A PP film and preparation method thereof

By using polypropylene resin, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer and nanozirconium silicate in polypropylene films, combined with extrusion and stretching processes, the The poor performance of polypropylene films under low temperature conditions has significantly improved its toughness and low temperature resistance and improved its application prospects.

CN118421006BActive Publication Date: 2024-11-05HUIZHOU TIANBO KEXING THIN FILM TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410652760.4
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-23
Publication Date
2024-11-05
Estimated Expiration
2044-05-23

AI Technical Summary

Technical Problem

The poor performance of polypropylene films under low temperature conditions, especially the low impact strength of low temperature limits its application range, and the low temperature resistance performance of the prior art below 0°C cannot be effectively solved.

Method used

The combination of polypropylene resin, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, silane coupling agent and nanozirconium silicate, nano aluminum silicate and nanomagnesium silicate combined filler, through The twin-screw extrusion and tensile process prepares PP films to form a multi-layer composite structure to enhance its toughness and low temperature resistance.

Benefits of technology

It significantly improves the toughness and low temperature resistance of PP films, enhances its tensile strength and impact damage quality at -50℃ and 23℃, and provides better comprehensive performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0004856916760000101
    Figure BDA0004856916760000101
Patent Text Reader

Abstract

The invention discloses a PP film and a preparation method thereof. The PP film comprises: 80-90 parts of a polypropylene resin, 10-20 parts of a maleic anhydride-modified polypropylene resin, 5-15 parts of a polyethylene resin, 2-7 parts of an ethylene-vinyl acetate copolymer, 3-10 parts of a filler, 3-7 parts of a silane coupling agent and 2-7 parts of an antioxidant; the filler is a composition of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate in a weight ratio of 1:2-7:1-3; the preparation method of the application obtains a polypropylene film by blending and granulating raw materials of various components, extruding and stretching the raw materials, and the polypropylene film has excellent tensile strength and low-temperature impact performance; the application also provides a multi-layer composite PP film, which further enhances the mechanical properties of the film; the PP film provided by the invention has excellent comprehensive performance and good application prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polypropylene films, and in particular to a PP film and a preparation method thereof. Background Art

[0002] PP is a thermoplastic resin that is non-toxic, odorless and tasteless. It is widely used in the automotive industry, home appliances, electronics, packaging, building materials and furniture.

[0003] However, in the actual processing and application process, it was found that polypropylene film materials generally have shortcomings such as poor low-temperature performance and low low-temperature impact strength. The existence of these problems has greatly limited the application and development of polypropylene film materials.

[0004] Patent CN114989532B discloses an ultra-low temperature heat-sealing material for polypropylene film, a preparation method and an application thereof, which is obtained by vulcanization extrusion granulation of copolymerized polypropylene, polyoleamide, low-density polyethylene, elastomer, vulcanizing agent and antioxidant, and has the advantages of low heat-sealing temperature, wide temperature range, high hot adhesive strength and good light transmittance. However, the initial heat-sealing disclosed in the patent is below 75°C, and it is unknown whether the low-temperature resistance at lower temperatures, such as below 0°C, can meet the use requirements.

[0005] Therefore, it is necessary to continue to develop new polypropylene film materials, further improve the low-temperature performance of polypropylene film materials, and enhance their low-temperature resistance. Summary of the invention

[0006] The purpose of the present invention is to provide a PP film and a preparation method thereof, so as to improve its low temperature resistance, enhance its tensile strength, enhance its toughness, and make it have better low temperature resistance.

[0007] To this end, the present invention adopts the following technical solution:

[0008] In a first aspect, the present invention provides a PP film, comprising the following raw materials in parts by weight: 80-90 parts of polypropylene resin, 10-20 parts of maleic anhydride modified polypropylene resin, 5-15 parts of polyethylene resin, 2-7 parts of ethylene-vinyl acetate copolymer, 3-10 parts of filler, 3-7 parts of silane coupling agent and 2-7 parts of antioxidant; the filler is a composition of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, and the weight ratio of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 1:2-7:1-3.

