A conductive silver paste for filling holes in ceramic packaging and a preparation method thereof
By using conductive silver paste with a specific proportion of nanomaterials and dispersants in ceramic packaging, the problem of poor dispersion effect of conductive silver paste is solved, and better printing effect and conductive performance are achieved.
Patent Information
- Application Number
- CN202410924346.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-11
- Publication Date
- 2024-11-08
- Estimated Expiration
- 2044-07-11
AI Technical Summary
The existing conductive silver paste has poor dispersion effect in ceramic packaging, resulting in poor filling or voiding problems, affecting the printing effect.
85%~91% silver particles, 3%~6% nanomaterial additives (including Al2O3, SiO2, Bi2O3, SrCaO3), 0.2~0.5% dispersant (BYK-111 or BYK-104), 3%~ 10% of the first carrier and 0.5~0.8% of the additive are premixed, stirred and dispersed through specific proportions and process flows to avoid nano agglomeration and improve dispersion effect and uniformity.
It significantly improves the dispersion effect and uniformity, improves the hole filling effect during the printing process, avoids the problems of incomplete filling or void light leakage, and improves the conductivity.
Smart Images

Figure CN118486498B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a via-filling conductive silver paste, in particular to a via-filling conductive silver paste applied to ceramic packaging, and further to a preparation method of the via-filling conductive silver paste applied to ceramic packaging. Background Art
[0002] Conductive silver paste is an industrial coating material and a type of conductive paste, while conductive paste is a type of electronic paste. Conductive paste contains a variety of conductive substances, such as precious metal silver powder, silver-coated copper powder, base metal copper powder, nickel (Ni) powder, aluminum powder, tungsten, molybdenum, manganese and conductive inorganic powders such as carbon powder, graphene, etc. Conductive silver paste is a conductive paste with different silver contents, and its conductive properties are mainly achieved by silver powder. Paste refers to "paste", which usually refers to a blend of carrier bonding phase, additives and auxiliary agents, which plays a role in load-bearing and enhancing the conductive material. The functions of conductive silver paste are, first, conductivity, and second, bonding and adhesion.
[0003] In the prior art, conductive silver paste usually includes inorganic additives such as calcium carbonate (CaCO3). In this prior art, due to the inclusion of raw materials such as calcium carbonate (CaCO3), the mixed slurry has problems such as poor dispersion and unevenness. As a result, in the actual printing process, it may cause problems such as incomplete filling or light leakage in the voids, resulting in poor printing / filling effects. Summary of the invention
[0004] The technical problem to be solved by the present invention is to provide a conductive silver paste for hole filling used in ceramic packaging and a preparation method thereof. By improving the composition of the conductive silver paste for hole filling and the preparation method thereof, the dispersion effect is made better and more uniform, so as to improve the printing effect, avoid the problems of incomplete filling or light leakage in the voids in the prior art, and effectively improve the hole filling effect of the printing process.
[0005] To this end, the present invention provides a conductive silver paste for hole filling used in ceramic packaging, comprising: 85% to 91% of silver particles, 3% to 6% of a nano material additive, 0.2% to 0.5% of a dispersant, 3% to 10% of a first carrier, 0.5% to 0.8% of an auxiliary agent and 1.5% to 3.5% of a solvent; the nano material additive comprises Al2O3, SiO2, Bi2O3 and SrCaO3, and the dispersant adopts BYK-111 dispersant or BYK-104 dispersant.
[0006] A further improvement of the present invention is that the weight ratio of Al2O3, SiO2, Bi2O3 and SrCaO3 is 13:8:7:3.
[0007] A further improvement of the present invention is that the auxiliary agent includes a silane coupling agent and / or an aluminate coupling agent.
[0008] A further improvement of the present invention is that the first carrier is a mixed carrier of resin and alcohol, the weight ratio of the resin and alcohol is 1:2~6; or a mixed carrier of resin and ether is used, the weight ratio of the resin and ether is 1:2~5.5; the solvent is alcohol and / or ether.
