhesive layer material and improve the bonding between the adhesive layer material and the adjacent layer material.
[0172] The present invention uses 3-mercaptopropionic acid to modify the surface of silver nanowires, thereby improving the dispersibility of the silver nanowires. At the same time, due to the interaction between the modified silver nanowires and the carboxyl groups in the adhesive layer material, the silver nanowires are tightly compounded with the adhesive layer material and are not easy to peel off. At the same time, the adhesive layer material also protects the silver nanowires and is not easily affected by external forces to damage the conductive properties of the film. After the various layers of materials are compounded and photocured, a flexible conductive barrier film is obtained. Since the use of adhesive is reduced, the overall thickness of the film is reduced, so that the flexible conductive barrier film is more flexible and has excellent barrier properties and conductivity.
[0173] Comparative Example 1 does not have a barrier layer and lacks the multilayer structure of the inorganic / organic composite film layer in the barrier layer. This structure can reduce the continuous diffusion path of water vapor in the film, thereby reducing the water vapor permeability, and the composite use of aluminum oxide film and titanium dioxide film can further improve the chemical stability and barrier properties of the inorganic film layer; the insertion of the organic film layer into the inorganic film layer can prevent defects from growing through the inorganic layer and provide a smooth surface for subsequent inorganic film layer deposition, which can further increase the barrier properties of the composite film layer, so the barrier properties of Comparative Example 1 are lower than those of the embodiment.
[0174] In the preparation process of the intermediate layer of Comparative Example 2, polyaniline is not added, and polyaniline is not added to the adhesive layer material. Due to the lack of the enhancement effect of polyaniline on the conductivity of the film, the square resistance of Comparative Example 2 is higher than that of the embodiment, and the conductivity is lower than that of the embodiment.
[0175] In comparative example 3, no modified polyacrylate is added to the adhesive layer material. Since the carboxyl group in the modified polyacrylate can enhance the bonding performance of the adhesive layer material and improve the bonding between the adhesive layer material and the adjacent layer material, the bonding performance of the adhesive layer material without the addition of modified polyacrylate is reduced. Therefore, the interlayer peeling strength of comparative example 3 is lower than that of the embodiment.
[0176] Although embodiments of the present invention have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present invention, and that the scope of the present invention is defined by the appended claims and their equivalents.
Claims
1. A method for preparing a flexible conductive barrier film, characterized in that: The following steps are involved: Step (1), washing the polyethylene terephthalate film with acetone, drying, and treating both sides of the dried polyethylene terephthalate film with a low-temperature argon / oxygen mixed plasma technology to obtain a base film; immersing the base film in aniline, taking out the base film with aniline attached after immersion, suspending it on the surface of an aniline / hydrochloric acid / ammonium persulfate mixed solution, reacting, and washing and drying after the reaction is completed to obtain an intermediate layer material; Step (2), using an atomic layer deposition method to alternately deposit an aluminum oxide film and a titanium dioxide film on the side of the intermediate layer material that is not attached with polyaniline, and after the deposition, attaching a layer of polymethyl methacrylate through an inkjet printing system, and forming a polymethyl methacrylate film after photocuring, and repeating the deposition, inkjet printing, and photocuring operations three times to obtain a barrier layer / intermediate layer composite material; Step (3), mixing the modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate, and a photoinitiator under light-proof conditions to obtain an outer layer material, coating the outer layer material on the barrier layer surface of the barrier layer / intermediate layer composite material, and light curing to obtain an outer layer / barrier layer / intermediate layer composite material; The mass ratio of modified epoxy resin, polyurethane acrylate, trimethylolpropane trimethacrylate and photoinitiator is 10-20:30-40:50:2-3; the coating thickness of the outer layer material is 1-2 μm; the photocuring conditions are: photocuring for 2 minutes in a nitrogen atmosphere and UV-LED ultraviolet light; Wherein, the modified epoxy resin is prepared by the following steps: Acrylic acid, tetramethylammonium chloride and p-hydroxyanisole are mixed and dissolved to obtain an acrylic acid mixed solution, and the acrylic acid mixed solution is added dropwise to the epoxy resin. After the addition is completed, the mixture is reacted to obtain a modified epoxy resin. The mass ratio of acrylic acid, tetramethylammonium chloride, p-hydroxyanisole and epoxy resin is 150-180:0.25-0.3:0.75-0.85:250-300. The dropping time of the acrylic acid mixed solution is 20-30 minutes. The reaction conditions are: reacting at a temperature of 90-100°C for 3-4 hours. Polyurethane acrylate is prepared by the following steps: The polycarbonate diol, isophorone diisocyanate, hexamethylene diisocyanate and dibutyltin dilaurate are mixed, and the reaction is performed for the first time. After the reaction is completed, 1,4-butanediol and 