Functional wood for separating oil and water contaminants containing heavy metals

By pretreating and placing epoxy resin solution on the wood, combining titanium dioxide containing substituted sulfhydryl groups, functional wood is prepared, which solves the problem of heavy metal separation in traditional oil and water pollutant treatment, and achieves rapid and efficient adsorption and detection of multiple heavy metals. Reduced the risk of secondary pollution.

CN118454655BActive Publication Date: 2024-11-26DONGGUAN UNIV OF TECH
View PDF 8 Cites 0 Cited by

Patent Information

Application Number
CN202410559617.0
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-08
Publication Date
2024-11-26
Estimated Expiration
2044-05-08

AI Technical Summary

Technical Problem

The traditional oil and water pollutant treatment methods have complex processes and are difficult to detect and separate heavy metals. The existing superhydrophobic materials have slow separation speed, low efficiency, and a single type of separation of heavy metals, which has the problem of secondary pollution.

Method used

By pretreating and placing an epoxy resin solution on the wood, combining titanium dioxide containing substituted thiol groups, functional wood with superhydrophobic, porous structure and high specific surface area is prepared, and complexing reactions between thiol groups and heavy metal ions are used to achieve rapid detection and high efficiency Adsorption.

Benefits of technology

It achieves rapid separation and efficient adsorption of a variety of heavy metals, reduces the risk of secondary pollution, and has excellent photocatalytic properties, which can degrade adsorbed organic pollutants.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118454655B_ABST
    Figure CN118454655B_ABST
Patent Text Reader

Abstract

The present invention relates to the technical field of sewage treatment, and discloses a functional wood for separating oily water pollutants containing heavy metals. First, natural balsa wood is treated with sodium chlorite to remove lignin and hemicellulose, and then immersed in an epoxy resin solution, and then loaded with titanium dioxide containing sulfhydryl groups through a pre-curing process. The functional wood prepared by the present invention not only has a super-hydrophobic surface, but also has a three-dimensional porous structure and a large specific surface area, and has high adsorption efficiency and fast separation efficiency. In addition, the presence of a large number of sulfhydryl groups makes the functional wood highly sensitive to the color development of different heavy metals, and can also utilize the photocatalytic effect of titanium dioxide to degrade the organic pollutants adsorbed by the functional wood, giving the functional wood excellent photocatalytic performance, and then achieving the purpose of not causing secondary pollution.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sewage treatment, and in particular to a functional wood for separating oily water pollutants containing heavy metals. Background Art

[0002] There are complex components in oily wastewater, and heavy metals, as typical pollutants that are difficult to biodegrade, are widely present in oil and water pollutants. Traditional oil spill recovery methods, such as floating oil salvage, chemical dispersion, combustion and bioremediation, all have serious shortcomings such as complex processes, secondary pollution and difficulty in detecting and separating heavy metals. In order to treat oil and water pollutants and detect and separate heavy metals in them, a new and efficient detection and separation technology is urgently needed.

[0003] Superhydrophobic material is a material with special surface properties, and its static contact angle of water droplets is greater than 150°. In recent years, with the continuous development of science and technology, this material has received extensive attention and application in the field of oil-water separation. However, the presence of heavy metals not only increases the difficulty of treating oily wastewater, but may also react chemically with related devices, resulting in material corrosion and performance degradation. Since the current oil-water separation materials containing heavy metals have problems such as slow separation speed, low efficiency, single type of separated heavy metals, and secondary pollution, therefore, developing a stable superhydrophobic wood with fast separation speed, high separation efficiency, easy detection and adsorption of multiple heavy metals, and no pollution, and applying it to the rapid detection and separation of heavy metal oil and water pollutants is of great significance to solving heavy metal and oil pollution. Summary of the invention

[0004] In order to solve the technical problems mentioned in the background technology, the object of the present invention is to provide a functional wood for separating water pollutants containing heavy metals.

