A method for preparing highly hygroscopic polyester fiber

By reacting terephthalic acid and ethylene glycol with modified monomers, mixing with tannic acid-cyclodextrin-halloysite nanotubes and then spinning, the problem of poor hygroscopicity of polyester fiber was solved and achieved It combines high moisture absorption and excellent mechanical properties, making it suitable for industrial production and expanding its application fields.

CN118422368BActive Publication Date: 2024-10-29SHANGHAI JINSHANGLI NEW MATERIAL TECH CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202410877099.7
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-02
Publication Date
2024-10-29
Estimated Expiration
2044-07-02

AI Technical Summary

Technical Problem

Polyester fiber has poor hygroscopic properties, which limits its application in fields that require good hygroscopic and breathable properties.

Method used

Polyester materials are obtained by reacting terephthalic acid, ethylene glycol and modified monomers under a catalyst, and are mixed with tannic acid-cyclodextrin-halloysite nanotubes and then fibers are prepared by spinning. And carry out alkali weight reduction treatment to obtain highly hygroscopic polyester fiber. The modified monomer is prepared by the reaction of 2-acrylamide-2-methylpropanesulfonic acid and mercaptohexanol. The tannic acid is combined with cyclodextrin and reacts with halloysite nanotubes to form a composite material to improve the fiber structure. Increase micropores and channels to improve moisture absorption performance.

Benefits of technology

It significantly improves the moisture absorption performance of polyester fiber while maintaining excellent mechanical properties. It is suitable for industrial production, has long-lasting effects, and expands the application fields of polyester fiber.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118422368B_ABST
    Figure CN118422368B_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of polyester fibers, and specifically discloses a method for preparing a highly hygroscopic polyester fiber. The method comprises the following steps: firstly reacting terephthalic acid, ethylene glycol and a modified monomer under a catalyst to obtain a polyester material; then uniformly mixing the polyester material with tannic acid-cyclodextrin-halloysite nanotubes, preparing fibers through a spinning method, and subjecting the fibers to an alkali reduction treatment to obtain the highly hygroscopic polyester fiber; the modified monomer is prepared by reacting 2-acrylamide-2-methylpropanesulfonic acid and mercaptohexanol under the action of a photoinitiator; and the alkali solution used for the alkali reduction treatment comprises sodium hydroxide, guar hydroxypropyltrimethylammonium chloride, dodecyldimethylbenzyl ammonium chloride and polyoxyethylene ether; the preparation method has simple steps, low cost and is suitable for industrial production; the obtained polyester fiber has significant hygroscopicity and excellent mechanical properties and has broad market prospects.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polyester fibers, and more particularly to a method for preparing highly hygroscopic polyester fibers. Background Art

[0002] Polyester fibers are widely used in textile and other non-clothing fields due to their high modulus, high strength, excellent wrinkle resistance, shape retention and heat resistance. However, a major drawback of this synthetic fiber is its poor hygroscopicity, which limits its application in fields that require good moisture absorption and breathability. Polyester fibers have densely arranged molecules, high crystallinity, lack hydrophilic groups on the macromolecules, and have no other polar groups except for two terminal alcohol hydroxyl groups. They also contain a large number of hydrophobic ester groups. In addition, their smooth surface makes their hygroscopicity much lower than that of natural cotton fibers.

[0003] At present, CN115058889A discloses a hydrophilic polyester fiber and a modification method, comprising the following steps: step 1: preparing a low eutectic solvent; step 2: immersing the polyester fiber in the low eutectic solvent for treatment; washing and drying after treatment to obtain the hydrophilic polyester fiber; the molar ratio of the hydrogen bond donor and the hydrogen bond acceptor in the low eutectic solvent is (1-4): (4-1); the hydrogen bond donor is one or two or more of p-toluenesulfonic acid, phenylacetic acid, citric acid, oxalic acid, formic acid, acetic acid, and lactic acid mixed in any proportion; the hydrogen bond acceptor is one or two or more of choline chloride, choline hydroxide, and betaine mixed in any proportion; the hydrophilic polyester fiber obtained by the method of the invention has increased oxygen-containing functional groups on the surface, has good hydrophilicity and hygroscopicity, but the low eutectic solvent has poor bonding strength with the fiber, and has a temporary effect. As the number of uses and time increase, the hygroscopicity effect decreases significantly.

[0004] Therefore, developing a method for preparing polyester fibers with long-lasting hygroscopic properties will help broaden the application areas of polyester fibers, better meet the market demand for high-performance and multifunctional textile materials, and bring more innovations and opportunities to the textile industry. Summary of the invention

[0005] In order to solve the problem of poor moisture absorption performance of existing polyester fibers, the present invention provides a method for preparing polyester fibers.

[0006] In order to achieve the above object, the present invention is implemented by the following technical solutions:

[0007] A method for preparing polyester fiber comprises the following steps:

[0008] Step S1, reacting terephthalic acid, ethylene glycol and a modified monomer in the presence of a catalyst to obtain a polyester material;

[0009] Step S2, after uniformly mixing the polyester material with tannic acid-cyclodextrin-halloysite nanotubes, preparing fibers by a spinning method, and subjecting the fibers to an alkali reduction treatment to obtain highly hygroscopic polyester fibers;

[0010] The modified monomer is prepared by reacting 2-acrylamide-2-methylpropanesulfonic acid and mercaptohexanol under the action of a photoinitiator.