[0009] Preferably, the weight ratio of the polypropylene resin: maleic anhydride modified polypropylene resin: polyethylene resin: ethylene-vinyl acetate copolymer is 4-6:1:0.5-1:0.25-0.48.

[0010] Preferably, the silane coupling agent includes one or more of γ-ureidopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropyltriethoxysilane.

[0011] Preferably, the antioxidant is any one of a hindered phenol antioxidant, a phosphite antioxidant and a thioester antioxidant.

[0012] Furthermore, the PP film also includes 0.5-3 parts of a flame retardant and / or 1-3 parts of an antibacterial agent.

[0013] Preferably, the flame retardant is one or more of a sulfonate flame retardant, a phosphazene flame retardant, an organic phosphate ester and a silicon-based flame retardant.

[0014] Preferably, the antibacterial agent is at least one of nano-titanium dioxide and nano-silver antibacterial agent.

[0015] In a second aspect, the present invention further provides a method for preparing a PP film, comprising the following steps:

[0016] S1: Weigh polypropylene, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, filler, silane coupling agent and antioxidant according to the proportion, add them into a mixer, and stir for 0.5-1.5h;

[0017] S2: using a twin-screw extruder to extrude and granulate the material stirred in step 1 at a temperature of 180-240° C., and drying after granulation to obtain modified polypropylene masterbatch;

[0018] S3: adding the modified polypropylene masterbatch prepared in step 2 into a single screw extruder for extrusion, longitudinal stretching, and then transverse stretching or simultaneous longitudinal and transverse stretching to obtain a polypropylene film.

[0019] In a third aspect, the present invention provides a multi-layer composite PP film, which is obtained by hot pressing of a surface layer, an intermediate layer and an inner layer structure; the surface layer and the inner layer are respectively made of the raw materials described in the first aspect of the present invention, and the intermediate layer is made of maleic anhydride modified polypropylene resin.

[0020] Preferably, the raw material components of the PP films of the surface layer and the middle layer are the same or different.

[0021] Preferably, the thickness of the surface layer and the inner layer is 0.8-50 um, and the thickness of the middle layer is 10-100 um.

[0022] Compared with the prior art, the present invention has the following beneficial effects:

[0023] The present invention adopts polypropylene resin, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, silane coupling agent, and filler composed of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, so as to significantly enhance the toughness of the PP film, improve its low temperature resistance, and have excellent tensile strength and elongation at break.

[0024] The maleic anhydride modified polypropylene resin, polyethylene resin and ethylene-vinyl acetate copolymer of the present invention can synergistically enhance the transverse tensile strength, longitudinal tensile strength and impact breakage quality of the polypropylene resin at -50°C and 23°C.

[0025] The invention adopts a combination of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, controls the proportions of each within an appropriate range, and has the advantages of more significantly enhancing the transverse tensile strength, longitudinal tensile strength and impact breakage quality of polypropylene resin at -50°C and 23°C than conventional fillers.

[0026] The multilayer composite film provided by the present invention adopts polypropylene resin, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, silane coupling agent, and nano zirconium silicate, nano aluminum silicate and nano magnesium silicate composite filler as raw materials to make the surface layer and the inner layer, and maleic anhydride modified polypropylene resin is used to make the middle layer. The surface layer, the middle layer and the inner layer structure are co-extruded, which can more significantly enhance the transverse tensile strength, longitudinal tensile strength and impact damage quality of the polypropylene resin of the film at -50°C and 23°C.

[0027] In summary, the PP film provided by the present invention has excellent comprehensive properties and good application prospects. DETAILED DESCRIPTION

[0028] The specific implementation methods of the technical solution of this specification are further described below through specific examples. These examples are for the purpose of describing the technical solution in detail, rather than for limiting the technical solution. Based on the examples in this specification, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of this specification.

[0029] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art, and the reagents and materials used in the following examples are commercially available, including: polypropylene resin, model 2252E3; maleic anhydride grafted polypropylene, brand 50E806; ethylene-vinyl acetate copolymer, model VC640; polyethylene resin, brand 2420H.