3-methyl-1,5-pentanediol are added. After the reaction is completed for the second time, pentaerythritol triacrylate and hydroxyethyl acrylate are added. After the reaction is completed for the third time, polyurethane acrylate is obtained. The polycarbonate diol, isophorone diisocyanate, 1,6-hexamethylene diisocyanate, 1,4-butanediol, 3-methyl-1,5-pentanediol, pentaerythritol triacrylate and hydroxyethyl acrylate are added. The molar ratio of tetraol triacrylate and 2-hydroxyethyl acrylate is 1:1:1:0.4-0.5:0.3-0.4:0.1:0.1-0.3, and the amount of dibutyltin dilaurate added is 0.05wt% of the mass of polycarbonate diol; the first reaction conditions are: in a nitrogen atmosphere, the first reaction is at a temperature of 60-70°C for 3-4h; the second reaction conditions are: at a temperature of 70-80°C for 1.5-2h; the third reaction conditions are: at a temperature of 70-80°C for 1-2h; Step (4), mixing isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone, and azobisisovaleronitrile, and reacting them to obtain modified polyacrylate; mixing the modified polyacrylate, modified polyurethane acrylate, and a photoinitiator under light-proof conditions to obtain a glue layer material; The mass ratio of isooctyl acrylate, hydroxyethyl acrylate, β-carboxyethyl acrylate, vinyl trimethoxysilane, ethyl acetate, butanone and azobisisovaleronitrile is 120-130:10-20:11.5-13:7.5-10:4-5:200:0.15-0.2; the reaction conditions are: react at 65-75°C for 18-24h; the mass ratio of modified polyacrylate, modified polyurethane acrylate and photoinitiator is 5-10:90-95:1; Wherein, the modified polyurethane acrylate is prepared by the following steps: Mix water, xylene and polyurethane acrylate evenly, add dodecylbenzene sulfonic acid and continue mixing, add aniline, dropwise add ammonium persulfate aqueous solution, react after the dropwise addition is complete, and dry after the reaction is complete to obtain modified polyurethane acrylate; The polyurethane acrylate is the same as the polyurethane acrylate described in step (3); the mass ratio of dodecylbenzenesulfonic acid, water, xylene, polyurethane acrylate, aniline, and ammonium persulfate aqueous solution is 40-45:50-60:85-100:16-25:10-40:100-110; the ammonium persulfate aqueous solution is 1.2 mol / L ammonium persulfate aqueous solution, and the dropwise addition time is 15-20 min; the reaction conditions are: react at a temperature of 0-5°C for 6-8 h; Silver nanowires, 3-mercaptopropionic acid and water are mixed and stirred, centrifuged, filtered, washed and dried to obtain modified silver nanowires, the modified silver nanowires are mixed with isopropanol to obtain a modified silver nanowire / isopropanol mixed solution, the modified silver nanowire / isopropanol mixed solution is deposited on a substrate film layer to obtain a substrate film layer having a modified silver nanowire network on the surface, a glue layer material is coated on the side having the modified silver nanowire network on the substrate film layer having the modified silver nanowire network on the surface, an outer layer / barrier layer / middle layer composite material is covered, a side of the outer layer / barrier layer / middle layer composite material with polyaniline is brought into contact with the glue layer material, photocuring is performed, and the substrate film layer is peeled off to obtain a flexible conductive barrier film.
2. The method for preparing a flexible conductive barrier film according to claim 1, characterized in that: In the step (1), the conditions for the low-temperature argon / oxygen mixed plasma technology treatment are: the plasma discharge power is 100-150 W, the treatment time is 400-600 s; the thickness of the base film is 40 μm, and the mass ratio of the base film to aniline is 1:10; the reaction conditions are: react at room temperature for 6-8 hours; the thickness of the intermediate layer material is 45-50 μm.
3. The method for preparing a flexible conductive barrier film according to claim 1, characterized in that: In the step (2), the precursor materials used in the atomic layer deposition method are trimethylaluminum, titanium tetrachloride and distilled water at room temperature, the temperature of film deposition is 80°C, the chamber pressure is 43 Pa, the carrier gas is nitrogen, the carrier gas volume is 300 mL / min, the thickness of the aluminum oxide film formed by a single deposition and the titanium dioxide film formed by a single deposition are both 5 nm, and the number of alternating depositions is 6 times; the photocuring conditions are: photocuring in a nitrogen atmosphere and UV-LED ultraviolet light for 30 seconds; the thickness of the polymethyl methacrylate film formed after a single inkjet printing and photocuring is 1 μm.
4. The method for preparing a flexible conductive barrier film according to claim 1, characterized in that: In the step (4), the mass ratio of silver nanowires, 3-mercaptopropionic acid and water is 1:1:300, and the stirring time is 12 hours; the coating thickness of the adhesive layer material is 5-6 μm; The light curing conditions are: light curing in a nitrogen atmosphere and UV-LED ultraviolet light for 30-40 seconds; The deposition operation includes: depositing the modified silver nanowire / isopropanol mixed solution on the substrate film layer by spin coating, and drying at a temperature of 80-90° C. for 10-20 minutes; The spin coating parameters of the spin coating method are: slow spin coating speed is 400 r / min, time is 6 s, fast spin coating speed is 3500 r / min, time is 20 s, and the number of spin coating deposition is 4 times.
5. A flexible conductive barrier film prepared by the method for preparing a flexible conductive barrier film according to any one of claims 1 to 4.
6. Use of the flexible conductive barrier film as claimed in claim 5.