[0009] The present invention also provides a method for preparing a via-filling conductive silver paste, which is used to prepare the via-filling conductive silver paste applied to ceramic packaging as described above, and comprises the following steps:
[0010] Step S1, premixing the nano material additive, dispersant, first carrier, auxiliary agent and solvent in proportion to prepare a second carrier;
[0011] Step S2, detecting whether the fineness and viscosity of the second carrier meet the requirements, if yes, jumping to step S3; if not, stirring after heating or cooling, and returning after stirring to re-detect whether the fineness and viscosity of the second carrier meet the requirements;
[0012] Step S3, adding the silver particles to the stirred second carrier in proportion, and stirring and mixing again at a first preset temperature;
[0013] Step S4, taking out the slurry after the stirring in step S3, and dispersing it through a grinding device at a second preset temperature;
[0014] Step S5, filtering the dispersed slurry using a filter screen with a preset mesh size to obtain a conductive silver paste for hole filling.
[0015] A further improvement of the present invention is that step S2 includes the following sub-steps:
[0016] Step S201: when the fineness of the second carrier is not greater than 6 μm and the viscosity of the second carrier is 60-200 PaS, it is judged to meet the requirements and jump to step S3; if it does not meet the requirements, jump to step S202;
[0017] Step S202, judging whether the viscosity of the second carrier is greater than 200 PaS, if so, stirring is performed after temperature control, and after stirring is completed, returning to the step S201 for another judgment; if not, jumping to step S203;
[0018] Step S203, judging whether the viscosity of the second carrier is less than 60 PaS, if so, stirring is performed after the temperature is lowered, and after the stirring is completed, the process returns to the step S201 for another judgment; if not, the process jumps to step S204;
[0019] Step S204, determine whether the fineness of the second carrier is not greater than 6 μm, if so, jump to step S3; if not, maintain the current temperature and continue stirring until the fineness of the second carrier is not greater than 6 μm, then jump to step S3.
[0020] A further improvement of the present invention is that in step S202 and step S203, the temperature adjustment range of the temperature increase control and the temperature decrease control is 5-10°C / time, and after each temperature increase control or temperature decrease control, the stirring speed is controlled to 60-200 r / min, and the stirring time is 12-16 min.
[0021] A further improvement of the present invention is that in step S3, the silver particles are added to the stirred second carrier in proportion, and the mixture is stirred and mixed again at 65-70° C., the stirring speed is controlled at 60-180 r / min, and the stirring time is 25-30 min.
[0022] A further improvement of the present invention is that in step S4, the slurry after stirring in step S3 is taken out and dispersed by a grinding device at 30-55° C. until the dispersion fineness of the slurry is controlled to be no more than 4 μm and the viscosity of the slurry is controlled to be in the range of 800-1200 Kcps.
[0023] A further improvement of the present invention is that in step S4, the operating environment pressure of the dispersion treatment is controlled within a range of 1.05-1.08 MPa.
[0024] Compared with the prior art, the beneficial effects of the present invention are: nanomaterial additives including Al2O3, SiO2, Bi2O3 and SrCaO3 are used, and CaCO3 is no longer needed; and in order to further deal with the problem of nano-agglomeration that may occur in the preparation process of the nanomaterial additives, dispersants are added in a targeted manner, and the percentages between the various components and their preparation methods are optimized, thereby effectively improving the dispersion effect and uniformity, making the printing effect better, effectively avoiding the problems of incomplete filling or light leakage in the prior art, and efficiently improving the hole filling effect in the printing process. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] Figure 1 It is a schematic diagram of the working process of an embodiment of the present invention. DETAILED DESCRIPTION
[0026] The preferred embodiments of the present invention will be further described in detail below in conjunction with the accompanying drawings.
[0027] like Figure 1As shown, this embodiment provides a conductive silver paste for hole filling applied to ceramic packaging, including: 85% to 91% of silver particles, 3% to 6% of nano material additives, 0.2% to 0.5% of dispersant, 3% to 10% of a first carrier, 0.5% to 0.8% of an auxiliary agent and 1.5% to 3.5% of a solvent; the nano material additive includes Al2O3, SiO2, Bi2O3 and SrCaO3, the weight ratio of Al2O3, SiO2, Bi2O3 and SrCaO3 is 13:8:7:3, and the dispersant is BYK-111 dispersant or BYK-104 dispersant.