[0030] In a first aspect of the present application, a PP film is provided, comprising the following raw materials in parts by weight: 80-90 parts of polypropylene resin, 10-20 parts of maleic anhydride modified polypropylene resin, 5-15 parts of polyethylene resin, 2-7 parts of ethylene-vinyl acetate copolymer, 3-10 parts of filler, 3-7 parts of silane coupling agent and 2-7 parts of antioxidant; the filler is a composition of nano-zirconium silicate, nano-aluminum silicate and nano-magnesium silicate, and the weight ratio of the nano-zirconium silicate, nano-aluminum silicate and nano-magnesium silicate is 1:2-7:1-3.

[0031] Preferably, the weight ratio of the polypropylene resin: maleic anhydride modified polypropylene resin: polyethylene resin: ethylene-vinyl acetate copolymer is 4-6:1:0.5-1:0.25-0.48.

[0032] Preferably, the silane coupling agent includes one or more of γ-ureidopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropyltriethoxysilane.

[0033] Preferably, the antioxidant is any one of a hindered phenol antioxidant, a phosphite antioxidant and a thioester antioxidant.

[0034] Furthermore, the PP film also includes 0.5-3 parts of a flame retardant and / or 1-3 parts of an antibacterial agent.

[0035] Preferably, the flame retardant is one or more of a sulfonate flame retardant, a phosphazene flame retardant, an organic phosphate ester and a silicon-based flame retardant.

[0036] Preferably, the antibacterial agent is at least one of nano-titanium dioxide and nano-silver antibacterial agent.

[0037] In a second aspect of the present application, a method for preparing a PP film is also provided, comprising the following steps:

[0038] S1: Weigh polypropylene, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, filler, silane coupling agent and antioxidant according to the proportion, add them into a mixer, and stir for 0.5-1.5h;

[0039] S2: using a twin-screw extruder to extrude and granulate the material stirred in step 1 at a temperature of 180-240° C., and drying after granulation to obtain modified polypropylene masterbatch;

[0040] S3: adding the modified polypropylene masterbatch prepared in step 2 into a single screw extruder for extrusion, longitudinal stretching, and then transverse stretching or simultaneous longitudinal and transverse stretching to obtain a polypropylene film.

[0041] In the third aspect of the present application, a multi-layer composite PP film is provided, wherein the multi-layer composite film is obtained by hot pressing of a surface layer, an intermediate layer and an inner layer structure; the surface layer and the inner layer are respectively made of the raw materials described in the first aspect above, and the intermediate layer is made of maleic anhydride modified polypropylene resin.

[0042] Preferably, the PP films of the surface layer and the middle layer are the same or different.

[0043] Preferably, the thickness of the surface layer and the inner layer is 0.8-50 um, and the thickness of the middle layer is 10-100 um.

[0044] Example 1

[0045] This embodiment provides a PP film, comprising the following raw materials in parts by weight: 80 parts of polypropylene resin, 15 parts of maleic anhydride modified polypropylene resin, 15 parts of polyethylene resin, 5 parts of ethylene-vinyl acetate copolymer, 10 parts of filler, 4 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 2 parts of antioxidant 1010.

[0046] The filler is a composition of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, the weight ratio of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 1:3:1.5, and the average particle diameters of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate are all 50nm.

[0047] The method for preparing the above PP film comprises the following steps:

[0048] S1: Weigh polypropylene, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, filler, silane coupling agent and antioxidant according to the proportion, add them into a mixer, and stir for 1 hour;

[0049] S2: using a twin-screw extruder to extrude and granulate the material stirred in step 1 at a temperature of 183° C., and drying after granulation to obtain a modified polypropylene masterbatch;

[0050] S3: adding the modified polypropylene masterbatch prepared in step 2 into a single screw extruder for sheet extrusion, longitudinal stretching, and then transverse stretching to obtain a polypropylene film.

[0051] Example 2

[0052] This embodiment provides a PP film, comprising the following raw materials in parts by weight: 90 parts of polypropylene resin, 10 parts of maleic anhydride modified polypropylene resin, 6 parts of polyethylene resin, 4 parts of ethylene-vinyl acetate copolymer, 6 parts of filler, 3 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 2 parts of antioxidant 1010.