[0005] The purpose of the present invention can be achieved through the following technical solutions:

[0006] A functional wood for separating oil and water pollutants containing heavy metals, wherein the preparation method of the functional wood comprises the following steps:

[0007] Step 1: Wood pretreatment

[0008] After cleaning the wood surface, drying it, placing it in a sodium chlorite solution, heating it, keeping it warm at 60-100° C. for 0.5-3 hours, taking it out, washing it and drying it, to obtain the pretreated wood;

[0009] Step 2: Prepare epoxy resin solution

[0010] Mix epoxy resin and curing agent polyamide in a mass ratio of 1:1, add an organic solvent, stir and mix, and prepare an epoxy resin solution with a mass fraction of 5-80%;

[0011] Step 3: Prepare functional wood

[0012] The pretreated wood is immersed in an epoxy resin solution, taken out after 10-60 minutes, pre-cured at a temperature of 40-80°C for 5-60 minutes, then immersed in an acetone solution of titanium dioxide containing substituted mercapto groups, taken out after 1-3 minutes, and dried at a temperature of 60-100°C for 1-8 hours to obtain functional wood.

[0013] Specifically, in the first step, the wood is treated with sodium chlorite, and the lignin and hemicellulose in the wood are oxidized and decomposed, which causes a large number of pore structures to form on the surface of the wood and increases the pore size of the original pores, which is beneficial for the wood to show a larger specific surface area.

[0014] In the third step, the wood is first soaked in an epoxy resin solution. During this process, the epoxy resin adheres to the surface of the wood to form epoxy resin-loaded wood. The presence of epoxy resin can increase the light reflectivity of the wood, giving the wood super-hydrophobic properties and translucent characteristics, thereby improving the observability of subsequent color changes after the wood complexes with metal ions. Then, the curing degree of the epoxy resin is controlled, and titanium dioxide containing substituted mercapto groups is deposited on the surface of the wood to increase the surface roughness of the wood and give the wood photocatalytic function.

[0015] As a further embodiment of the present invention, in the first step, the wood is natural balsa wood with a density of 80-120 kg / m 3 .

[0016] As a further embodiment of the present invention, in the first step, the concentration of the sodium chlorite solution is 5-30 g / L.

[0017] As a further embodiment of the present invention, in the second step, the organic solvent is at least one of toluene, tetrahydrofuran or acetone.

[0018] As a further embodiment of the present invention, in the third step, the titanium dioxide acetone solution containing substituted mercapto groups is prepared by the following method:

[0019] Step 1: Preparation of modified titanium dioxide

[0020] Mix α-lipoic acid and tetrahydrofuran, stir evenly, add a condensing agent and a catalyst to the resulting mixed solution, stir at room temperature for 20-30 minutes, then add nano-titanium dioxide to the mixed solution, ultrasonically treat at an ultrasonic frequency of 80-100 kHz for 30-40 minutes, and then stir at a speed of 1000-2000 r / min for 4-6 hours, filter the material, wash and dry it to form a titanium dioxide modified body;

[0021] Step 2: Preparation of titanium dioxide containing substituted mercapto groups

[0022] The modified titanium dioxide is dispersed in N,N-dimethylformamide, and a reducing agent is added to the dispersion under continuous stirring. After the addition is completed, stirring is continued for 2-4 hours at room temperature, and then the material is discharged and the solid material is separated to obtain titanium dioxide containing substituted mercapto groups.

[0023] Step 3: Preparation of titanium dioxide acetone solution containing substituted mercapto groups

[0024] The titanium dioxide containing substituted mercapto groups is mixed with acetone, and ultrasonically treated at an ultrasonic frequency of 60-80 kHz for 1-2 hours to form an acetone solution of titanium dioxide containing substituted mercapto groups.

[0025] Specifically, in step 1, a condensing agent and a catalyst are first used to activate the substituted carboxyl group in the α-lipoic acid structure, so that it can undergo esterification condensation with the hydroxyl group on the surface of nano-titanium dioxide to form a modified titanium dioxide.

[0026] In step 2, due to the presence of a reducing agent, the disulfide bonds in the lipoic acid modified on the surface of the titanium dioxide modifier are reduced to two equivalent thiol functional groups to obtain titanium dioxide containing substituted thiol groups, which is finally ultrasonically dispersed in acetone to form an acetone solution of titanium dioxide containing substituted thiol groups.

[0027] As a further solution of the present invention, in step 1, the nano titanium dioxide is anatase nano titanium dioxide with a particle size of 5-30 nm.

[0028] As a further embodiment of the present invention, in step 1, the condensing agent is any one of N,N'-dicyclohexylcarbodiimide or 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride.

