A negative electrode binder, a negative electrode composition, a negative electrode sheet and a lithium ion battery thereof

By adopting a core-shell structured negative electrode binder, the problem of low bonding strength in the negative electrode slurry was solved, thereby improving the peel strength of the negative electrode sheet and the electrochemical performance of the lithium-ion battery.

CN118448635BActive Publication Date: 2024-11-05SHENZHEN HAODYNE TECH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202410906600.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-08
Publication Date
2024-11-05
Estimated Expiration
2044-07-08

AI Technical Summary

Technical Problem

The low bonding strength of SBR in existing negative electrode slurries leads to low peel strength of the prepared negative electrode sheets.

Method used

The negative electrode binder adopts a core-shell structure. The core layer is composed of aromatic vinyl monomers, aliphatic conjugated unsaturated monomers and vinyl unsaturated carboxylic acid monomers, while the outer shell layer is composed of (meth)acrylate monomers, nitrified vinyl monomers and vinyl unsaturated carboxylic acid monomers, which improves the adhesiveness and affinity of the binder to the electrolyte.

Benefits of technology

It improves the peel strength of the negative electrode and the transport efficiency of lithium ions at the negative electrode interface, thereby enhancing the rate performance and low-temperature performance of the battery.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
Patent Text Reader

Abstract

To overcome the problems of low bonding strength and low peel strength of the prepared negative electrode sheet still existing in the preparation of negative electrode compositions using SBR, this invention provides a negative electrode binder, a negative electrode composition, a negative electrode sheet, and a lithium-ion battery thereof. The negative electrode binder has a core-shell structure, including a core layer and an outer shell layer disposed on the outer surface of the core layer and at least partially covering the core layer. The comonomers of the core layer include aromatic vinyl monomers, aliphatic conjugated unsaturated monomers, vinyl unsaturated carboxylic acid monomers, and multifunctional crosslinking monomers; the comonomers of the outer shell layer include (meth)acrylate monomers, cyanide vinyl monomers, and vinyl unsaturated carboxylic acid monomers. The negative electrode bonding strength provided by this application improves the peel strength of the negative electrode sheet, improves the lithium-ion transport efficiency at the negative electrode interface, and improves the rate performance and low-temperature performance of the battery.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention belongs to the technical field of secondary batteries, and in particular relates to a negative electrode binder, a negative electrode composition, a negative electrode sheet and a lithium ion battery thereof. Background Art

[0002] Lithium-ion batteries have the advantages of high voltage, high specific energy, stable discharge voltage, good cycle performance, good safety performance, and long service life. They are widely used in power vehicles, energy storage and other fields.

[0003] Lithium-ion batteries are generally composed of a positive electrode, a negative electrode, a separator and an electrolyte; the negative electrode includes a negative electrode active material layer, which is obtained by coating the negative electrode slurry on the surface of the negative electrode current collector, drying, rolling and slitting. The negative electrode slurry includes a negative electrode active material, a conductive agent and a negative electrode binder. The existing negative electrode binder is generally SBR, which combines with negative electrode active materials such as graphite and conductive agents such as conductive carbon black through hydrophobic groups on the one hand, and condenses with hydrophilic groups and groups on the surface of the current collector on the other hand, so that the negative electrode binder can connect the negative electrode active material and the conductive agent, and adhere them to the surface of the negative electrode current collector, thereby forming a complete battery structure. In the existing negative electrode slurry preparation process, water-based CMC+SBR has been widely used because it is environmentally friendly, but CMC+SBR still has the problem of low bonding strength and low peeling strength of the prepared negative electrode sheet. Summary of the invention

[0004] The technical problem to be solved by the present invention is that the addition of SBR in the existing negative electrode slurry preparation still has the problem of low bonding strength and low peeling strength of the prepared negative electrode sheet. The present invention provides a negative electrode binder, a negative electrode composition, a negative electrode sheet and a lithium ion battery thereof.

[0005] In order to solve the above technical problems, the present invention provides a negative electrode binder, which has a core-shell structure, including an inner core layer and an outer shell layer disposed on the outer surface of the inner core layer and at least partially covering the inner core layer.

[0006] The comonomers of the inner core layer include aromatic vinyl monomers, aliphatic conjugated unsaturated monomers, vinyl unsaturated carboxylic acid monomers and multifunctional crosslinking monomers;

[0007] The comonomers of the outer shell layer include (meth) acrylic acid ester monomers, cyanide vinyl monomers and vinyl unsaturated carboxylic acid monomers.

[0008] Preferably, the copolymer monomers of the inner core layer include the following weight components: 0.1 to 50 parts of aromatic vinyl monomers, 0.1 to 50 parts of aliphatic conjugated unsaturated monomers, 0.1 to 20 parts of vinyl unsaturated carboxylic acid monomers and 0.1 to 20 parts of multifunctional crosslinking monomers;

[0009] The copolymer monomers of the outer shell layer include the following weight components: 20 to 100 parts of (meth) acrylic acid ester monomers, 1 to 20 parts of cyanide vinyl monomers and 0.1 to 20 parts of vinyl unsaturated carboxylic acid monomers.

[0010] Preferably, the mass percentage of the vinyl unsaturated carboxylic acid monomer in the outer shell layer is ≥ the mass percentage of the vinyl unsaturated carboxylic acid monomer in the inner core layer.

