A low-pressure casting method for low-cost thick-walled steering knuckle

By optimizing the production process of the steering knuckle through the low-pressure casting method and the bottom-injection pouring system, the problems of high forging molding costs and long cycle times are solved, and low-cost and efficient steering knuckle manufacturing is achieved.

CN118477981BActive Publication Date: 2024-10-29SHANDONG JINMA AUTOMOBILE EQUIP TECH CO LTD
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202410574293.8
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-05-10
Publication Date
2024-10-29
Estimated Expiration
2044-05-10

AI Technical Summary

Technical Problem

In the existing technology, the forging cost of the steering knuckle is high and the production cycle is long. Especially after aluminum alloy replaces steel materials, it is difficult to achieve low-cost and efficient manufacturing.

Method used

The low-pressure casting method is adopted, and the low-cost production of the steering knuckle is achieved through three-dimensional software modeling, bottom-gating pouring system design, numerical simulation analysis, initial pouring parameter calculation, pouring system structure optimization, casting process parameter optimization, mold design and other steps.

Benefits of technology

By accurately controlling the pressure and time of each stage of low-pressure casting, energy consumption is reduced, low-cost manufacturing of the steering knuckle is achieved, and production costs and cycles are reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN118477981B_ABST
    Figure CN118477981B_ABST
Patent Text Reader

Abstract

The present invention discloses a low-cost, thick-walled steering knuckle low-pressure casting method, which relates to the field of steering knuckle manufacturing, and specifically includes the steps of steering knuckle process analysis, pouring system design, mathematical model analysis of numerical simulation during casting, initial pouring parameter calculation, pouring system structure optimization, casting process parameter optimization, casting mold design, etc. In the present invention, low-pressure casting and bottom pouring are used to produce the steering knuckle, the cross-sectional ratio of the corresponding position of the steering knuckle is optimized, and the liquid lifting pressure, filling pressure, boost pressure, holding pressure and holding time, and pressure relief pressure and pressure relief time in each stage of low-pressure casting are accurately determined in combination with the pouring system and the casting data itself. When each stage is successfully completed, the entire low-pressure casting process of the steering knuckle is completed, and the pressure and time in each stage are controlled to reduce energy consumption and achieve low-cost manufacturing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steering knuckle manufacturing, in particular to a low-cost, thick-walled steering knuckle low-pressure casting method. Background Art

[0002] The steering knuckle, also known as the "ram's horn", is one of the important parts in the steering axle of the car. It can make the car run stably and transmit the driving direction sensitively. It transmits and bears the front load of the car, supports and drives the front wheel to rotate around the kingpin to make the car turn. When the car is running, it bears variable impact loads, so it is required to have high strength.

[0003] However, in the prior art, steering knuckles are usually produced by forging hydraulic presses. The metal material is heated to a certain temperature and then plastically deformed. The shape and structure of the material can be changed by forging. After the steps of material selection, preheating, forging and annealing, the required mechanical properties are obtained. However, as aluminum alloys replace materials such as steel, the forging cost is high and the production cycle is relatively long. Summary of the invention

[0004] The purpose of the present invention is to provide a low-cost, thick-walled steering knuckle low-pressure casting method to solve the problem of high forging cost and relatively long production cycle after aluminum alloy replaces steel and other materials mentioned in the background art.

[0005] To achieve the above object, the present invention provides the following technical solution: a low-cost, thick-walled steering knuckle low-pressure casting method, comprising the following steps:

[0006] S1. Steering knuckle process analysis: Use 3D software to model steering knuckles of different sizes;

[0007] S2. Casting system design: The steering knuckle is cast at low pressure using a bottom pouring system, which includes the design of the inner runner, the cross runner, and the riser pipe. The gating system model is established using the steering knuckle 3D model.

[0008] S3. Mathematical model analysis of numerical simulation in casting process: During the low-pressure casting filling and solidification process, the casting involves the shrinkage of aluminum alloy liquid. The mathematical model of the process is established to prepare for the subsequent numerical simulation analysis and defect prediction;

[0009] S4. Calculation of initial pouring parameters: The low-pressure casting process includes a liquid raising stage, a pressurization stage, a pressure holding stage, and a pressure relief and piece removal stage. The liquid raising pressure, filling pressure, pressurization pressure, pressure holding pressure and pressure holding time, and pressure relief pressure and pressure relief time are determined during the process.