[0011] Preferably, in step S1, the mass ratio of terephthalic acid, ethylene glycol, modified monomer and catalyst is 20:(10-14):(6-11):(0.1-1); the catalyst is antimony ethylene glycol.

[0012] Preferably, in step S2, the mass ratio of the polyester material to the tannic acid-cyclodextrin-halloysite nanotubes is 100:(7-15).

[0013] Preferably, the modified monomer is prepared by the following method: 2-acrylamide-2-methylpropanesulfonic acid, mercaptohexanol, photoinitiator, and N,N-dimethylformamide are mixed evenly in a ratio of 20 g: (26-30) g: (0.1-0.6) g: 100 mL, and then irradiated under ultraviolet light for reaction for 20-60 minutes, and the solution is rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain the modified monomer.

[0014] Preferably, the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.

[0015] Preferably, the tannic acid-cyclodextrin-halloysite nanotubes are prepared by the following method:

[0016] Step a), dissolving tannic acid and mono-6-ethylenediamino-β-cyclodextrin in N,N-dimethylformamide, stirring and reacting at 50-70° C. for 3-6 hours, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0017] Step b), first disperse the halloysite nanotubes in a Tris buffer solution with a pH of 8.0, then add tannic acid-cyclodextrin, stir and react at 30-40° C. for 12-24 hours, centrifuge, wash and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes.

[0018] Preferably, in step a), the ratio of tannic acid, mono-6-ethylenediamino-β-cyclodextrin, and N,N-dimethylformamide is 17 g: (10-15) g: (100-150) mL.

[0019] Preferably, the concentration of the Tris buffer solution in step b) is 0.01 mol / L; the usage ratio of the Tris buffer solution, halloysite nanotubes, and tannic acid-cyclodextrin is 100 mL: 5 g: (1-2) g.

[0020] Preferably, the specific process of step S1 is:

[0021] After terephthalic acid, ethylene glycol, modified monomer and catalyst are evenly mixed, nitrogen is introduced, and the reaction pressure is controlled at 0.2-0.3MPa. After the esterification reaction is carried out at 230-250°C for 3-4h, the temperature is raised to 255-275°C, and the reaction pressure is controlled at 50-80Pa for polycondensation reaction. After the reaction is carried out for 2-3h, the material is cooled and discharged to obtain a polyester material.

[0022] Preferably, the specific process of step S2 is:

[0023] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed and then added into a twin-screw extruder, the melting temperature is controlled to be 225-240°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 280-305°C and a spinning rate of 700-800m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3-4 times to obtain fibers; finally, the fibers are added into an alkali solution at a solid-liquid ratio of 1g: (50-100)mL, and after alkali reduction treatment at 80-120°C for 2-4h, the fibers are washed with deionized water and dried at 80-100°C to obtain highly hygroscopic polyester fibers.

[0024] Preferably, the alkali solution comprises the following components in parts by weight: 20-60 parts of sodium hydroxide, 10-20 parts of guar hydroxypropyltrimethylammonium chloride, 5-8 parts of dodecyldimethylbenzylammonium chloride, 1-2 parts of polyoxyethylene ether, and 1000 parts of deionized water.

[0025] In summary, the present invention has the following beneficial effects:

[0026] 1. The modified monomer of the present invention is obtained by a mercapto-ene click reaction between 2-acrylamide-2-methylpropanesulfonic acid and mercaptohexanol, and the modified monomer contains a hydrophilic amide group and a sulfonic acid group; in the polymerization process of terephthalic acid and ethylene glycol, the introduction of the modified monomer can destroy the regularity of the main chain of the polyester macromolecule, resulting in an increase in the proportion of the crystallinity reduction area of ​​the polyester fiber, making it easier for water molecules to diffuse into the fiber macromolecule, and the introduction of hydrophilic groups greatly improves the hygroscopicity of the polyester fiber.

[0027] 2. The present invention combines tannic acid and mono-6-ethylenediamine-β-cyclodextrin with chemical bonds to obtain tannic acid-cyclodextrin, and the carboxyl group of tannic acid-cyclodextrin reacts chemically with the halloysite nanotubes treated with a Tris buffer solution to obtain tannic acid-cyclodextrin-halloysite nanotubes; when the tannic acid-cyclodextrin-halloysite nanotubes are melted and blended with polyester materials, polyester fibers are obtained; tannic acid-cyclodextrin-halloysite nanotubes can improve the structure of polyester fibers, so that more micropores and channels are formed inside and outside the fibers, the contact area between the polyester fibers and the air is increased, which is conducive to the adsorption and diffusion of water molecules, thereby improving the hygroscopic performance; at the same time, tannic acid-cyclodextrin-halloysite nanotubes have significant hydrophilicity, so that the hydrophilicity of the polyester fiber surface is enhanced, and it is easier to adsorb water molecules in the air and improve the hygroscopic performance. At the same time, the addition of tannic acid-cyclodextrin-halloysite nanotubes can also enhance the mechanical, antibacterial, deodorizing and UV resistance of polyester fibers, expanding the application field of polyester fibers.

[0028] 3. The alkali solution used in the alkali reduction treatment of the present invention includes raw materials such as sodium hydroxide, guar hydroxypropyltrimethylammonium chloride, dodecyldimethylbenzylammonium chloride, polyoxyethylene ether, etc. The components interact with each other. After the alkali reduction treatment of the polyester fiber, the micro-pit structure and micropore structure on the surface of the polyester fiber are more significant, and the roughness is increased, thereby effectively improving the moisture absorption performance of the polyester fiber, while the polyester fiber still maintains excellent mechanical properties.