[0053] The filler is a composition of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, the weight ratio of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 1:2:1, and the average particle diameters of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate are all 50nm.

[0054] The method for preparing the above PP film comprises the following steps:

[0055] S1: Weigh polypropylene, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, filler, silane coupling agent and antioxidant according to the proportion, add them into a mixer, and stir for 1 hour;

[0056] S2: using a twin-screw extruder to extrude and granulate the material stirred in step 1 at a temperature of 183° C., and drying after granulation to obtain a modified polypropylene masterbatch;

[0057] S3: adding the modified polypropylene masterbatch prepared in step 2 into a single screw extruder for sheet extrusion, longitudinal stretching, and then transverse stretching to obtain a polypropylene film.

[0058] Example 3

[0059] This embodiment provides a PP film, comprising the following raw materials in parts by weight: 85 parts of polypropylene resin, 15 parts of maleic anhydride modified polypropylene resin, 8 parts of polyethylene resin, 6 parts of ethylene-vinyl acetate copolymer, 10 parts of filler, 5 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 2 parts of antioxidant 1010.

[0060] The filler is a composition of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, the weight ratio of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 1:3:2, and the average particle diameters of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate are all 50nm.

[0061] The method for preparing the above PP film comprises the following steps:

[0062] S1: Weigh polypropylene, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, filler, silane coupling agent and antioxidant according to the proportion, add them into a mixer, and stir for 1 hour;

[0063] S2: using a twin-screw extruder to extrude and granulate the material stirred in step 1 at a temperature of 183° C., and drying after granulation to obtain a modified polypropylene masterbatch;

[0064] S3: adding the modified polypropylene masterbatch prepared in step 2 into a single screw extruder for extrusion, longitudinal stretching, and then transverse stretching or simultaneous longitudinal and transverse stretching to obtain a polypropylene film.

[0065] Example 4

[0066] This embodiment provides a multi-layer composite PP film, which is directly co-extruded by a surface layer, an intermediate layer and an inner layer structure;

[0067] The surface layer is made of the following raw materials in parts by weight: 80 parts of polypropylene resin, 15 parts of maleic anhydride modified polypropylene resin, 15 parts of polyethylene resin, 5 parts of ethylene-vinyl acetate copolymer, 10 parts of filler, 4 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 2 parts of antioxidant 1010; the filler is a composition of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, the weight ratio of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 1:3:1.5, and the average particle size of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 50nm;

[0068] The inner layer is made of the following raw materials in parts by weight: 85 parts of polypropylene resin, 15 parts of maleic anhydride modified polypropylene resin, 8 parts of polyethylene resin, 6 parts of ethylene-vinyl acetate copolymer, 10 parts of filler, 5 parts of N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane and 2 parts of antioxidant 1010; the filler is a composition of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, the weight ratio of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 1:3:1.5, and the average particle size of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 50nm;

[0069] The middle layer is a film made of maleic anhydride modified polypropylene resin;

[0070] The middle layer melt, the surface layer melt and the inner layer melt are combined at the die head and extruded, and are rapidly cooled by a quench roller and a water tank to form a solid casting sheet; then longitudinal stretching is performed, the longitudinal stretching temperature is 100°C, and the longitudinal stretching multiple is 3.5 times; then transverse stretching is performed, the transverse stretching temperature is 120°C, and the transverse stretching multiple is 4 times; immediately after stretching, cooling and shaping treatment is performed, and the cold air temperature is 23°C; then online thickness measurement, edge material cutting, automatic winding, aging treatment are performed in turn, and finally slitting is performed to obtain a finished multi-layer composite PP film.

[0071] Comparative Example 1

[0072] Compared with Example 1, the difference is that maleic anhydride modified polypropylene resin is not included, and other components are the same.

[0073] The preparation method is the same as Example 1.

[0074] Comparative Example 2

[0075] Compared with Example 1, the difference is that polyethylene resin and ethylene-vinyl acetate copolymer are not included, and other components are the same.