[0011] Preferably, the aromatic vinyl monomer includes one or more of styrene, α-methylstyrene, and vinyltoluene;

[0012] The aliphatic conjugated unsaturated monomer includes one or more of 1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-butadiene, 1,3-cyclopentadiene, and 1,3-hexadiene;

[0013] The vinyl unsaturated carboxylic acid monomer includes one or more of acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, citraconic acid and anhydrides thereof;

[0014] The multifunctional cross-linking monomer includes one or more of dipropylene glycol diacrylate, triethylene glycol di(meth)acrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (300) diacrylate, polyethylene glycol (400) diacrylate, polypropylene glycol (400) diacrylate, tetraethylene glycol dimethacrylate, polyethylene glycol (200) dimethacrylate, polyethylene glycol (400) dimethacrylate, trimethylolpropane triacrylate, 2 (ethoxy) trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, methacryloxypropyl trimethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, allyl trimethoxysilane, methyl allyl trimethoxysilane, polyethylene glycol acrylamide, and N,N'-vinyl bisacrylamide;

[0015] The (meth)acrylate monomers include one or more of ethyl (meth)acrylate, isobutyl (meth)acrylate, butyl (meth)acrylate, 2-isooctyl (meth)acrylate, lauryl (meth)acrylate, and octadecyl (meth)acrylate;

[0016] The cyanated vinyl monomers include one or more of acrylonitrile, methacrylonitrile, 2-butenenitrile, 3-butenenitrile and 2-methyl-3-butenenitrile.

[0017] Preferably, the mass ratio of the inner core layer to the outer shell layer is 1:(0.01-100).

[0018] Preferably, the glass transition temperature of the outer shell layer is -80°C to 10°C.

[0019] Preferably, the mass swelling rate of the negative electrode binder electrolyte is 50% to 500%.

[0020] In a second aspect, the present application provides a negative electrode composition, comprising a negative electrode active material and the negative electrode binder described above.

[0021] Preferably, it further comprises a water-soluble polymer, wherein the water-soluble polymer comprises one or more of lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polyacrylic acid and modified substances thereof;

[0022] The D50 particle size of the negative electrode active material is 2-30 μm.

[0023] In a third aspect, the present application provides a negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one side of the negative electrode current collector, wherein the negative electrode active material layer comprises the negative electrode composition as described above.

[0024] In a fourth aspect, the present application provides a lithium-ion battery, comprising a positive electrode sheet, an electrolyte, and the negative electrode sheet as described above.

[0025] The negative electrode binder provided in the present application is a core-shell structure. When preparing the negative electrode composition, the negative electrode binder has a high viscosity, which can better connect the negative electrode active material and the conductive agent together, improve the cohesion between the negative electrode binder, the conductive agent (such as conductive carbon black), and the negative electrode active material (such as graphite) in the negative electrode sheet, improve the peeling force of the negative electrode sheet, and improve the peeling strength of the negative electrode sheet; the negative electrode binder provided in the present application has an improved affinity with the electrolyte, improves the transmission efficiency of lithium ions at the negative electrode interface, and improves the rate performance and low temperature performance of the battery. DETAILED DESCRIPTION

[0026] In order to make the technical problems, technical solutions and beneficial effects solved by the present invention more clearly understood, the present invention is further described in detail below in conjunction with the embodiments. It should be understood that the specific embodiments described herein are only used to explain the present invention and are not used to limit the present invention.

[0027] An embodiment of the present application provides a negative electrode binder, wherein the negative electrode binder is a core-shell structure, including an inner core layer and an outer shell layer disposed on the outer surface of the inner core layer and at least partially covering the inner core layer.

[0028] The comonomers of the inner core layer include aromatic vinyl monomers, aliphatic conjugated unsaturated monomers, vinyl unsaturated carboxylic acid monomers and multifunctional crosslinking monomers;

[0029] The comonomers of the outer shell layer include (meth) acrylic acid ester monomers, cyanide vinyl monomers and vinyl unsaturated carboxylic acid monomers.

[0030] The negative electrode binder provided in the present application is a core-shell structure. When preparing the negative electrode composition, the negative electrode binder has a high viscosity, which can better connect the negative electrode active material and the conductive agent together, improve the cohesion between the negative electrode binder, the conductive agent (such as conductive carbon black), and the negative electrode active material (such as graphite) in the negative electrode sheet, improve the peeling force of the negative electrode sheet, and improve the peeling strength of the negative electrode sheet; the negative electrode binder provided in the present application has an improved affinity with the electrolyte, improves the transmission efficiency of lithium ions at the negative electrode interface, and improves the rate performance and low temperature performance of the battery.

[0031] In some embodiments, the copolymer monomers of the inner core layer include the following weight components: 0.1 to 50 parts of aromatic vinyl monomers, 0.1 to 50 parts of aliphatic conjugated unsaturated monomers, 0.1 to 20 parts of vinyl unsaturated carboxylic acid monomers and 0.1 to 20 parts of multifunctional crosslinking monomers;

[0032] The copolymer monomers of the outer shell layer include the following weight components: 20 to 100 parts of (meth) acrylic acid ester monomers, 1 to 20 parts of cyanide vinyl monomers and 0.1 to 20 parts of vinyl unsaturated carboxylic acid monomers.