[0010] S5. Optimization of pouring system structure: Optimize the size of the runner and riser, and select the ratio of the cross-sectional area of ​​the runner to the inner gate as A. 横 :A 内 =2.4:1.6;

[0011] S6. Optimization of casting process parameters: Optimize the pouring temperature and mold preheating temperature with the goal of casting quality and casting efficiency;

[0012] S7. Casting mold design: determine the material, size, draft angle, cooling system and exhaust system of the metal mold;

[0013] S8. Using the above steps, a steering knuckle is obtained by low-pressure casting.

[0014] Preferably, in step S2, in the low-pressure casting process, the ingates of the pouring system play a role in introducing molten metal and compensating shrinkage of the casting during solidification. The cross-sectional area of ​​the ingates is usually calculated using the "thermal pitch circle method". The theoretical value is preliminarily calculated, and the formula is as follows:

[0015]

[0016] Where A is the cross-sectional area of ​​the ingrate, in cm2; G is the mass of the casting, in g; ρ is the density of the molten metal, in g / cm3; V is the linear velocity of the ingrate, in cm / s;

[0017] Then make numerical corrections based on actual pouring experience, the formula is as follows;

[0018]

[0019] t is the filling time, unit is s; h is the height of the metal mold cavity, unit is cm; v0 is the liquid rising speed, unit is cm / s;

[0020] When v≤15cm / s, the metal liquid level fills the mold cavity smoothly without turbulence. At the same time, the liquid rising speed is selected according to the wall thickness of the casting. The range of v0 is 1-6cm / s. For castings with thicker walls, the liquid rising speed takes a larger value.

[0021] When filling the mold, the riser pipe guides the molten metal in the crucible into the pouring system, which mainly plays the role of drainage and shrinkage compensation. When designing the riser pipe, the molten metal should have a stable liquid level during the filling process, and it is also necessary to meet the requirements of molten metal heat transfer, degassing, and slag filtering. In order to prevent the oxide inclusions in the crucible from entering the casting cavity through the riser pipe, the lower end of the riser pipe is required to be 50 to 100 mm away from the molten metal level in the crucible; at the same time, considering the convenience of cleaning, the inner diameter of the riser pipe is required to be greater than 35 mm.

[0022] Preferably, in step S3, the flow of the aluminum alloy liquid in the mold cavity follows the law of conservation of mass, the law of conservation of momentum and the law of conservation of energy, thereby establishing a mathematical model.

[0023] Preferably, in step S4:

[0024] The liquid rising stage: before the filling begins, all exhaust holes in the crucible are closed, and then dry gas is filled into the crucible. The gas pressure inside the crucible is continuously increased, so that the metal liquid surface starts to fill the mold from bottom to top through the liquid rising pipe, and the gas pressure is continuously increased until the metal liquid fills the entire pouring system, that is, the metal liquid rises in the pouring system, and the range of the liquid rising pressure is greater than or equal to 0.004MPa;

[0025] The filling stage: under the liquid pressure, the metal liquid level is now located at the inner gate, and the pressure continues to increase. The metal liquid level begins to rise slowly until it reaches the top of the steering knuckle. At this time, the aluminum alloy metal liquid will fill the entire cavity of the steering knuckle. The filling pressure range is 0.017-0.026MPa;

[0026] The pressurization stage: in order to make the casting more compact, after the molten metal fills the entire cavity, continue to apply pressure to the crucible, so that the filled casting begins to solidify and cool under relatively high pressure. In the pressurization stage, the molten metal begins to solidify, and the casting shrinks during the solidification process. Continuing to increase the pressure will make the shrinking casting compensated by new molten metal, that is, the aluminum alloy molten metal fills the entire cavity and begins to cool under pressure. The pressurization pressure range is 0.027-0.042MPa;

[0027] The holding stage: after the pressurization stage, the boost pressure needs to be maintained for a period of time in this stage. The unsolidified casting is cooled and solidified under the action of the holding pressure and the holding time to become a formed casting. At this time, the holding pressure is the same as the boost pressure, that is, the aluminum alloy molten metal solidifies and cools in this stage, and the holding pressure range is 0.027-0.042MPa; the selection of the holding time should take into account the solidification of the casting and the utilization rate of the molten metal. When the holding time is less than the solidification time of the casting, the quality of the casting in the mold cavity will be reduced; when the holding time is too long, the molten metal participating in the filling will solidify in the pouring system, and residues will appear on the inner wall of the pouring system, which requires manual cleaning later, and reduces the utilization rate of the casting molten metal, so the holding time is greater than or equal to 600s;