[0029] As a further embodiment of the present invention, in step 1, the catalyst is at least one of N-hydroxysuccinimide, 1-hydroxybenzotriazole or 4-dimethylaminopyridine.

[0030] As a further embodiment of the present invention, in step 2, the reducing agent is tributylphosphine.

[0031] As a further embodiment of the present invention, in step three, the mass fraction of the titanium dioxide acetone solution containing substituted mercapto groups is 1-30%.

[0032] Beneficial effects of the present invention:

[0033] 1) The present invention modifies nano titanium dioxide with α-lipoic acid and then reduces the disulfide bonds in the α-lipoic acid structure to obtain nano titanium dioxide with a large number of substituted thiol groups on the surface. The presence of these thiol groups can produce a complex reaction with heavy metal ions to form complexes. On the one hand, these complexes have special colors, thereby achieving the purpose of efficient and rapid heavy metal detection and adsorption. On the other hand, these complexes have strong hydrophobicity, which makes the solubility of the complexes in water low and easy to precipitate from the aqueous phase.

[0034] 2) The functional wood prepared by the present invention not only has a super-hydrophobic surface, but also has a three-dimensional porous structure and a large specific surface area, with high adsorption efficiency and fast separation efficiency. In addition, the presence of a large number of thiol groups makes the functional wood highly sensitive to the color development of different heavy metals, and can also utilize the photocatalytic effect of titanium dioxide to degrade organic pollutants adsorbed by the functional wood, giving the functional wood excellent photocatalytic properties, thereby achieving the purpose of not causing secondary pollution.

[0035] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0037] Figure 1 This is an infrared analysis test diagram of titanium dioxide containing substituted mercapto groups;

[0038] Figure 2 is a scanning electron microscope image of the pretreated wood in Example 2;

[0039] Figure 3 This is a scanning electron microscope image of the functional wood in Example 2. DETAILED DESCRIPTION

[0040] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0041] The titanium dioxide acetone solution containing substituted mercapto groups in the following examples is prepared by the following method:

[0042] Step 1: Preparation of modified titanium dioxide

[0043] 1.2 g of α-lipoic acid and tetrahydrofuran were mixed and stirred evenly, and then 0.5 g of N,N'-dicyclohexylcarbodiimide and 0.2 g of N-hydroxysuccinimide were added to the resulting mixed solution. After the addition was completed, the mixture was stirred at room temperature for 30 min. Then, 1.5 g of anatase nano-titanium dioxide with a particle size of 30 nm was added to the mixed solution, and ultrasonic treatment was performed at an ultrasonic frequency of 100 kHz for 30 min. Then, the mixture was stirred at a speed of 1500 r / min for 6 h, and the material was filtered, washed, and dried to form a titanium dioxide modified body;

[0044] Step 2: Preparation of titanium dioxide containing substituted mercapto groups

[0045] Disperse 1 g of modified titanium dioxide in N,N-dimethylformamide, add 0.5 g of tributylphosphine to the dispersion under continuous stirring, and after the addition is completed, continue stirring for 3 hours at room temperature, discharge the material, separate the solid material, and obtain titanium dioxide containing substituted mercapto groups;

[0046] Figure 1 This is the infrared analysis test diagram of the titanium dioxide containing substituted mercapto groups. The analysis shows that 3441cm -1 The absorption peak at 2561 cm is the characteristic absorption peak of the hydroxyl groups on the titanium dioxide surface that did not participate in the reaction. -1 The absorption peak at 1748 cm is the characteristic absorption peak of thiol. -1 The absorption peak that appears at is the C=O characteristic absorption peak of the ester group.

[0047] Step 3: Preparation of titanium dioxide acetone solution containing substituted mercapto groups

[0048] The titanium dioxide containing substituted mercapto groups is mixed with acetone, and ultrasonically treated at an ultrasonic frequency of 80 kHz for 1 hour to prepare a titanium dioxide acetone solution containing substituted mercapto groups with a mass fraction of 5%. Example

[0049] A functional wood for separating oily water pollutants containing heavy metals is prepared by the following method:

[0050] Step 1: Wood pretreatment

[0051] The specifications are 30mm×30mm×3mm and the density is 100kg / m 3 The surface of the natural balsa wood was cleaned, dried, placed in a sodium chlorite solution with a concentration of 5 g / L, the pH value was adjusted to 3, the heating was turned on, and the temperature was kept at 60°C for 3 hours, taken out, washed and dried to obtain the pretreated wood;