[0029] 4. The preparation method of the polyester fiber of the present invention has simple steps, low cost, and is suitable for industrial production. The obtained polyester fiber has excellent hygroscopic properties and mechanical properties, and the hygroscopic properties are long-lasting, and has broad market prospects. BRIEF DESCRIPTION OF THE DRAWINGS

[0030] Figure 1 This is a SEM image of the polyester fiber obtained in Example 1 of the present invention. DETAILED DESCRIPTION

[0031] The technical scheme of the present invention will be further described in detail below in conjunction with specific embodiments. It should be understood that the following embodiments are only exemplary descriptions and explanations of the present invention and should not be construed as limiting the scope of protection of the present invention. All technologies implemented based on the above content of the present invention are included in the scope that the present invention is intended to protect.

[0032] The raw materials used in the examples and comparative examples of the present invention are as follows:

[0033] 2-Acrylamide-2-methylpropanesulfonic acid, brand: Wokai, CAS number: 15214-89-8, national medicine code: XW011521489802, purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0034] Mercaptohexanol, 6-mercaptohexanol, brand Yuanye, CAS number: 1633-78-9, product number: S43320, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0035] 2-Hydroxy-2-methyl-1-phenyl-1-propanone, brand Yuanye, CAS number: 7473-98-5, product number: B65201, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0036] N,N-dimethylformamide, brand Shanghai Test, CAS number: 68-12-2, national medicine code: 81007718, purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0037] Tannic acid, brand Yuanye, CAS number: 5424-20-4, product number: T25393, purchased from Shanghai Yuanye Biotechnology Co., Ltd.;

[0038] Mono-6-ethylenediamino-β-cyclodextrin, brand Jusheng, CAS number: 60984-63-6, product number: JS6225, purchased from Hubei Jusheng Technology Co., Ltd.;

[0039] Halloysite nanotubes, brand: Xianfeng Nano, CAS No.: 1332-58-7, item No.: 103764, diameter: 50-300 nm, length: 1-10 μm, purchased from Jiangsu Xianfeng Nanomaterials Technology Co., Ltd.;

[0040] Tris(hydroxymethyl)aminomethane (Tris), brand Shanghai Test, CAS number: 77-86-1; National medicine code: 301882090, purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0041] Terephthalic acid, brand: Wokai, CAS number: 100-21-0, national medicine code: 30148085, purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0042] Ethylene glycol, brand Shanghai Test, CAS number: 107-21-1, national medicine code: 10009818, purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0043] Antimony glycolate, brand: Wokai, CAS number: 29736-75-2, national medicine code: XW012973675202; purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0044] Sodium hydroxide, brand Shanghai Test, CAS number: 1310-73-2, national medicine code: 10019718, purchased from Sinopharm Chemical Reagent Co., Ltd.;

[0045] Guar hydroxypropyltrimonium chloride, brand: McLean, CAS number: 65497-29-2, item number: G990026, purchased from Shanghai McLean Biochemical Technology Co., Ltd.;

[0046] Dodecyl dimethyl benzyl ammonium chloride, brand: McLean, CAS number: 139-07-1, product number: B801873, purchased from Shanghai McLean Biochemical Technology Co., Ltd.;

[0047] Polyoxyethylene ether, brand Yuanye, CAS number: 9004-95-9, product number: S51665, purchased from Shanghai Yuanye Biotechnology Co., Ltd.

[0048] Embodiment 1-5 provides a method for preparing a highly hygroscopic polyester fiber, as follows:

[0049] Example 1

[0050] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0051] Step S0, preparing modified monomer and tannic acid-cyclodextrin-halloysite nanoparticles

[0052] (1) Preparation of modified monomers

[0053] 20 g of 2-acrylamide-2-methylpropanesulfonic acid, 26 g of mercaptohexanol, and 0.1 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone were added to 100 mL of N,N-dimethylformamide and mixed evenly, and then irradiated under ultraviolet light for 20 min, and the solution was rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain a modified monomer;

[0054] (2) Preparation of tannic acid-cyclodextrin-halloysite nanotubes

[0055] Step a), dissolving 17 g of tannic acid and 10 g of mono-6-ethylenediamino-β-cyclodextrin in 100 mL of N,N-dimethylformamide, stirring and reacting at 50° C. for 3 h, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0056] Step b), first disperse 5g of halloysite nanotubes in 100mL of a Tris buffer solution with a pH of 8.0 and a concentration of 0.01mol / L, then add 1g of tannic acid-cyclodextrin, stir and react at 30°C for 12h, centrifuge, wash with water, and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes;

[0057] Step S1: preparing polyester material

[0058] 20g of terephthalic acid, 10g of ethylene glycol, 6g of modified monomer and 0.1g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.2MPa, and the esterification reaction was carried out at 230°C for 3h, then the temperature was raised to 255°C, the reaction pressure was controlled to be 50Pa for polycondensation reaction, and after reacting for 2h, the material was cooled and discharged to obtain a polyester material;

[0059] Step S2: preparing highly hygroscopic polyester fibers

[0060] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed at a mass ratio of 100:7, and then added to a twin-screw extruder, the melting temperature is controlled to be 225°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 280°C and a spinning rate of 700m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3 times to obtain fibers; finally, the fibers are added to an alkali solution at a solid-liquid ratio of 1g:50mL, and after an alkali reduction treatment at 80°C for 2h, the fibers are washed with deionized water and dried at 80°C to obtain highly hygroscopic polyester fibers;

[0061] The alkali solution is composed of the following components: 20g of sodium hydroxide, 10g of guar hydroxypropyltrimethylammonium chloride, 5g of dodecyldimethylbenzylammonium chloride, 1g of polyoxyethylene ether, and 1000g of deionized water.