[0033] Specifically, the inner core layer monomer contains 0.1 to 50 parts of aromatic vinyl monomers, which can improve the stability of the negative electrode binder. The specific number of parts of aromatic vinyl monomers in the inner core layer monomers can be 0.1, 5, 10, 13, 18, 23, 27, 30, 34, 38, 40, 42, 47, 50, etc.; as long as the aromatic vinyl monomer is between 0.1 and 50 parts. Preferably, the inner core layer monomer contains 5 to 40 parts of aromatic vinyl monomers, and more preferably, the inner core layer monomer contains 10 to 30 parts of aromatic vinyl monomers.

[0034] The inner core layer monomer contains 0.1 to 50 parts of aliphatic conjugated unsaturated monomers, which can improve the bonding force of the negative electrode binder, help improve the cohesion between the negative electrode binder and the conductive agent such as conductive carbon black, the negative electrode active material such as graphite, improve the bonding force between the negative electrode active material layer and the negative electrode current collector, improve the peeling strength of the negative electrode sheet, and effectively improve the affinity with the electrolyte and the bonding force and liquid retention ability. Specifically, the number of aliphatic conjugated unsaturated monomers in the inner core layer monomer can be 0.1, 5, 10, 13, 18, 23, 27, 30, 34, 38, 42, 47, 50, etc.; as long as the aliphatic conjugated unsaturated monomer is between 0.1 and 50 parts, it can be used.

[0035] The inner core layer monomer contains 0.1 to 20 parts of vinyl unsaturated carboxylic acid monomer, which can form an inner core layer with aliphatic conjugated unsaturated monomers and aromatic vinyl monomers under the action of multifunctional crosslinking monomers, thereby improving the binding force and cohesion of the negative electrode binder. Specifically, the number of parts of the vinyl unsaturated carboxylic acid monomer contained in the inner core layer monomer can be 0.1, 3, 5, 8, 10, 13, 15, 18, 20, etc.; as long as the vinyl unsaturated carboxylic acid monomer is between 0.1 and 20 parts, it can be used.

[0036] The multifunctional cross-linking monomer plays a cross-linking role.

[0037] The outer shell monomer contains 20 to 100 parts of (meth)acrylate monomers, which can improve the interaction between the active material and the conductive agent, improve the cohesion and peeling force of the material, and have a good effect on improving the lithium ion transmission capacity. Specifically, the number of (meth)acrylate monomers contained in the outer shell monomer can be 20, 30, 40, 50, 60, 70, 80, 90, 100, etc.; as long as the (meth)acrylate monomer is between 20 and 100 parts, it can be used.

[0038] The outer shell monomer contains 1 to 20 parts of cyanide vinyl monomers, which have the interaction force between the active material and the conductive agent, and the cohesive force of improving the bonding force. Specifically, the number of cyanide vinyl monomers contained in the outer shell monomer can be 1, 3, 5, 8, 10, 13, 15, 18, 20, etc.; as long as the cyanide vinyl monomers in the outer shell monomer are between 1 and 20 parts, it can be used.

[0039] The outer shell layer monomer contains 0.1 to 20 parts of vinyl unsaturated carboxylic acid monomers to improve the bonding performance of the binder and the adhesion between the binder and the negative electrode current collector. Specifically, the number of vinyl unsaturated carboxylic acid monomers contained in the outer shell layer monomers can be 0.1, 1.0, 3, 5, 8, 10, 13, 15, 18, 20, etc.; as long as the vinyl unsaturated carboxylic acid monomers in the outer shell layer monomers are between 0.1 and 20 parts. In this embodiment, the outer shell layer does not contain SBR.

[0040] In some embodiments, the mass percentage of the vinyl unsaturated carboxylic acid monomer in the outer shell layer is ≥ the mass percentage of the vinyl unsaturated carboxylic acid monomer in the inner core layer.

[0041] Specifically, the mass percentage of the vinyl unsaturated carboxylic acid monomer in the outer shell layer is limited to ≥ the mass percentage of the vinyl unsaturated carboxylic acid monomer in the inner core layer, so that the prepared negative electrode binder has a stronger interaction force with the negative electrode current collector, better adhesion to the negative electrode current collector, and improved peel strength of the electrode sheet.

[0042] In some embodiments, the aromatic vinyl monomer includes one or more of styrene, α-methylstyrene, and vinyltoluene.

[0043] In some embodiments, the aliphatic conjugated unsaturated monomer includes one or more of 1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-butadiene, 1,3-cyclopentadiene, and 1,3-hexadiene.

[0044] In some embodiments, the vinyl unsaturated carboxylic acid monomer includes one or more of acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, citraconic acid and anhydrides thereof.

[0045] In some embodiments, the multifunctional cross-linking monomer includes one or more of dipropylene glycol diacrylate, triethylene glycol di(meth)acrylate, polyethylene glycol (200) diacrylate, polyethylene glycol (300) diacrylate, polyethylene glycol (400) diacrylate, polypropylene glycol (400) diacrylate, tetraethylene glycol dimethacrylate, polyethylene glycol (200) dimethacrylate, polyethylene glycol (400) dimethacrylate, trimethylolpropane triacrylate, 2 (ethoxy) trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, methacryloxypropyl trimethoxysilane, vinyl triethoxysilane, vinyl trimethoxysilane, allyl trimethoxysilane, methylallyl trimethoxysilane, polyethylene glycol acrylamide, and N,N'-vinyl bisacrylamide.