[0052] Step 2: Prepare epoxy resin solution

[0053] E44 epoxy resin and curing agent polyamide were mixed in a mass ratio of 1:1, and an organic solvent was added, stirred and mixed to prepare an epoxy resin solution with a mass fraction of 5%;

[0054] Step 3: Prepare functional wood

[0055] The pretreated wood is immersed in an epoxy resin solution, taken out after 10 minutes, pre-cured at 40°C for 60 minutes, then immersed in an acetone solution of titanium dioxide containing substituted mercapto groups, taken out after 1 minute, and dried at 60°C for 8 hours to obtain functional wood. Example

[0056] A functional wood for separating oily water pollutants containing heavy metals is prepared by the following method:

[0057] Step 1: Wood pretreatment

[0058] The specifications are 30mm×30mm×3mm and the density is 100kg / m 3 The surface of the natural balsa wood was cleaned and dried, and then placed in a sodium chlorite solution with a concentration of 10 g / L, the pH value was adjusted to 3, and the heating was turned on. The solution was kept at 80°C for 2 hours, and then taken out, washed and dried to obtain the pretreated wood.

[0059] Figure 2 The scanning electron microscope (SEM) image of the pretreated wood is Figure 2 It can be seen that it has a honeycomb porous structure with large pores, which is conducive to the subsequent filling of epoxy resin.

[0060] Step 2: Prepare epoxy resin solution

[0061] E44 epoxy resin and curing agent polyamide were mixed in a mass ratio of 1:1, and toluene was added and stirred to prepare an epoxy resin solution with a mass fraction of 30%;

[0062] Step 3: Prepare functional wood

[0063] The pretreated wood is immersed in an epoxy resin solution, taken out after 20 minutes, and pre-cured at 60°C for 30 minutes. Then, it is immersed in an acetone solution of titanium dioxide containing substituted mercapto groups, taken out after 2 minutes, and dried at 80°C for 4 hours to obtain functional wood.

[0064] Figure 3 This is the scanning electron microscope (SEM) image of functional wood. Figure 3 It can be seen that the surface of the wood is evenly wrapped by the epoxy resin, and the titanium dioxide is firmly fixed on the wood by the epoxy resin. Example

[0065] A functional wood for separating oily water pollutants containing heavy metals is prepared by the following method:

[0066] Step 1: Wood pretreatment

[0067] The specifications are 30mm×30mm×3mm and the density is 100kg / m 3 The surface of the natural balsa wood was cleaned and dried, and then placed in a sodium chlorite solution with a concentration of 30 g / L, the pH value was adjusted to 3, the heating was turned on, and the temperature was kept at 100° C. for 0.5 h, and then taken out, washed and dried to obtain the pretreated wood;

[0068] Step 2: Prepare epoxy resin solution

[0069] E44 epoxy resin and curing agent polyamide were mixed in a mass ratio of 1:1, and toluene was added and stirred to prepare an epoxy resin solution with a mass fraction of 80%;

[0070] Step 3: Prepare functional wood

[0071] The pretreated wood is immersed in an epoxy resin solution, taken out after 60 minutes, pre-cured at 80°C for 5 minutes, then immersed in an acetone solution of titanium dioxide containing substituted mercapto groups, taken out after 3 minutes, and dried at 100°C for 1 hour to obtain functional wood.

[0072] Comparative Example 1

[0073] A functional wood is prepared by the following method:

[0074] Step 1: Wood pretreatment

[0075] The specifications are 30mm×30mm×3mm and the density is 100kg / m 3The surface of the natural balsa wood was cleaned and dried, and then placed in a sodium chlorite solution with a concentration of 10 g / L, the pH value was adjusted to 3, the heating was turned on, and the temperature was kept at 80°C for 2 hours, and then the pretreated wood was obtained after washing and drying.

[0076] Step 2: Prepare epoxy resin solution

[0077] E44 epoxy resin and curing agent polyamide were mixed in a mass ratio of 1:1, and toluene was added and stirred to prepare an epoxy resin solution with a mass fraction of 30%;

[0078] Step 3: Prepare functional wood

[0079] The pretreated wood was immersed in epoxy resin solution, taken out after 20 minutes, and pre-cured at 60°C for 8 hours to obtain functional wood.