[0076] The preparation method is the same as Example 1.

[0077] Comparative Example 3

[0078] Compared with Example 1, the difference is that maleic anhydride-modified polypropylene resin, polyethylene resin and ethylene-vinyl acetate copolymer are not included.

[0079] The preparation method is the same as Example 1.

[0080] Comparative Example 4

[0081] Compared with Example 1, the difference is that the filler is replaced by an equal weight of nano aluminum hydroxide, and the other components are the same.

[0082] The preparation method is the same as Example 1.

[0083] Comparative Example 5

[0084] Compared with Example 1, the difference is that the weight ratio of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate in the filler is 5:0.5:0.1, and the other components are the same.

[0085] The preparation method is the same as Example 1.

[0086] Performance testing:

[0087] Dart impact strength: The impact damage quality of strong and tough polypropylene film at -50℃ and 23℃ is measured according to GBT 9639.1-2008 "Test method for impact resistance of plastic film and sheeting".

[0088] Tensile strength: The longitudinal tensile strength and transverse tensile strength of strong and tough polypropylene film are measured according to GB T 10003-2008 "Test method for tensile properties of plastic films".

[0089] Elongation at break: The elongation at break of strong and tough polypropylene film is measured according to GB / T 10003-2008 “General purpose biaxially oriented polypropylene film”.

[0090] The performance of the PP films of Examples 1-4 and Comparative Examples 1-5 was tested, and the size of the polypropylene film test samples was prepared according to the requirements of the following test standards, and the film thickness was 0.5 mm. The test results are shown in Table 1.

[0091] Table 1 Performance test results of polypropylene film

[0092]

[0093] From the test results in Table 1, it can be seen that the impact damage mass of the polypropylene film obtained in the embodiment of the present invention at -50°C and 23°C can reach up to 485g and 513g; the longitudinal tensile strength and transverse tensile strength can reach up to 265MPa and 182MPa; the elongation at break can reach 458%, which significantly improves the toughness and low temperature resistance of the polypropylene film. The multilayer composite PP film provided in Example 4 has better tensile strength and low temperature resistance.

[0094] Comparative Example 1 Compared with Example 1, the PP film of Comparative Example 1 does not include a maleic anhydride-modified polypropylene resin component, and both the transverse tensile strength and the longitudinal tensile strength decrease, and both the -50°C impact breakage mass and the 23°C impact breakage mass decrease.

[0095] Compared with Example 1, the PP film of Comparative Example 2 does not include polyethylene resin and ethylene-vinyl acetate copolymer components, and the transverse tensile strength and longitudinal tensile strength are both reduced, and the -50°C impact damage mass and 23°C impact damage mass are both reduced.

[0096] Compared with Example 1, the PP film of Comparative Example 3 does not include maleic anhydride modified polypropylene resin, polyethylene resin, and ethylene-vinyl acetate copolymer components, and the transverse tensile strength and longitudinal tensile strength are significantly reduced, and the -50°C impact damage mass and 23°C impact damage mass are significantly reduced, and the decline is greater than that of Comparative Example 1 and Comparative Example 2.

[0097] Compared with Example 1, in Comparative Example 4, the filler in the PP film of Comparative Example 4 is replaced with an equal weight of nano-aluminum hydroxide, and the transverse tensile strength and the longitudinal tensile strength are both reduced, and the -50°C impact damage mass and the 23°C impact damage mass are both reduced, indicating that the filler used in Example 1 of the present invention can enhance the tensile strength of the PP film and improve the low-temperature impact resistance.

[0098] Comparative Example 5 Compared with Example 1, the weight ratio of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate in the filler of Comparative Example 5 is 5:0.5:0.1, and the transverse tensile strength and the longitudinal tensile strength are both reduced, and the -50°C impact damage mass and the 23°C impact damage mass are both reduced, indicating that the use of fillers within the ratio range of the present invention can enhance the tensile strength of the PP film and improve the low-temperature impact resistance. Exceeding the compatibility ratio range of the present invention will cause the mechanical properties and low-temperature resistance of the PP film to decrease.