[0062] Example 2

[0063] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0064] Step S0, preparing modified monomer and tannic acid-cyclodextrin-halloysite nanoparticles

[0065] (1) Preparation of modified monomers

[0066] 20 g of 2-acrylamide-2-methylpropanesulfonic acid, 27 g of mercaptohexanol, and 0.2 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone were added to 100 mL of N,N-dimethylformamide and mixed evenly, and then irradiated under ultraviolet light for reaction for 30 min, and the solution was rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain a modified monomer;

[0067] (2) Preparation of tannic acid-cyclodextrin-halloysite nanotubes

[0068] Step a), dissolving 17 g of tannic acid and 11.5 g of mono-6-ethylenediamino-β-cyclodextrin in 110 mL of N,N-dimethylformamide, stirring and reacting at 55° C. for 4 h, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0069] Step b), first disperse 5g of halloysite nanotubes in 100mL of a 0.01mol / L Tris buffer solution with a pH of 8.0, then add 1.2g of tannic acid-cyclodextrin, stir and react at 32°C for 15h, centrifuge, wash with water, and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes;

[0070] Step S1: preparing polyester material

[0071] 20g of terephthalic acid, 11g of ethylene glycol, 7g of modified monomer and 0.3g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.23MPa, and the esterification reaction was carried out at 235°C for 3.2h, and then the temperature was raised to 260°C, the reaction pressure was controlled to be 55Pa for polycondensation reaction, and after the reaction was carried out for 2.5h, the material was cooled and discharged to obtain a polyester material;

[0072] Step S2: preparing highly hygroscopic polyester fibers

[0073] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed at a mass ratio of 100:9, and then added to a twin-screw extruder, the melting temperature is controlled to be 230°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 285°C and a spinning rate of 720m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3.5 times to obtain fibers; finally, the fibers are added to an alkali solution at a solid-liquid ratio of 1g:60mL, and after an alkali reduction treatment at 90°C for 2.5h, the fibers are washed with deionized water and dried at 90°C to obtain highly hygroscopic polyester fibers;

[0074] The alkali solution is composed of the following components: 30 g of sodium hydroxide, 12 g of guar hydroxypropyltrimethylammonium chloride, 6 g of dodecyldimethylbenzylammonium chloride, 1.2 g of polyoxyethylene ether, and 1000 g of deionized water.

[0075] Example 3

[0076] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0077] Step S0, preparing modified monomer and tannic acid-cyclodextrin-halloysite nanoparticles

[0078] (1) Preparation of modified monomers

[0079] 20 g of 2-acrylamide-2-methylpropanesulfonic acid, 28 g of mercaptohexanol, and 0.4 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone were added to 100 mL of N,N-dimethylformamide and mixed evenly, and then irradiated under ultraviolet light for 40 min, and the solution was rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain a modified monomer;

[0080] (2) Preparation of tannic acid-cyclodextrin-halloysite nanotubes

[0081] Step a), dissolving 17 g of tannic acid and 13 g of mono-6-ethylenediamino-β-cyclodextrin in 120 mL of N,N-dimethylformamide, stirring and reacting at 60° C. for 4.5 h, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0082] Step b), first disperse 5g of halloysite nanotubes in 100mL of a 0.01mol / L Tris buffer solution with a pH of 8.0, then add 1.5g of tannic acid-cyclodextrin, stir and react at 35°C for 18h, centrifuge, wash with water, and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes;

[0083] Step S1: preparing polyester material

[0084] 20g of terephthalic acid, 12g of ethylene glycol, 8g of modified monomer and 0.5g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.25MPa, and the esterification reaction was carried out at 240°C for 3.5h, and then the temperature was raised to 265°C, and the reaction pressure was controlled to be 70Pa for polycondensation reaction. After the reaction was carried out for 2.5h, the material was cooled and discharged to obtain a polyester material;

[0085] Step S2: preparing highly hygroscopic polyester fibers

[0086] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed at a mass ratio of 10:1, and then added to a twin-screw extruder, the melting temperature is controlled to be 230°C, and granulation is performed after melt extrusion; the granules are then melt-spun in a melt spinning machine at a temperature of 295°C and a spinning rate of 750m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3.5 times to obtain fibers; finally, the fibers are added to an alkali solution at a solid-liquid ratio of 1g:80mL, and after an alkali reduction treatment at 100°C for 3h, the fibers are washed with deionized water and dried at 90°C to obtain highly hygroscopic polyester fibers;

[0087] The alkali solution is composed of the following components: 40 g of sodium hydroxide, 15 g of guar hydroxypropyltrimethylammonium chloride, 7.5 g of dodecyldimethylbenzylammonium chloride, 1.5 g of polyoxyethylene ether, and 1000 g of deionized water.