[0080] Comparative Example 2

[0081] A functional wood is prepared by the following method:

[0082] Step 1: Wood pretreatment

[0083] The specifications are 30mm×30mm×3mm and the density is 100kg / m 3 The surface of the natural balsa wood was cleaned and dried, and then placed in a sodium chlorite solution with a concentration of 10 g / L, the pH value was adjusted to 3, the heating was turned on, and the temperature was kept at 80°C for 2 hours, and then the pretreated wood was obtained after washing and drying.

[0084] Step 2: Prepare functional wood

[0085] The pretreated wood is immersed in an acetone solution of titanium dioxide containing substituted mercapto groups, taken out after 2 minutes, and dried at 80°C for 8 hours to obtain functional wood.

[0086] Comparative Example 3

[0087] A functional wood is prepared by the following method:

[0088] Step 1: Wood pretreatment

[0089] The specifications are 30mm×30mm×3mm and the density is 100kg / m 3 The surface of the natural balsa wood was cleaned and dried, and then placed in a sodium chlorite solution with a concentration of 10 g / L, the pH value was adjusted to 3, the heating was turned on, and the temperature was kept at 80°C for 2 hours, and then the pretreated wood was obtained after washing and drying.

[0090] Step 2: Prepare epoxy resin solution

[0091] E44 epoxy resin and curing agent polyamide were mixed in a mass ratio of 1:1, and toluene was added and stirred to prepare an epoxy resin solution with a mass fraction of 30%;

[0092] Step 3: Prepare functional wood

[0093] The pretreated wood was immersed in an epoxy resin solution, taken out after 20 minutes, then immersed in an acetone solution of titanium dioxide containing substituted mercapto groups, taken out after 2 minutes, and dried at 80°C for 4 hours to obtain functional wood.

[0094] The functional wood in Examples 1 to 3 and Comparative Examples 1 to 3 was subjected to the following tests:

[0095] ①. Use SDC-200S contact angle meter to test water contact angle;

[0096] ②. Use glass tube, functional wood, clamps and beaker to form a simple oil-water separation device, in which the functional wood is fixed in the middle of the glass tube as a filter membrane. Take 10g toluene-acetone solution, 10g water and 100mg / L copper sulfate solution in a beaker and mix them to prepare heavy metal oil-water pollutants. Pour it from the top of the glass tube, record the quality of toluene-acetone solution separated and recovered by the functional wood, and evaluate the oil-water separation ability of the functional wood;

[0097] ③. Take out the functional wood tested in ②, put it into the oven to dry completely, then take it out to observe the color and evaluate the heavy metal color detection ability of the functional wood;

[0098] ④. Prepare the same heavy metal oil and water pollutants as in ②, immerse the functional wood in the heavy metal oil and water pollutants, take out and dry after 8 hours, and determine the heavy metal adsorption capacity of the functional wood by calculating the mass difference before and after adsorption;

[0099] The test results are shown in the table below:

[0100]

[0101] Analysis of the test data in the table shows that the functional wood prepared in Examples 1 to 3 of the present invention has a super-hydrophobic surface and exhibits excellent heavy metal adsorption and color development capabilities, and can quickly separate oil and water pollutants containing heavy metals and detect heavy metal types.

[0102] Compared with the embodiment, the various properties of the functional wood prepared by Comparative Examples 1 to Comparative Examples 3 all show different degrees of reduction, which indicates that when the loading of mercapto-modified titanium dioxide, the loading of epoxy resin or the pre-curing process conditions change, the various properties of the functional wood will be greatly affected. Among them, the functional wood prepared without impregnation with epoxy resin solution presents an opaque characteristic, so no obvious color change on the surface can be observed after separating copper, oil and water pollutants, and the adsorption effect is greatly reduced due to the shedding of titanium dioxide. Part of the titanium dioxide in the functional wood prepared without pre-curing process will be wrapped inside by epoxy resin, resulting in the inability to exert the original adsorption effect, so the heavy metal adsorption effect is poor.