[0099] It can be seen from the test results of the embodiments and comparative examples that the maleic anhydride modified polypropylene resin, polyethylene resin, and ethylene-vinyl acetate copolymer provided by the present invention can synergistically enhance the transverse tensile strength and longitudinal tensile strength of PP and improve the low temperature resistance and impact resistance; the filler provided by the present invention can enhance the transverse tensile strength and longitudinal tensile strength of PP and improve the low temperature resistance and impact resistance within a suitable ratio range. Therefore, the PP film and multi-layer composite PP film provided by the present invention have excellent strength and toughness, and good low temperature resistance.

[0100] Although the embodiments of the present description have been shown and described, it will be appreciated by those skilled in the art that various changes, modifications, substitutions and variations may be made to the embodiments without departing from the principles and spirit of the present description, the scope of which is defined by the appended claims and their equivalents.

Claims

1. A PP film, characterized in that: The invention comprises the following raw materials in parts by weight: 80-90 parts of polypropylene resin, 10-20 parts of maleic anhydride modified polypropylene resin, 5-15 parts of polyethylene resin, 2-7 parts of ethylene-vinyl acetate copolymer, 3-10 parts of filler, 3-7 parts of silane coupling agent and 2-7 parts of antioxidant; the filler is a composition of nano zirconium silicate, nano aluminum silicate and nano magnesium silicate, and the weight ratio of the nano zirconium silicate, nano aluminum silicate and nano magnesium silicate is 1:2-3:1-2.

2. The PP film according to claim 1, characterized in that: The weight ratio of the polypropylene resin: maleic anhydride modified polypropylene resin: polyethylene resin: ethylene-vinyl acetate copolymer is 4-6:1:0.5-1:0.25-0.

48.

3. The PP film according to claim 1, characterized in that: The silane coupling agent includes one or more of γ-ureidopropyltriethoxysilane, N-(β-aminoethyl)-γ-aminopropyltrimethoxysilane, γ-aminopropyltriethoxysilane, and N-β-(aminoethyl)-γ-aminopropyltriethoxysilane.

4. The PP film according to claim 1, characterized in that: The antioxidant is any one of a hindered phenol antioxidant, a phosphite antioxidant and a thioester antioxidant.

5. The PP film according to claim 1, characterized in that: It also includes 0.5-3 parts of flame retardant and / or 1-3 parts of antibacterial agent.

6. The PP film according to claim 5, characterized in that: The flame retardant is one or more of sulfonate flame retardant, phosphazene flame retardant, organic phosphate and silicon flame retardant; and / or the antibacterial agent is at least one of nano titanium dioxide and nano silver antibacterial agent.

7. The method for preparing a PP film according to any one of claims 1 to 4, characterized in that: The method comprises the following steps: S1: weighing polypropylene, maleic anhydride modified polypropylene resin, polyethylene resin, ethylene-vinyl acetate copolymer, filler, silane coupling agent and antioxidant according to a proportion, adding the mixture into a mixer and stirring for 0.5-1.5 hours; S2: using a twin-screw extruder to extrude and granulate the material stirred in step 1 at a temperature of 180-240° C., drying the material after granulation to obtain modified polypropylene masterbatch; S3: adding the modified polypropylene masterbatch prepared in step 2 into a single-screw extruder to extrude sheets, longitudinally stretch the material, and then transversely stretch the material or simultaneously longitudinally and transversely stretch the material to obtain a polypropylene film.

8. A multi-layer composite PP film, characterized in that: The multi-layer composite film is made by direct co-extrusion of a surface layer, an intermediate layer and an inner layer structure; the surface layer and the inner layer are respectively made of the PP film according to any one of claims 1 to 6, and the intermediate layer is made of maleic anhydride modified polypropylene resin.

9. The multi-layer composite PP film according to claim 8, characterized in that: The raw material components of the PP films of the surface layer and the inner layer are the same or different.

10. The multi-layer composite PP film according to claim 8, characterized in that: The thickness of the surface layer and the inner layer is 0.8-50 um, and the thickness of the middle layer is 10-100 um.