[0046] In some embodiments, the (meth)acrylate monomer includes one or more of ethyl (meth)acrylate, isobutyl (meth)acrylate, butyl (meth)acrylate, 2-isooctyl (meth)acrylate, lauryl (meth)acrylate, and octadecyl (meth)acrylate.

[0047] Specifically, the (meth)acrylate monomer includes at least one of a methacrylate monomer and an acrylate monomer.

[0048] Furthermore, the methacrylate monomer includes one or more of ethyl methacrylate, isobutyl methacrylate, butyl methacrylate, 2-isooctyl methacrylate, lauryl methacrylate, and octadecyl methacrylate.

[0049] The acrylic acid ester monomers include one or more of ethyl acrylate, isobutyl acrylate, butyl acrylate, 2-isooctyl acrylate, lauryl acrylate, and octadecyl acrylate.

[0050] In some embodiments, the cyanated vinyl monomer includes one or more of acrylonitrile, methacrylonitrile, 2-butenenitrile, 3-butenenitrile and 2-methyl-3-butenenitrile.

[0051] In some embodiments, the mass ratio of the inner core layer to the outer shell layer is 1:(0.01-100).

[0052] Specifically, the mass ratio of the inner core layer to the outer shell layer of the negative electrode binder provided by the present application is 1: (0.01~100), which has a wide range, and the inner core layer and the outer shell layer have a higher degree of freedom in selecting the size, thereby increasing the interaction between the negative electrode binder and the negative electrode current collector and increasing the bonding force to the negative electrode current collector. Specifically, the mass ratio of the inner core layer to the outer shell layer can be 1: 0.01, 1: 1, 1: 20, 1: 40, 1: 50, 1: 70, 1: 80, 1: 90, 1: 100, etc., as long as the mass ratio of the inner core layer to the outer shell layer is in the range of 1: (0.01~100).

[0053] In some embodiments, the outer shell layer has a glass transition temperature of -80°C to 10°C.

[0054] Specifically, the glass transition temperature of the outer shell layer is between -80°C and 10°C. A low glass transition temperature is conducive to melting the outer shell layer of the negative electrode binder into a liquid, increasing the contact area with the negative electrode current collector, and improving the bonding force with the negative electrode current collector. Specifically, the glass transition temperature of the outer shell layer is between -80°C and -70°C, -70°C and -60°C, -60°C and -50°C, -50°C and -40°C, -40°C and -30°C, -30°C and -20°C, -20°C and -10°C, -10°C and 0°C or 0°C and 10°C.

[0055] In some embodiments, the mass swelling rate of the negative electrode binder electrolyte is 50% to 500%.

[0056] The mass swelling rate of the negative electrode binder electrolyte is in the range of 50% to 500%, which is beneficial to the storage of the electrolyte, improves the injection efficiency of the electrolyte and the liquid retention effect during the circulation process, and enhances the kinetic performance of the lithium-ion battery.

[0057] In a second aspect, the present application provides a method for preparing a negative electrode binder, comprising the following steps: (1) mixing monomers of a core layer, adding an auxiliary agent, and stirring under heating to obtain a reactant (1);

[0058] (2) After the monomers of the outer shell layer are mixed evenly, the reactant (1) is added and stirred under heating to obtain reactant 2.

[0059] (3) Filter the reactant (2) and add an auxiliary agent to obtain the reactant (3).

[0060] In some embodiments, the auxiliary agent includes one or more of sodium persulfate, ammonium persulfate, potassium persulfate, tert-butyl hydroperoxide, azobisisobutyronitrile, a combination of benzoyl peroxide and sucrose, a combination of tert-butyl hydroperoxide and dactilite, a combination of tert-butyl hydroperoxide and sodium metabisulfite, a combination of benzoyl peroxide and N,N-dimethylaniline, a combination of ammonium persulfate and sodium bisulfite, a combination of potassium persulfate and sodium bisulfite, a combination of hydrogen peroxide and tartaric acid, a combination of hydrogen peroxide and dactilite, a combination of ammonium persulfate and ferrous sulfate, a combination of hydrogen peroxide and ferrous sulfate, a combination of benzoyl peroxide and N,N-diethylaniline, a combination of benzoyl peroxide and ferrous pyrophosphate, a combination of potassium persulfate and silver nitrate, a combination of persulfate and mercaptan, a combination of isopropylbenzene hydroperoxide and ferrous chloride, a combination of potassium persulfate and ferrous chloride, a combination of hydrogen peroxide and ferrous chloride, and a combination of isopropylbenzene hydroperoxide and tetraethyleneimine.

[0061] In a third aspect, the present application provides a negative electrode composition, comprising a negative electrode active material and the negative electrode binder described above.

[0062] The negative electrode composition provided by the present application includes the negative electrode binder of the core-shell structure, which has high viscosity and can better connect the negative electrode active material and the conductive agent together, improve the cohesion between the negative electrode binder, the conductive agent such as conductive carbon black, and the negative electrode active material such as graphite in the negative electrode sheet, improve the peeling force of the negative electrode sheet, and improve the peeling strength of the negative electrode sheet. At the same time, it improves the affinity for the electrolyte and increases the retention capacity of the electrolyte, improves the lithium ion transmission efficiency, and thus improves the kinetic performance of the battery.