[0028] The pressure relief and component removal stage: when the steering knuckle has completed solidification, it is necessary to close the inflation valve and open the air holes in the crucible. At this time, the aluminum alloy liquid in the riser will flow back to the crucible from top to bottom along the inner wall of the pouring system. When the gas pressure drops to 0, the component removal begins, that is, after the steering knuckle has completed solidification, the pressure is removed to open the mold and remove the component. Therefore, the pressure relief pressure is 0MPa, and the pressure relief time is greater than or equal to 1.5s.

[0029] Preferably, in step S6, the pouring temperature ranges from 660 to 710°C, and the mold preheating temperature ranges from 260 to 310°C.

[0030] Preferably, in step S7, the upper die and the lower die in the mold are made of H13 hot working die steel, and the remaining materials are made of 45 steel.

[0031] Preferably, in step S7, the size of the mold needs to take into account the size of the cavity and the size of the core. Since the steering knuckle is a solid casting, the core is not considered for design. The calculation formula of the cavity size is as follows:

[0032] L = L0(1+δ);

[0033] Where, L is the casting cavity size, in mm; L0 is the casting nominal size, in mm; δ is the casting alloy shrinkage coefficient;

[0034] δ=k(ε-η·T)

[0035] Wherein, k is the hindered shrinkage coefficient, k range is less than or equal to 1; ε is the linear shrinkage rate of the metal liquid; η is the linear expansion coefficient of the metal mold material; T is the preheating temperature of the metal mold, unit is ℃.

[0036] Preferably, in step S7, the draft angle is an angle of 2° perpendicular to the parting surface direction, and the draft direction is the same as the demoulding direction.

[0037] Preferably, in step S7, the cooling system is a water cooling system, the water pipeline is set at 15 mm away from the casting, and a ring pipeline with a diameter of 12 mm is laid. Since the cooling capacity of one water channel is limited and the position of the isolated liquid phase area is large, 4 water cooling pipelines are used, and the interval between adjacent water cooling pipelines is 12 mm.

[0038] Preferably, in step S7, the interior of the metal mold is basically sealed, but during the filling process of the aluminum alloy molten metal, there will be residual gas in the runner and the cavity. If the gas is not successfully removed, the residual gas will form a back pressure that hinders the filling of the molten metal as the cavity space continues to decrease and the temperature continues to rise. Therefore, the exhaust system is designed as a triangular exhaust groove with a depth of 1.2 mm and an angle of 60 degrees.

[0039] Compared with the prior art, the present invention has the following beneficial effects:

[0040] The present invention adopts low-pressure casting and bottom pouring method to produce the steering knuckle, optimizes the cross-sectional ratio of the corresponding position of the steering knuckle, combines the pouring system and the casting's own data, accurately determines the liquid rising pressure, filling pressure, boost pressure, holding pressure and holding time, pressure relief pressure and pressure relief time in each stage of low-pressure casting, and completes the entire low-pressure casting process of the steering knuckle when each stage is successfully completed. By controlling the pressure and time in each stage, the energy consumption is reduced, and low-cost manufacturing is achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0041] Figure 1 The present invention is a flowchart of a low-pressure casting method for a low-cost thick-wall steering knuckle. DETAILED DESCRIPTION

[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the implementation regulations described are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] Example

[0044] Reference Figure 1 -shown: A low-pressure casting method for a low-cost thick-walled steering knuckle, comprising the following steps:

[0045] Step 1: Steering knuckle process analysis: Use 3D software to model steering knuckles of different sizes

[0046] Step 2: gating system design: Use a bottom pouring system to perform low-pressure casting on the steering knuckle, which includes the design of the inner runner, the cross runner and the riser pipe. Use the three-dimensional model of the steering knuckle to establish a gating system model.