[0088] Example 4

[0089] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0090] Step S0, preparing modified monomer and tannic acid-cyclodextrin-halloysite nanoparticles

[0091] (1) Preparation of modified monomers

[0092] 20 g of 2-acrylamide-2-methylpropanesulfonic acid, 29 g of mercaptohexanol, and 0.55 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone were added to 100 mL of N,N-dimethylformamide and mixed evenly, and then irradiated under ultraviolet light for reaction for 55 min, and the solution was rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain a modified monomer;

[0093] (2) Preparation of tannic acid-cyclodextrin-halloysite nanotubes

[0094] Step a), dissolving 17 g of tannic acid and 14.5 g of mono-6-ethylenediamino-β-cyclodextrin in 140 mL of N,N-dimethylformamide, stirring and reacting at 65° C. for 5.5 h, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0095] Step b), first disperse 5g of halloysite nanotubes in 100mL of a 0.01mol / L Tris buffer solution with a pH of 8.0, then add 1.8g of tannic acid-cyclodextrin, stir and react at 35°C for 18h, centrifuge, wash with water, and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes;

[0096] Step S1: preparing polyester material

[0097] 20g of terephthalic acid, 13.5g of ethylene glycol, 9g of modified monomer and 0.8g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.28MPa, and the esterification reaction was carried out at 245°C for 3.8h, and then the temperature was raised to 270°C, and the reaction pressure was controlled to be 75Pa for polycondensation reaction. After the reaction was carried out for 2.8h, the material was cooled and discharged to obtain a polyester material;

[0098] Step S2: preparing highly hygroscopic polyester fibers

[0099] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed at a mass ratio of 100:13, and then added to a twin-screw extruder, the melting temperature is controlled to be 235°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 300°C and a spinning rate of 780m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3.8 times to obtain fibers; finally, the fibers are added to an alkali solution at a solid-liquid ratio of 1g:90mL, and after an alkali reduction treatment at 110°C for 3.5h, the fibers are washed with deionized water and dried at 95°C to obtain highly hygroscopic polyester fibers;

[0100] The alkali solution is composed of the following components: 50 g of sodium hydroxide, 18 g of guar hydroxypropyltrimethylammonium chloride, 7.8 g of dodecyldimethylbenzylammonium chloride, 1.8 g of polyoxyethylene ether, and 1000 g of deionized water.

[0101] Example 5

[0102] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0103] Step S0, preparing modified monomer and tannic acid-cyclodextrin-halloysite nanoparticles

[0104] (1) Preparation of modified monomers

[0105] 20 g of 2-acrylamide-2-methylpropanesulfonic acid, 30 g of mercaptohexanol, and 0.6 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone were added to 100 mL of N,N-dimethylformamide and mixed evenly, and then irradiated under ultraviolet light for 60 min, and the solution was rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain a modified monomer;

[0106] (2) Preparation of tannic acid-cyclodextrin-halloysite nanotubes

[0107] Step a), dissolving 17 g of tannic acid and 15 g of mono-6-ethylenediamino-β-cyclodextrin in 150 mL of N,N-dimethylformamide, stirring and reacting at 70° C. for 6 h, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0108] Step b), first disperse 5g of halloysite nanotubes in 100mL of a Tris buffer solution with a pH of 8.0 and a concentration of 0.01mol / L, then add 2g of tannic acid-cyclodextrin, stir and react at 40°C for 24h, centrifuge, wash with water, and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes;

[0109] Step S1: preparing polyester material

[0110] 20g of terephthalic acid, 14g of ethylene glycol, 11g of modified monomer and 1g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.3MPa, and the esterification reaction was carried out at 250°C for 4h, then the temperature was raised to 275°C, the reaction pressure was controlled to be 80Pa for polycondensation reaction, and after the reaction was carried out for 3h, the material was cooled and discharged to obtain a polyester material;

[0111] Step S2: preparing highly hygroscopic polyester fibers

[0112] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed at a mass ratio of 20:3, and then added to a twin-screw extruder, the melting temperature is controlled to be 240°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 305°C and a spinning rate of 800m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 4 times to obtain fibers; finally, the fibers are added to an alkali solution at a solid-liquid ratio of 1g:100mL, and after alkali reduction treatment at 120°C for 4h, the fibers are washed with deionized water and dried at 100°C to obtain highly hygroscopic polyester fibers;

[0113] The alkali solution is composed of the following components: 60g of sodium hydroxide, 20g of guar hydroxypropyltrimethylammonium chloride, 8g of dodecyldimethylbenzylammonium chloride, 2g of polyoxyethylene ether, and 1000g of deionized water.

[0114] In order to verify the preparation method of the highly hygroscopic polyester fiber provided by the present invention, the applicant set up comparative examples 1-4, wherein:

[0115] Comparative Example 1

[0116] Comparative Example 1 is the same as Example 1, except that no modifying monomer is added, as follows:

[0117] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0118] Step S0, preparing tannic acid-cyclodextrin-halloysite nanoparticles

[0119] Step a), dissolving 17 g of tannic acid and 10 g of mono-6-ethylenediamino-β-cyclodextrin in 100 mL of N,N-dimethylformamide, stirring and reacting at 50° C. for 3 h, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0120] Step b), first disperse 5g of halloysite nanotubes in 100mL of a Tris buffer solution with a pH of 8.0 and a concentration of 0.01mol / L, then add 1g of tannic acid-cyclodextrin, stir and react at 30°C for 12h, centrifuge, wash with water, and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes;

[0121] Step S1: preparing polyester material

[0122] 20g of terephthalic acid, 10g of ethylene glycol and 0.1g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.2MPa, and the esterification reaction was carried out at 230°C for 3h, then the temperature was raised to 255°C, the reaction pressure was controlled to be 50Pa for polycondensation reaction, and after reacting for 2h, the material was cooled and discharged to obtain a polyester material;

[0123] Step S2: preparing highly hygroscopic polyester fibers

[0124] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed at a mass ratio of 100:7, and then added to a twin-screw extruder, the melting temperature is controlled to be 225°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 280°C and a spinning rate of 700m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3 times to obtain fibers; finally, the fibers are added to an alkali solution at a solid-liquid ratio of 1g:50mL, and after an alkali reduction treatment at 80°C for 2h, the fibers are washed with deionized water and dried at 80°C to obtain highly hygroscopic polyester fibers;

[0125] The alkali solution is composed of the following components: 20g sodium hydroxide, 10g guar hydroxypropyltrimethylammonium chloride, and 10g dodecyl dimethyl benzyl ammonium chloride.