[0063] In some embodiments, a water-soluble polymer is also included, and the water-soluble polymer includes one or more of lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polyacrylic acid and modifications thereof.

[0064] Specifically, the water-soluble polymer is combined with the negative electrode binder to improve the ability to better connect the negative electrode active material and the conductive agent together, improve the cohesion between the negative electrode binder, the conductive agent such as conductive carbon black, and the negative electrode active material such as graphite in the negative electrode sheet, enhance the peeling force of the negative electrode sheet, and enhance the peeling strength of the negative electrode sheet.

[0065] In some embodiments, the D50 particle size of the negative electrode active material is 2-30 μm.

[0066] Limiting the particle size of the negative electrode active material to the range of 2 to 30 μm helps the negative electrode binder to connect the negative electrode active material and the conductive agent together, improves the cohesion between the negative electrode binder, the conductive agent such as conductive carbon black, and the negative electrode active material such as graphite in the negative electrode sheet, improves the peeling force of the negative electrode sheet, and improves the peeling strength of the negative electrode sheet. Specifically, the particle size of the negative electrode active material is 2 μm, 5 μm, 8 μm, 10 μm, 15 μm, 17 μm, 19 μm, 20 μm, 22 μm, 25 μm, 28 μm, 30 μm, etc.

[0067] The negative electrode active material includes at least one of graphite and silicon-carbon negative electrode.

[0068] The conductive agent includes at least one of conductive carbon black, carbon nanotubes, graphene, conductive graphite, and carbon fiber.

[0069] In a fourth aspect, the present application provides a negative electrode sheet, comprising a negative electrode current collector and a negative electrode active material layer disposed on at least one side of the negative electrode current collector, wherein the negative electrode active material layer comprises the negative electrode composition as described above.

[0070] The negative electrode sheet provided by the present application comprises the above-mentioned negative electrode composition. The above-mentioned core-shell structured negative electrode binder contained in the negative electrode composition can improve the cohesion between the negative electrode binder, the conductive agent and the negative electrode active material in the negative electrode sheet, improve the adhesion between the negative electrode active material and the negative electrode collector, and improve the peel strength of the negative electrode sheet; and the nucleophilicity of the negative electrode binder and the electrolyte is improved, thereby improving the transmission efficiency of lithium ions at the negative electrode interface, and improving the rate performance and low temperature performance of the battery.

[0071] The negative electrode current collector includes copper foil.

[0072] In a fifth aspect, the present application provides a lithium-ion battery, comprising a positive electrode sheet, an electrolyte and the negative electrode sheet described above.

[0073] The lithium-ion battery provided in the present application contains the negative electrode binder with the core-shell structure, which can improve the cohesion between the negative electrode binder, the conductive agent and the negative electrode active material in the negative electrode sheet, improve the adhesion between the negative electrode active material and the negative electrode collector, and improve the peel strength of the negative electrode sheet; and the nucleophilicity of the negative electrode binder and the electrolyte is improved, thereby improving the transmission efficiency of lithium ions at the negative electrode interface, and improving the rate performance and low temperature performance of the battery.

[0074] The present invention is further described below by way of examples.

[0075] The negative electrode binder, negative electrode composition, negative electrode sheet and lithium ion battery disclosed in the present invention are specifically described.

[0076] Example 1

[0077] 1) Preparation of negative electrode binder

[0078] The comonomers of the inner core layer in Example 1 include the following components: 20 parts of styrene, 30 parts of 1,3-butadiene, 5 parts of methacrylic acid, 8 parts of dipropylene glycol diacrylate and 5 parts of N,N'-vinylbisacrylamide.

[0079] The comonomers of the outer shell layer comprised the following components: 80 parts ethyl acrylate, 8 parts acrylonitrile and 10 parts methacrylic acid.

[0080] The preparation of the negative electrode binder comprises the following steps: (1) mixing the monomers of the inner core layer, adding an auxiliary agent, and stirring under heating to obtain a reactant (1);

[0081] (2) After the monomers of the shell layer are mixed evenly, the reactant (1) is added and stirred under heating to obtain reactant 2.

[0082] (3) Filter the reactant (2) and add an auxiliary agent to obtain the reactant (3).

[0083] The core-shell structured negative electrode binder prepared in Example 1 has a mass ratio of the inner core layer to the outer shell layer of 1:1.44; the glass transition temperature of the outer shell layer is -5°C; and the mass swelling rate of the negative electrode binder electrolyte is 200%.

[0084] 2) Preparation of negative electrode sheet:

[0085] 1.5% of negative electrode binder, 96% of negative electrode active material graphite, 1% of negative electrode conductive agent conductive carbon black, and 1.5% of thickener sodium carboxymethyl cellulose (CMC) were mixed, and deionized water was added for stirring to prepare a negative electrode composition. The negative electrode composition was then coated on both surfaces of the negative electrode current collector Cu foil, and after drying, cold pressing, slitting and other processes, a negative electrode sheet was obtained.

[0086] The particle size of graphite, the negative electrode active material, is 20 μm.