[0047] Specifically, in the low-pressure casting process, the ingates of the pouring system play the role of introducing molten metal and compensating the shrinkage of the casting during solidification. The cross-sectional area of ​​the ingates is usually calculated using the "thermal pitch circle method". The theoretical value is preliminarily calculated, and the formula is as follows:

[0048]

[0049] Where A is the cross-sectional area of ​​the ingrate, in cm2; G is the mass of the casting, in g; ρ is the density of the molten metal, in g / cm3; V is the linear velocity of the ingrate, in cm / s;

[0050] Then make numerical corrections based on actual pouring experience, the formula is as follows;

[0051]

[0052] t is the filling time, unit is s; h is the height of the metal mold cavity, unit is cm; v0 is the liquid rising speed, unit is cm / s;

[0053] When v≤15cm / s, the metal liquid level fills the mold cavity smoothly without turbulence. At the same time, the liquid rising speed is selected according to the wall thickness of the casting. The range of v0 is 1-6cm / s. For castings with thicker walls, the liquid rising speed takes a larger value.

[0054] When filling the mold, the riser pipe guides the molten metal in the crucible into the pouring system, which mainly plays the role of drainage and shrinkage compensation. When designing the riser pipe, the molten metal should have a stable liquid level during the filling process, and it is also necessary to meet the requirements of molten metal heat transfer, degassing, and slag filtering. In order to prevent oxide inclusions in the crucible from entering the casting cavity through the riser pipe, the lower end of the riser pipe is required to be 50 to 100 mm away from the molten metal level in the crucible; at the same time, considering the convenience of cleaning, the inner diameter of the riser pipe is required to be greater than 35 mm;

[0055] Step 3: Analysis of mathematical model of numerical simulation in casting process: During the low-pressure casting filling and solidification process, the casting involves the transmission of energy of aluminum alloy liquid and the contraction of aluminum alloy liquid. Its flow in the mold cavity follows the law of conservation of mass, momentum and energy. Based on this, a mathematical model is established to prepare for the subsequent numerical simulation analysis and defect prediction.

[0056] Step 4: Calculation of initial pouring parameters: The low-pressure casting process includes the liquid raising stage, the pressurization stage, the pressure holding stage and the pressure relief and part removal stage. The liquid raising pressure, filling pressure, pressurization pressure, pressure holding pressure and pressure holding time, pressure relief pressure and pressure relief time are determined during the process;

[0057] Specifically, the liquid rising stage: before the filling begins, all exhaust holes in the crucible are closed, and then dry gas is filled into the crucible. The gas pressure inside the crucible is continuously increased, so that the metal liquid surface starts to fill the mold from bottom to top through the liquid rising pipe, and the gas pressure is continuously increased until the metal liquid fills the entire pouring system, that is, the metal liquid rises in the pouring system, and the range of the liquid rising pressure is greater than or equal to 0.004MPa;

[0058] The filling stage: under the liquid pressure, the metal liquid level is now located at the inner gate, and the pressure continues to increase. The metal liquid level begins to rise slowly until it reaches the top of the steering knuckle. At this time, the aluminum alloy metal liquid will fill the entire cavity of the steering knuckle. The filling pressure range is 0.017-0.026MPa;

[0059] The pressurization stage: in order to make the casting more compact, after the molten metal fills the entire cavity, continue to apply pressure to the crucible, so that the filled casting begins to solidify and cool under relatively high pressure. In the pressurization stage, the molten metal begins to solidify, and the casting shrinks during the solidification process. Continuing to increase the pressure will make the shrinking casting compensated by new molten metal, that is, the aluminum alloy molten metal fills the entire cavity and begins to cool under pressure. The pressurization pressure range is 0.027-0.042MPa;

[0060] The holding stage: after the pressurization stage, the boost pressure needs to be maintained for a period of time in this stage. The unsolidified casting is cooled and solidified under the action of the holding pressure and the holding time to become a formed casting. At this time, the holding pressure is the same as the boost pressure, that is, the aluminum alloy molten metal solidifies and cools in this stage, and the holding pressure range is 0.027-0.042MPa; the selection of the holding time should take into account the solidification of the casting and the utilization rate of the molten metal. When the holding time is less than the solidification time of the casting, the quality of the casting in the mold cavity will be reduced; when the holding time is too long, the molten metal participating in the filling will solidify in the pouring system, and residues will appear on the inner wall of the pouring system, which requires manual cleaning later, and reduces the utilization rate of the casting molten metal, so the holding time is greater than or equal to 600s;

[0061] The pressure relief and component removal stage: when the steering knuckle is solidified, the inflation valve needs to be closed and the air hole in the crucible needs to be opened. At this time, the aluminum alloy liquid in the riser will flow back to the crucible from top to bottom along the inner wall of the pouring system. When the gas pressure drops to 0, the component removal begins. That is, after the steering knuckle is solidified, the pressure is removed to open the mold and remove the component. Therefore, the pressure relief pressure is 0 MPa, and the pressure relief time is greater than or equal to 1.5 s.