[0126] 5g, polyoxyethylene ether 1g, deionized water 1000g.

[0127] Comparative Example 2

[0128] Comparative Example 2 is the same as Example 1, except that the same mass of halloysite nanotubes is used to replace the tannic acid-cyclodextrin-haloysite nanotubes, as follows:

[0129] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0130] Step S0: preparing modified monomer

[0131] 20 g of 2-acrylamide-2-methylpropanesulfonic acid, 26 g of mercaptohexanol, and 0.1 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone were added to 100 mL of N,N-dimethylformamide and mixed evenly, and then irradiated under ultraviolet light for 20 min, and the solution was rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain a modified monomer;

[0132] Step S1: preparing polyester material

[0133] 20g of terephthalic acid, 10g of ethylene glycol, 6g of modified monomer and 0.1g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.2MPa, and the esterification reaction was carried out at 230°C for 3h, then the temperature was raised to 255°C, the reaction pressure was controlled to be 50Pa for polycondensation reaction, and after reacting for 2h, the material was cooled and discharged to obtain a polyester material;

[0134] Step S2: preparing highly hygroscopic polyester fibers

[0135] The polyester material and the halloysite nanotubes were mixed at a mass ratio of 100:7, and then added to a twin-screw extruder, the melting temperature was controlled to be 225°C, and granulation was performed after melt extrusion; the granules were melt-spun in a melt spinning machine at a temperature of 280°C and a spinning rate of 700m / min; after spinning, the fibers were stretched and the stretch ratio was controlled to be 3 times to obtain fibers; finally, the fibers were added to an alkali solution at a solid-liquid ratio of 1g:50mL, and after an alkali reduction treatment at 80°C for 2h, the fibers were washed with deionized water and dried at 80°C to obtain highly hygroscopic polyester fibers;

[0136] The alkali solution is composed of the following components: 20g of sodium hydroxide, 10g of guar hydroxypropyltrimethylammonium chloride, 5g of dodecyldimethylbenzylammonium chloride, 1g of polyoxyethylene ether, and 1000g of deionized water.

[0137] Comparative Example 3

[0138] Comparative Example 3 is the same as Example 1, except that an equal amount of guar hydroxypropyltrimethylammonium chloride is used in the alkali solution to replace dodecyldimethylbenzyl ammonium chloride, as follows:

[0139] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0140] Step S0, preparing modified monomer and tannic acid-cyclodextrin-halloysite nanoparticles

[0141] (1) Preparation of modified monomers

[0142] 20 g of 2-acrylamide-2-methylpropanesulfonic acid, 26 g of mercaptohexanol, and 0.1 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone were added to 100 mL of N,N-dimethylformamide and mixed evenly, and then irradiated under ultraviolet light for 20 min, and the solution was rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain a modified monomer;

[0143] (2) Preparation of tannic acid-cyclodextrin-halloysite nanotubes

[0144] Step a), dissolving 17 g of tannic acid and 10 g of mono-6-ethylenediamino-β-cyclodextrin in 100 mL of N,N-dimethylformamide, stirring and reacting at 50° C. for 3 h, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0145] Step b), first disperse 5g of halloysite nanotubes in 100mL of a Tris buffer solution with a pH of 8.0 and a concentration of 0.01mol / L, then add 1g of tannic acid-cyclodextrin, stir and react at 30°C for 12h, centrifuge, wash with water, and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes;

[0146] Step S1: preparing polyester material

[0147] 20g of terephthalic acid, 10g of ethylene glycol, 6g of modified monomer and 0.1g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.2MPa, and the esterification reaction was carried out at 230°C for 3h, then the temperature was raised to 255°C, the reaction pressure was controlled to be 50Pa for polycondensation reaction, and after reacting for 2h, the material was cooled and discharged to obtain a polyester material;

[0148] Step S2: preparing highly hygroscopic polyester fibers

[0149] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed at a mass ratio of 100:7, and then added to a twin-screw extruder, the melting temperature is controlled to be 225°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 280°C and a spinning rate of 700m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3 times to obtain fibers; finally, the fibers are added to an alkali solution at a solid-liquid ratio of 1g:50mL, and after an alkali reduction treatment at 80°C for 2h, the fibers are washed with deionized water and dried at 80°C to obtain highly hygroscopic polyester fibers;

[0150] The alkali solution is composed of the following components: 20g of sodium hydroxide, 15g of guar hydroxypropyltrimethylammonium chloride, 1g of polyoxyethylene ether, and 1000g of deionized water.