[0087] 3) Preparation of positive electrode:

[0088] 97.3% of positive electrode active material lithium iron phosphate, 1% of positive electrode conductive agent conductive carbon black, and 1.7% of positive electrode binder polyvinylidene fluoride were added to N-methylpyrrolidone and stirred to prepare positive electrode slurry. The positive electrode slurry was then coated on both surfaces of the positive electrode current collector Al foil, and after drying, cold pressing, slitting and other processes, the positive electrode sheet was obtained.

[0089] 4) Lithium-ion battery preparation:

[0090] The positive electrode sheet, the isolation film (PE film), and the negative electrode sheet are stacked in order, with the isolation film placed between the positive and negative electrodes to play an isolating role, to form an electrode assembly, which is placed in an outer package, injected with commercially available electrolyte and packaged, and then subjected to processes such as liquid injection, formation, and exhaust to obtain a lithium-ion battery.

[0091] Example 2

[0092] Most of the steps of Example 2 and Example 1 are the same, except that the components of the inner core layer monomer added to the negative electrode binder are different, as shown below.

[0093] The comonomers of the inner core layer in Example 2 include the following components: 5 parts of styrene, 8 parts of 1,3-butadiene, 2 parts of methacrylic acid, 2 parts of dipropylene glycol diacrylate and 1 part of N,N'-vinylbisacrylamide.

[0094] The core-shell structured negative electrode binder prepared in Example 2 has a mass ratio of the inner core layer to the outer shell layer of 1:5.44; the glass transition temperature of the outer shell layer is -5°C; and the mass swelling rate of the negative electrode binder electrolyte is 320%.

[0095] Example 3

[0096] Most of the steps of Example 3 are the same as those of Example 1, except that the components of the inner core layer monomer added to the negative electrode binder are different, as described below.

[0097] The comonomers of the inner core layer in Example 3 include the following components: 46 parts of styrene, 43 parts of 1,3-butadiene, 7 parts of methacrylic acid, 12 parts of dipropylene glycol diacrylate and 8 parts of N,N'-vinylbisacrylamide.

[0098] The core-shell structured negative electrode binder prepared in Example 3 has a mass ratio of the inner core layer to the outer shell layer of 1:0.84; the glass transition temperature of the outer shell layer is -5°C; and the mass swelling rate of the negative electrode binder electrolyte is 170%.

[0099] Example 4

[0100] Most of the steps of Example 4 are the same as those of Example 1, except that the components of the outer shell layer monomer added to the negative electrode binder are different, as described below.

[0101] The comonomers of the outer shell layer in Example 4 include the following components: 20 parts of ethyl acrylate, 3 parts of acrylonitrile and 8 parts of methacrylic acid.

[0102] The core-shell structured negative electrode binder prepared in Example 4 has a mass ratio of the inner core layer to the outer shell layer of 1:0.46; the glass transition temperature of the outer shell layer is 30° C.; and the mass swelling rate of the negative electrode binder electrolyte is 98%.

[0103] Example 5

[0104] Most of the steps of Example 5 are the same as those of Example 1, except that the components of the outer shell layer monomer added to the negative electrode binder are different, as described below.

[0105] The comonomers of the outer shell layer in Example 5 comprised the following components: 10 parts of ethyl acrylate, 3 parts of acrylonitrile and 8 parts of methacrylic acid.

[0106] The core-shell structured negative electrode binder prepared in Example 5 has a mass ratio of the inner core layer to the outer shell layer of 1:0.31; the glass transition temperature of the outer shell layer is 38° C.; and the mass swelling rate of the negative electrode binder electrolyte is 88%.

[0107] Example 6

[0108] Most of the steps of Example 6 are the same as those of Example 1, except that the components of the outer shell layer monomer added to the negative electrode binder are different, as described below.

[0109] The comonomers of the outer shell layer in Example 6 comprised the following components: 100 parts of ethyl acrylate, 19 parts of acrylonitrile and 18 parts of methacrylic acid.

[0110] The core-shell structured negative electrode binder prepared in Example 6 has a mass ratio of the inner core layer to the outer shell layer of 1:2.01; the glass transition temperature of the outer shell layer is 5°C; and the mass swelling rate of the negative electrode binder electrolyte is 380%.

[0111] Example 7

[0112] Most of the steps of Example 7 are the same as those of Example 1, except that the components of the outer shell layer monomer added to the negative electrode binder are different, as described below.

[0113] The comonomers of the outer shell layer in Example 7 comprised the following components: 50 parts of ethyl acrylate, 10 parts of acrylonitrile and 12 parts of methacrylic acid.

[0114] The core-shell structured negative electrode binder prepared in Example 7 has a mass ratio of the inner core layer to the outer shell layer of 1:1.06; the glass transition temperature of the outer shell layer is 6°C; and the mass swelling rate of the negative electrode binder electrolyte is 330%.

[0115] Example 8

[0116] Most of the steps of Example 8 are the same as those of Example 1, except that the components of the outer shell layer monomer added to the negative electrode binder are different, as described below.

[0117] The comonomers of the outer shell layer in Example 8 comprised the following components: 80 parts of ethyl acrylate, 8 parts of acrylonitrile and 3 parts of methacrylic acid.

[0118] The core-shell structured negative electrode binder prepared in Example 8 has a mass ratio of the inner core layer to the outer shell layer of 1:1.34; the glass transition temperature of the outer shell layer is -10°C; and the mass swelling rate of the negative electrode binder electrolyte is 180%.