[0062] Step 5: Optimize the pouring system structure: Optimize the size of the runner and the riser, and select the ratio of the cross-sectional area of ​​the runner to the ingates as A. 横 :A 内 =2.4:1.6;

[0063] Step 6: Optimization of casting process parameters: Taking casting quality and casting efficiency as the goal, the pouring temperature and mold preheating temperature are optimized, wherein the pouring temperature range is 660-710 degrees Celsius, and the mold preheating temperature is 260-310 degrees Celsius;

[0064] Step 7: Casting mold design: determine the material, size, draft angle, cooling system and exhaust system of the metal mold;

[0065] The upper and lower molds in the mold are made of H13 hot working die steel, and the remaining materials are made of 45 steel;

[0066] The size of the mold needs to take into account the cavity size and the core size. Since the steering knuckle is a solid casting, the core is not considered for design. The cavity size calculation formula is as follows:

[0067] L = L0(1+δ);

[0068] Where, L is the casting cavity size, in mm; L0 is the casting nominal size, in mm; δ is the casting alloy shrinkage coefficient;

[0069] δ=k(ε-η·T)

[0070] Where, k is the hindered shrinkage coefficient, and the range of k is less than or equal to 1; ε is the linear shrinkage rate of the metal liquid; η is the linear expansion coefficient of the metal mold material; T is the preheating temperature of the metal mold, unit ℃;

[0071] The draft angle is 2° perpendicular to the parting surface, and the draft direction is the same as the demoulding direction;

[0072] The cooling system is a water cooling system. The water pipeline is set at 15 mm away from the casting. A circular pipeline with a diameter of 12 mm is laid. Since the cooling capacity of one water pipeline is limited and the position of the isolated liquid phase area is large, four water cooling pipelines are used, and the interval between adjacent water cooling pipelines is 12 mm.

[0073] The inside of the metal mold is basically sealed, but during the filling process of the aluminum alloy molten metal, there will be residual gas in the runner and the cavity. If these gases are not successfully removed, the residual gas will form a counter pressure that hinders the filling of the molten metal as the cavity space continues to decrease and the temperature continues to rise. Therefore, the exhaust system is designed as a triangular exhaust groove with a depth of 1.2mm and an angle of 60 degrees;

[0074] Step 8: Using the above steps, the steering knuckle is cast by low pressure casting.