[0103] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

[0104] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. Such modifications or replacements will not cause the essence of the corresponding technical solutions to deviate from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A functional wood for separating oil and water pollutants containing heavy metals, characterized in that: The method for preparing the functional wood comprises the following steps: Step 1: Wood pretreatment After cleaning the wood surface, drying it, placing it in a sodium chlorite solution, heating it, keeping it warm at 60-100° C. for 0.5-3 hours, taking it out, washing it and drying it, to obtain the pretreated wood; Step 2: Prepare epoxy resin solution Mix epoxy resin and curing agent polyamide in a mass ratio of 1:1, add an organic solvent, stir and mix, and prepare an epoxy resin solution with a mass fraction of 5-80%; Step 3: Prepare functional wood The pretreated wood is immersed in an epoxy resin solution, taken out after 10-60 minutes, pre-cured at a temperature of 40-80°C for 5-60 minutes, then immersed in an acetone solution of titanium dioxide containing substituted mercapto groups, taken out after 1-3 minutes, and dried at a temperature of 60-100°C for 1-8 hours to obtain functional wood; The titanium dioxide acetone solution containing substituted mercapto groups is prepared by the following method: Step 1: Preparation of modified titanium dioxide Mix α-lipoic acid and tetrahydrofuran, stir evenly, add a condensing agent and a catalyst to the resulting mixed solution, stir at room temperature for 20-30 minutes, then add nano-titanium dioxide to the mixed solution, ultrasonically treat at an ultrasonic frequency of 80-100 kHz for 30-40 minutes, and then stir at a speed of 1000-2000 r / min for 4-6 hours, filter the material, wash and dry it to form a titanium dioxide modified body; Step 2: Preparation of titanium dioxide containing substituted mercapto groups The modified titanium dioxide is dispersed in N,N-dimethylformamide, and a reducing agent is added to the dispersion under continuous stirring. After the addition is completed, stirring is continued for 2-4 hours at room temperature, and then the material is discharged and the solid material is separated to obtain titanium dioxide containing a substituted mercapto group; Step 3: Preparation of titanium dioxide acetone solution containing substituted mercapto groups The titanium dioxide containing substituted mercapto groups is mixed with acetone, and ultrasonically treated at an ultrasonic frequency of 60-80 kHz for 1-2 hours to form an acetone solution of titanium dioxide containing substituted mercapto groups.

2. The functional wood for separating oil and water pollutants containing heavy metals according to claim 1, characterized in that: In the first step, the wood is natural balsa wood with a density of 80-120 kg / m 3 .

3. The functional wood for separating oil and water pollutants containing heavy metals according to claim 1, characterized in that: In the first step, the concentration of the sodium chlorite solution is 5-30 g / L.

4. The functional wood for separating oil and water pollutants containing heavy metals according to claim 1, characterized in that: In the second step, the organic solvent is at least one of toluene, tetrahydrofuran or acetone.

5. The functional wood for separating oil and water pollutants containing heavy metals according to claim 1, characterized in that: In step 1, the nano titanium dioxide is anatase nano titanium dioxide with a particle size of 5-30 nm.

6. The functional wood for separating oil and water pollutants containing heavy metals according to claim 1, characterized in that: In step 1, the condensing agent is any one of N,N'-dicyclohexylcarbodiimide or 1-ethyl-3-(3-dimethylaminopropyl)carbodiimide hydrochloride.

7. The functional wood for separating oil and water pollutants containing heavy metals according to claim 1, characterized in that: In step 1, the catalyst is at least one of N-hydroxysuccinimide, 1-hydroxybenzotriazole or 4-dimethylaminopyridine.

8. The functional wood for separating oil and water pollutants containing heavy metals according to claim 1, characterized in that: In step 2, the reducing agent is tributylphosphine.

9. The functional wood for separating oil and water pollutants containing heavy metals according to claim 1, characterized in that: In step 3, the mass fraction of the titanium dioxide acetone solution containing substituted mercapto groups is 1-30%.

Citation Information

Patent Citations

  • Method for preparing adsorbent of heavy metal ions in water

    CN101954268A

  • Air purifying material preparation method

    CN108479707A

  • Novel polyaniline / titanium dioxide composite material and application thereof to environment restoration

    CN108554459A

  • Preparation method of carbon fiber-loaded nano titanium dioxide photocatalysis composite material

    CN109331805A

  • Super-hydrophobic and photocatalytic paint and preparation method thereof

    CN111019476A