[0119] Example 9

[0120] Most of the steps of Example 9 are the same as those of Example 1, except that the components of the outer shell layer monomer added to the negative electrode binder are different, as described below.

[0121] The comonomers of the inner core layer in Example 9 include the following components: 12 parts of α-methylstyrene, 8 parts of vinyltoluene, 10 parts of 1,3-pentadiene, 20 parts of 2-methyl-1,3-butadiene, 3 parts of maleic acid, 2 parts of citraconic acid, 3 parts of polyethylene glycol (200) dimethacrylate, 5 parts of 2 (ethoxy) trimethylolpropane triacrylate and 5 parts of N,N'-vinylbisacrylamide.

[0122] The comonomers of the outer shell layer include the following components: 30 parts of 2-isooctyl acrylate, 50 parts of isobutyl acrylate, 8 parts of acrylonitrile, 6 parts of maleic acid, 2 parts of citraconic acid and 10 parts of methacrylic acid.

[0123] The core-shell structured negative electrode binder prepared in Example 9 has a mass ratio of the inner core layer to the outer shell layer of 1:1.56; the glass transition temperature of the outer shell layer is -25°C; and the mass swelling rate of the negative electrode binder electrolyte is 220%.

[0124] Example 10

[0125] Most of the steps of Example 10 are the same as those of Example 1, except that in the preparation of the negative electrode sheet, the particle size of the negative electrode active material graphite added is different, and the particle size of the negative electrode active material graphite is 5 μm.

[0126] Embodiment 11

[0127] Most of the steps of Example 11 are the same as those of Example 1, except that in the preparation of the negative electrode sheet, the particle size of the negative electrode active material graphite added is different, and the particle size of the negative electrode active material graphite is 25 μm.

[0128] Comparative Example 1

[0129] Most of the steps of Comparative Example 1 and Example 1 are the same, except that the components of the outer shell layer monomer added to the negative electrode binder are different, as shown below.

[0130] The comonomers of the inner core layer in Comparative Example 1 include the following components: 20 parts of styrene, 30 parts of 1,3-butadiene, 5 parts of methacrylic acid, 8 parts of dipropylene glycol diacrylate and 5 parts of N,N'-vinylbisacrylamide.

[0131] The comonomers of the outer shell layer comprised the following components: 20 parts styrene, 80 parts ethyl acrylate, 8 parts acrylonitrile and 10 parts methacrylic acid.

[0132] In the negative electrode binder with a core-shell structure prepared in Comparative Example 1, the mass ratio of the inner core layer to the outer shell layer is 1:1.74; the glass transition temperature of the outer shell layer is 10°C; and the mass swelling rate of the negative electrode binder electrolyte is 140%.

[0133] Comparative Example 2

[0134] Most of the steps of Comparative Example 2 and Example 1 are the same, except that the components of the outer shell layer monomer added to the negative electrode binder are different, as shown below.

[0135] The comonomers of the inner core layer in Comparative Example 2 include the following components: 20 parts of styrene, 30 parts of 1,3-butadiene, 5 parts of methacrylic acid, 8 parts of dipropylene glycol diacrylate and 5 parts of N,N'-vinylbisacrylamide.

[0136] The comonomers of the outer shell layer comprised the following components: 80 parts of ethyl acrylate and 10 parts of methacrylic acid.

[0137] The core-shell structured negative electrode binder prepared in Comparative Example 2 has a mass ratio of the inner core layer to the outer shell layer of 1:1.32; the glass transition temperature of the outer shell layer is -10°C; and the mass swelling rate of the negative electrode binder electrolyte is 155%.

[0138] Comparative Example 3

[0139] Most of the steps of Comparative Example 3 are the same as those of Example 1, except that the negative electrode binder of Comparative Example 3 adopts the existing SBR; the preparation of the negative electrode sheet, the positive electrode sheet, and the lithium-ion battery is the same as that of Example 1.

[0140] Electrical performance test:

[0141] The negative electrode sheets and lithium-ion batteries prepared in the above examples and comparative examples were subjected to the following tests.

[0142] 1) Negative electrode peel strength test:

[0143] After the negative electrode is compacted, a tensile test machine is used to measure the peel strength of the negative electrode sheet. The test method refers to GB2792-2014.

[0144] 2) Low temperature discharge test

[0145] The specific method is: let the soft-pack battery stand until the temperature reaches 25℃±2℃, test the capacity of the soft-pack battery and record it as the capacity before storage, discharge the soft-pack battery at a constant current of 0.5C to a voltage of 2.75V, put it in a -20℃ constant temperature box and let it stand for 300min, charge it at a constant current of 0.5C to a voltage of 4.25V, test the capacity of the soft-pack battery at this time, which is the low-temperature discharge capacity, calculate the discharge capacity retention rate, and the test results are shown in Table 1 below.

[0146] 3) Rate performance test

[0147] The specific method is: let the soft-pack battery stand until the temperature reaches 25℃±2℃, charge to 4.35V at 1C constant current and constant voltage, with a cut-off current of 0.05C; discharge to 2.75V at 1C constant current, and record the discharge capacity; repeat the cycle for 3 weeks, and use the discharge capacity in the third week as the 1C discharge benchmark capacity; charge to 4.35V at 1C constant current and constant voltage, with a cut-off current of 0.05C; discharge to 2.75V at 2C current, record the discharge capacity, and calculate the 2C discharge capacity retention rate.