[0075] Although the present invention has been described in detail with reference to the aforementioned embodiments, it is still possible for those skilled in the art to modify the technical solutions described in the aforementioned embodiments, or to make equivalent substitutions for some of the technical features therein. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A low-pressure casting method for a low-cost thick-walled steering knuckle, characterized in that: The following steps are involved: S1. Steering knuckle process analysis: Use 3D software to model steering knuckles of different sizes; S2. Casting system design: The steering knuckle is cast at low pressure using a bottom pouring system, which includes the design of the inner runner, the cross runner, and the riser pipe. The gating system model is established using the steering knuckle 3D model. The cross-sectional area of ​​the ingates is usually calculated using the "thermal pitch circle method". The theoretical value is preliminarily calculated using the following formula: Where A is the cross-sectional area of ​​the ingrate, in cm2; G is the mass of the casting, in g; ρ is the density of the molten metal, in g / cm3; V is the linear velocity of the ingrate, in cm / s; Then make numerical corrections based on actual pouring experience, the formula is as follows; t is the filling time, unit is s; h is the height of the metal mold cavity, unit is cm; v0 is the liquid rising speed, unit is cm / s; When v≤15cm / s, the metal liquid level fills the mold cavity smoothly without turbulence. At the same time, the liquid rising speed is selected according to the wall thickness of the casting. The range of v0 is 1-6cm / s. For castings with thicker walls, the liquid rising speed takes a larger value. The lower opening of the liquid riser is 50 to 100 mm away from the metal liquid surface in the crucible; considering the convenience of cleaning, the inner diameter of the liquid riser should be greater than 35 mm; S3. Mathematical model analysis of numerical simulation in casting process: Establish mathematical model of the process to prepare for subsequent numerical simulation analysis and defect prediction; S4. Calculation of initial pouring parameters: The low-pressure casting process includes a liquid raising stage, a pressurization stage, a pressure holding stage, and a pressure relief and piece removal stage. The liquid raising pressure, filling pressure, pressurization pressure, pressure holding pressure and pressure holding time, and pressure relief pressure and pressure relief time are determined during the process. The liquid rising stage: that is, the molten metal rises in the pouring system, and the range of the liquid rising pressure is greater than or equal to 0.004MPa; The filling stage: at this time, the aluminum alloy molten metal will fill the entire cavity of the steering knuckle, and the filling pressure range is 0.017-0.026MPa; The pressurization stage: the aluminum alloy molten metal fills the entire cavity and begins to cool under pressure. The pressurization pressure range is 0.027-0.042MPa; The holding stage: the aluminum alloy liquid solidifies and cools in this stage, the holding pressure range is 0.027-0.042MPa; the holding time is greater than or equal to 600s; The pressure relief and component removal stage: after the steering knuckle is solidified, the pressure is removed to open the mold and remove the component, the pressure relief pressure is 0 MPa, and the pressure relief time is greater than or equal to 1.5 s; S5. Optimization of pouring system structure: Optimize the size of the runner and riser, and select the ratio of the cross-sectional area of ​​the runner to the inner gate as A. 横 :A 内 =2.4:1.6; S6. Casting process parameter optimization: Optimize the pouring temperature and mold preheating temperature; S7. Casting mold design: determine the material, size, draft angle, cooling system and exhaust system of the metal mold; The size of the mold needs to take into account the cavity size and the core size. Since the steering knuckle is a solid casting, the core is not considered for design. The cavity size calculation formula is as follows: L = L0(1+δ); Where, L is the casting cavity size, in mm; L0 is the casting nominal size, in mm; δ is the casting alloy shrinkage coefficient; δ=k(ε-η·T) Where, k is the hindered shrinkage coefficient, and the range of k is less than or equal to 1; ε is the linear shrinkage rate of the metal liquid; η is the linear expansion coefficient of the metal mold material; T is the preheating temperature of the metal mold, unit ℃; S8. Using the above steps, a steering knuckle is obtained by low-pressure casting.

2. A low-cost, thick-walled steering knuckle low-pressure casting method according to claim 1, characterized in that: In step S3, the flow of aluminum alloy liquid in the mold cavity follows the law of conservation of mass, the law of conservation of momentum and the law of conservation of energy, and a mathematical model is established accordingly.

3. The low-pressure casting method of a low-cost thick-walled steering knuckle according to claim 1, characterized in that: In step S6, the pouring temperature ranges from 660 to 710°C, and the mold preheating temperature ranges from 260 to 310°C.

4. A low-cost, thick-walled steering knuckle low-pressure casting method according to claim 3, characterized in that: In step S7, the upper die and the lower die in the die are made of H13 hot working die steel, and the remaining materials are made of 45 steel.

5. The low-pressure casting method of a low-cost thick-walled steering knuckle according to claim 1, characterized in that: In the step S7, the draft angle is an angle of 2° perpendicular to the parting surface direction, and the draft direction is the same as the demoulding direction.

6. The low-pressure casting method for a low-cost thick-walled steering knuckle according to claim 1, characterized in that: In step S7, the cooling system is a water cooling system, the water pipe is located 15 mm away from the casting, a circular pipe with a diameter of 12 mm is laid, 4 water cooling pipes are used, and the interval between adjacent water cooling pipes is 12 mm.

7. A low-cost, thick-walled steering knuckle low-pressure casting method according to claim 1, characterized in that: In step S7, the exhaust system is designed as a triangular exhaust groove with a depth of 1.2 mm and an angle of 60 degrees.

Citation Information

Patent Citations

  • Low-pressure casting process and mould for aluminium alloy steering knuckle

    CN102699312A

  • Low-pressure casting process of aluminum alloy steering joint

    CN104741574A

  • Method for maintaining pressures and then quickly boosting pressures for metal low-pressure casting molding of aluminum alloy automobile chassis castings

    CN105598418A

  • Low-pressure casting technology for aluminum alloy hubs

    CN106086546A

  • Knuckle for automobile and manufacturing method thereof

    JP2006007802A