[0151] Comparative Example 4

[0152] Comparative Example 4 is the same as Example 1, except that the guar hydroxypropyltrimethylammonium chloride is replaced with an equal amount of dodecyl dimethyl benzyl ammonium chloride in the alkali solution, as follows:

[0153] A method for preparing highly hygroscopic polyester fiber comprises the following steps:

[0154] Step S0, preparing modified monomer and tannic acid-cyclodextrin-halloysite nanoparticles

[0155] (1) Preparation of modified monomers

[0156] 20 g of 2-acrylamide-2-methylpropanesulfonic acid, 26 g of mercaptohexanol, and 0.1 g of 2-hydroxy-2-methyl-1-phenyl-1-propanone were added to 100 mL of N,N-dimethylformamide and mixed evenly, and then irradiated under ultraviolet light for 20 min, and the solution was rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain a modified monomer;

[0157] (2) Preparation of tannic acid-cyclodextrin-halloysite nanotubes

[0158] Step a), dissolving 17 g of tannic acid and 10 g of mono-6-ethylenediamino-β-cyclodextrin in 100 mL of N,N-dimethylformamide, stirring and reacting at 50° C. for 3 h, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin;

[0159] Step b), first disperse 5g of halloysite nanotubes in 100mL of a Tris buffer solution with a pH of 8.0 and a concentration of 0.01mol / L, then add 1g of tannic acid-cyclodextrin, stir and react at 30°C for 12h, centrifuge, wash with water, and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes;

[0160] Step S1: preparing polyester material

[0161] 20g of terephthalic acid, 10g of ethylene glycol, 6g of modified monomer and 0.1g of ethylene glycol antimony were mixed evenly, nitrogen was introduced, the reaction pressure was controlled to be 0.2MPa, and the esterification reaction was carried out at 230°C for 3h, then the temperature was raised to 255°C, the reaction pressure was controlled to be 50Pa for polycondensation reaction, and after reacting for 2h, the material was cooled and discharged to obtain a polyester material;

[0162] Step S2: preparing highly hygroscopic polyester fibers

[0163] First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed at a mass ratio of 100:7, and then added to a twin-screw extruder, the melting temperature is controlled to be 225°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 280°C and a spinning rate of 700m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3 times to obtain fibers; finally, the fibers are added to an alkali solution at a solid-liquid ratio of 1g:50mL, and after an alkali reduction treatment at 80°C for 2h, the fibers are washed with deionized water and dried at 80°C to obtain highly hygroscopic polyester fibers;

[0164] The alkali solution is composed of the following components: 20 g of sodium hydroxide, 15 g of dodecyl dimethyl benzyl ammonium chloride, 1 g of polyoxyethylene ether, and 1000 g of deionized water.

[0165] The properties of the polyester fibers in Examples 1-5 of the present invention and Comparative Examples 1-4 were tested respectively, and the following results were obtained as shown in Tables 1 and Figure 1 As shown:

[0166] (1) Tensile breaking performance test: refer to standard GB / T 14344-2008 "Test method for tensile properties of chemical fiber filaments"; Moisture regain performance test: refer to standard GB / T 6503-2017 "Test method for moisture regain of chemical fibers"; Water absorption performance test: Spin and knit polyester fibers according to conventional methods to obtain ordinary fabrics, cut the fabrics into 3 small pieces, record their initial mass (M1), put them into a beaker filled with water, and soak them in it for 1 hour. After taking them out, use filter paper to absorb the moisture on the surface of the fabric until no water drops naturally, weigh their mass (M2), and calculate the water absorption rate. Take the average of the 3 results and calculate the water absorption rate using the following formula: M = (M2-M1) / M1, where M is the water absorption rate, M1 is the dry weight of the fabric, and M2 is the weight of the fabric after water absorption.

[0167] Breaking strength cN / dtex Elongation at break % Moisture regain% Water absorption % Example 1 3.85 40.2 3.56 40.2 Example 2 4.32 41.5 3.68 43.6 Example 3 4.61 43.4 3.94 41.4 Example 4 4.24 41.7 3.76 42.5 Example 5 3.93 40.8 3.63 41.2 Comparative Example 1 3.02 35.1 1.43 10.3 Comparative Example 2 2.85 30.2 2.01 21.4 Comparative Example 3 3.49 38.2 2.85 34.8 Comparative Example 4 3.26 37.4 2.56 30.3

[0168] From the data shown in Table 1 above, it can be seen that the performance of the polyester fibers obtained in Examples 1-5 of the present invention is significantly better than that in Comparative Examples 1-4, and the polyester fibers have high hygroscopicity while maintaining excellent mechanical properties.

[0169] It can be seen from Example 1 and Comparative Example 1 that: in Example 1, a modified monomer is added during the preparation of the polyester material, while in Comparative Example 1, only terephthalic acid and ethylene glycol are polymerized, and the moisture absorption performance of the polyester fiber obtained in Example 1 is significantly improved.

[0170] It can be seen from Example 1 and Comparative Example 2 that Example 1 uses polyester material and tannic acid-cyclodextrin-halloysite nanotubes for melt granulation, while Comparative Example 2 uses unmodified halloysite nanotubes. The polyester fiber obtained in Example 1 has excellent moisture absorption performance and better tensile performance.

[0171] It can be seen from Example 1 and Comparative Examples 3 and 4 that the guar hydroxypropyl trimethyl ammonium chloride and dodecyl dimethyl benzyl ammonium chloride in the alkali solution of Example 1 work synergistically, while Comparative Examples 3 and 4 only use a single guar hydroxypropyl trimethyl ammonium chloride or dodecyl dimethyl benzyl ammonium chloride. The moisture absorption performance of the polyester fibers obtained in Comparative Examples 3 and 4 is not as good as that in Example 1.

[0172] (2) Morphological structure observation: After the polyester fiber sample obtained in Example 1 was subjected to vacuum gold spraying, the surface morphology of the polyester fiber was observed using a scanning electron microscope (SEM). Figure 1 shown.