[0148] (1) The test results obtained in the embodiments and comparative examples are listed in Table 1.

[0149] Table 1

[0150]

[0151] It can be seen that the negative electrode sheet obtained by this method has high peel strength and good electrical properties. As the proportion of the outer layer increases, the peeling force is correspondingly improved, and the electrical properties also tend to increase accordingly. It has good compatibility with graphite, and both large-particle graphite and small-particle graphite show good comprehensive performance. From the comparative example, it can be seen that the use of aromatic monomers in the shell may lead to a decrease in peeling force. Acrylonitrile has a greater effect on peeling force and electrical properties. Compared with conventional SBR, the SBR obtained by this method has excellent comprehensive performance.

[0152] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A negative electrode binder, characterized in that: The negative electrode binder is a core-shell structure, including an inner core layer and an outer shell layer disposed on the outer surface of the inner core layer and at least partially covering the inner core layer. The copolymer monomers of the inner core layer include the following weight components: 0.1 to 50 parts of aromatic vinyl monomers, 0.1 to 50 parts of aliphatic conjugated unsaturated monomers, 0.1 to 20 parts of vinyl unsaturated carboxylic acid monomers and 0.1 to 20 parts of multifunctional crosslinking monomers; The comonomer of the outer shell layer is selected from the following weight components: 20 to 100 parts of (meth)acrylate monomers, 1 to 20 parts of cyanide vinyl monomers and 0.1 to 20 parts of vinyl unsaturated carboxylic acid monomers; The multifunctional cross-linking monomer is selected from one or more of dipropylene glycol diacrylate, triethylene glycol di(meth)acrylate, polyethylene glycol 200 diacrylate, polyethylene glycol 300 diacrylate, polyethylene glycol 400 diacrylate, polypropylene glycol 400 diacrylate, tetraethylene glycol dimethacrylate, polyethylene glycol 200 dimethacrylate, polyethylene glycol 400 dimethacrylate, trimethylolpropane triacrylate, 2(ethoxy)trimethylolpropane triacrylate, pentaerythritol triacrylate, pentaerythritol tetraacrylate, and N,N'-vinyl bisacrylamide; The (meth)acrylate monomer is selected from one or more of ethyl acrylate, isobutyl acrylate, butyl acrylate, isooctyl acrylate, lauryl (meth)acrylate, and octadecyl acrylate.

2. The negative electrode binder according to claim 1, characterized in that The mass percentage of the vinyl unsaturated carboxylic acid monomer in the outer shell layer is ≥ the mass percentage of the vinyl unsaturated carboxylic acid monomer in the inner core layer.

3. The negative electrode binder according to claim 1, characterized in that The aromatic vinyl monomer is selected from one or more of styrene, α-methylstyrene, and vinyltoluene; The aliphatic conjugated unsaturated monomer is selected from one or more of 1,3-butadiene, 1,3-pentadiene, 2-methyl-1,3-butadiene, 1,3-cyclopentadiene, and 1,3-hexadiene; The vinyl unsaturated carboxylic acid monomer is selected from one or more of acrylic acid, methacrylic acid, fumaric acid, maleic acid, itaconic acid, citraconic acid and anhydrides thereof; The cyanated vinyl monomer is selected from one or more of acrylonitrile, methacrylonitrile, 2-butenenitrile, 3-butenenitrile, and 2-methyl-3-butenenitrile.

4. The negative electrode binder according to claim 1, characterized in that The mass ratio of the inner core layer to the outer shell layer is 1:(0.01-100).

5. The negative electrode binder according to claim 1, characterized in that The glass transition temperature of the outer shell layer is -80°C to 10°C; the mass swelling rate of the negative electrode binder electrolyte is 50% to 500%.

6. A negative electrode composition, characterized in that: The invention comprises a negative electrode active material and a negative electrode binder as claimed in any one of claims 1 to 5.

7. The negative electrode composition according to claim 6, characterized in that: It also includes a water-soluble polymer, wherein the water-soluble polymer is selected from one or more of lithium carboxymethyl cellulose, sodium carboxymethyl cellulose, polyacrylic acid and modified substances thereof; The D50 particle size of the negative electrode active material is 2-30 μm.

8. A negative electrode sheet, characterized in that: It comprises a negative electrode current collector and a negative electrode active material layer arranged on at least one side of the negative electrode current collector, wherein the negative electrode active material layer comprises the negative electrode composition as claimed in claim 6 or claim 7.

9. A lithium ion battery, characterized in that: It comprises a positive electrode sheet, an electrolyte and the negative electrode sheet as claimed in claim 8.

Citation Information

Patent Citations

  • Carboxylic styrene butadiene latex and preparation method and application thereof

    CN110407983A

  • Water dispersion type polymer microparticle emulsion binder for lithium ion battery and preparation method of water dispersion type polymer microparticle emulsion binder

    CN115044331A

  • Preparation method of emulsion type binder and application of emulsion type binder in negative electrode of lithium ion battery

    CN115850591A

  • Binder for lithium ion battery, preparation method, negative pole piece and lithium ion battery

    CN117334912A

  • Binder for negative electrode of lithium-ion battery, and preparation method therefor and use thereof

    WO2024002199A1