[0173] Depend on Figure 1 It can be seen that the polyester fiber obtained in Example 1 of the present invention is not solid, and its surface contains micro-pit structures and micropore structures of various sizes and shapes. The surface roughness is increased, which can enhance the wetting effect and wicking effect of the polyester fiber and further improve the moisture absorption capacity of the fiber.

[0174] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited to the specific details in the above embodiments. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, and these simple modifications all belong to the protection scope of the present invention. In addition, the various embodiments of the present invention can also be arbitrarily combined, as long as they do not violate the concept of the present invention, they should also be regarded as the contents disclosed by the present invention.

Claims

1. A method for preparing polyester fiber, characterized in that: The following steps are involved: Step S1, reacting terephthalic acid, ethylene glycol and a modified monomer in the presence of a catalyst to obtain a polyester material; Step S2, after uniformly mixing the polyester material with tannic acid-cyclodextrin-halloysite nanotubes, preparing fibers by a spinning method, and subjecting the fibers to an alkali reduction treatment to obtain polyester fibers; The modified monomer is prepared by reacting 2-acrylamide-2-methylpropanesulfonic acid and mercaptohexanol under the action of a photoinitiator; The alkali solution used for alkali weight reduction treatment in step S2 comprises the following components in parts by weight: 20-60 parts of sodium hydroxide, 10-20 parts of guar hydroxypropyltrimethylammonium chloride, 5-8 parts of dodecyldimethylbenzylammonium chloride, 1-2 parts of polyoxyethylene ether, and 1000 parts of deionized water.

2. The method for preparing polyester fiber according to claim 1, characterized in that: In the step S1, the mass ratio of terephthalic acid, ethylene glycol, modified monomer and catalyst is 20:(10-14):(6-11):(0.1-1); the catalyst is antimony ethylene glycol.

3. The method for preparing polyester fiber according to claim 1, characterized in that: In the step S2, the mass ratio of the polyester material to the tannic acid-cyclodextrin-halloysite nanotubes is 100:(7-15).

4. The method for preparing polyester fiber according to claim 1, characterized in that: The modified monomer is prepared by the following method: 2-acrylamide-2-methylpropanesulfonic acid, mercaptohexanol, a photoinitiator, and N,N-dimethylformamide are mixed evenly in a ratio of 20 g: (26-30) g: (0.1-0.6) g: 100 mL, and then irradiated under ultraviolet light for reaction for 20-60 minutes, and the solution is rotary evaporated to remove the solvent, washed with toluene, and rotary evaporated to obtain the modified monomer; The photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.

5. The method for preparing polyester fiber according to claim 1, characterized in that: The tannic acid-cyclodextrin-halloysite nanotubes are prepared by the following method: Step a), dissolving tannic acid and mono-6-ethylenediamino-β-cyclodextrin in N,N-dimethylformamide, stirring and reacting at 50-70° C. for 3-6 hours, cooling to room temperature, filtering, washing, and rotary evaporation to obtain tannic acid-cyclodextrin; Step b), first disperse the halloysite nanotubes in a Tris buffer solution with a pH of 8.0, then add tannic acid-cyclodextrin, stir and react at 30-40° C. for 12-24 hours, centrifuge, wash and dry to obtain tannic acid-cyclodextrin-halloysite nanotubes.

6. The method for preparing polyester fiber according to claim 5, characterized in that: In the step a), the ratio of tannic acid, mono-6-ethylenediamino-β-cyclodextrin and N,N-dimethylformamide is 17 g: (10-15) g: (100-150) mL.

7. The method for preparing polyester fiber according to claim 6, characterized in that: The concentration of the Tris buffer solution in step b) is 0.01 mol / L; the usage ratio of the Tris buffer solution, halloysite nanotubes, and tannic acid-cyclodextrin is 100 mL: 5 g: (1-2) g.

8. The method for preparing polyester fiber according to claim 1, characterized in that: The specific process of step S1 is as follows: After terephthalic acid, ethylene glycol, modified monomer and catalyst are evenly mixed, nitrogen is introduced, and the reaction pressure is controlled at 0.2-0.3MPa. After the esterification reaction is carried out at 230-250°C for 3-4h, the temperature is raised to 255-275°C, and the reaction pressure is controlled at 50-80Pa for polycondensation reaction. After the reaction is carried out for 2-3h, the material is cooled and discharged to obtain a polyester material.

9. The method for preparing polyester fiber according to claim 1, characterized in that: The specific process of step S2 is: First, the polyester material and tannic acid-cyclodextrin-halloysite nanotubes are mixed and then added into a twin-screw extruder, the melting temperature is controlled to be 225-240°C, and granulation is performed after melt extrusion; the granules are melt-spun in a melt spinning machine at a temperature of 280-305°C and a spinning rate of 700-800m / min; after spinning, the fibers are stretched and the stretch ratio is controlled to be 3-4 times to obtain fibers; finally, the fibers are added into an alkali solution at a solid-liquid ratio of 1g: (50-100)mL, and the fibers are subjected to an alkali reduction treatment at 80-120°C for 2-4h, and then washed with deionized water and dried at 80-100°C to obtain polyester fibers.

Citation Information

Patent Citations

  • Spinning solution, nuclear shell nanofiber as well as preparation method and application thereof

    CN103046158A

  • Super-hydrophilicity polyester nanofiber membrane and preparation method thereof

    CN107747165A