[0028] In order to overcome the problem of poor dispersion and uneven dispersion in the prior art using raw materials such as calcium carbonate (CaCO3), the present application adds nanomaterial additives including Al2O3, SiO2, Bi2O3 and SrCaO3, without the need for raw materials such as CaCO3; the nanomaterial additive is preferably obtained by chemical preparation, such as chemical liquid phase precipitation; however, in the preparation process using the nanomaterial additive, the problem of nano-agglomeration may occur, which affects the actual preparation effect, because the present embodiment also specifically adds 0.2~0.5% dispersant, and the dispersant is Use BYK-111 dispersant or BYK-104 dispersant. BYK-111 dispersant is also called BYK111 wetting dispersant. It is a non-ionic dispersant with excellent dispersing performance and stability. It can effectively disperse particles and prevent their center aggregation. BYK-104 dispersant, also called BYK104 wetting dispersant, is used for medium-polar to high-polarity solvent-based coatings. By adding 0.2~0.5% of BYK-111 dispersant or BYK-104 dispersant, a stable and reliable dispersion effect can be achieved to further promote the dispersion effect and uniformity of the preparation of the conductive silver paste for filling holes.
[0029] It is worth noting that, since the present embodiment no longer uses the raw material CaCO3, but replaces it with nano-material additives such as Al2O3, SiO2, Bi2O3 and SrCaO3, the weight ratio between the corresponding components is also very important. The effect that can be achieved by different proportions of the components is not a linear reaction and cannot be obtained through a limited number of conventional experiments; more specifically, the weight ratio of Al2O3, SiO2, Bi2O3 and SrCaO3 in the present embodiment is 13:8:7:3, and the dispersant uses BYK-111 dispersant or BYK-104 dispersant, which can not only better play the role of the nano-material additive, but also be more conducive to subsequent dispersion processing, so as to improve the corresponding conductive properties of the conductive silver paste for filling holes.
[0030] The silver particles described in this embodiment preferably use silver powder of 2~4μm to better meet the actual application requirements. The auxiliary agent includes a silane coupling agent and / or an aluminate coupling agent. The solvent uses alcohols and / or ethers. In this embodiment, the first carrier uses a mixed carrier of resin and alcohols, and the weight ratio of the resin and alcohols is 1:2~6, that is, 1 part of resin corresponds to 2~6 parts of alcohol; or a mixed carrier of resin and ethers is used, and the weight ratio of the resin and ethers is 1:2~5.5, that is, 1 part of resin corresponds to 2~5.5 parts of ethers; the resin includes phenolic resin and / or polyvinyl chloride resin, etc.
[0031] This embodiment also provides a method for preparing a via-filling conductive silver paste, which is used to prepare the via-filling conductive silver paste applied to ceramic packaging as described above, and includes the following steps:
[0032] Step S1, premixing the nano material additive, dispersant, first carrier, auxiliary agent and solvent in proportion to prepare a second carrier;
[0033] Step S2, detecting whether the fineness and viscosity of the second carrier meet the requirements, if yes, jumping to step S3; if not, stirring after heating or cooling, and returning after stirring to re-detect whether the fineness and viscosity of the second carrier meet the requirements;
[0034] Step S3, adding the silver particles to the stirred second carrier in proportion, and stirring and mixing again at a first preset temperature;
[0035] Step S4, taking out the slurry after the stirring in step S3, and dispersing it through a grinding device at a second preset temperature;
[0036] Step S5, filtering the dispersed slurry with a preset mesh size to obtain the conductive silver paste for filling holes. The preset mesh size can be set and adjusted according to actual conditions, and preferably, a filter with a mesh size of 325 or 400 is used to filter the dispersed slurry.
[0037] Different from the prior art, the present application first premixes the raw materials except the silver particles and modulates them into a second carrier, so as to better play the auxiliary role of the dispersant, improve the carrier basis for the subsequent dispersion treatment, and avoid the drawback that the fineness and viscosity cannot meet the actual requirements due to stirring all the materials together at the beginning. On this basis, it is further tested whether the fineness and viscosity of the second carrier meet the requirements, and then it is ensured that the silver particles are added in proportion on the basis of meeting the requirements, so as to achieve more efficient stirring and mixing, which can well avoid the problem of nano-agglomeration and facilitate the rapid and efficient acquisition of the required slurry.
[0038] Step S2 in this embodiment includes the following sub-steps:
[0039] Step S201: when the fineness of the second carrier is not greater than 6 μm, the error is controlled to be ±0.5 μm, and the viscosity of the second carrier is 60-200 PaS, it is judged to meet the requirements and jump to step S3; if it does not meet the requirements, jump to step S202;
[0040] Step S202, judging whether the viscosity of the second carrier is greater than 200 PaS, if so, stirring is performed after temperature control, and after stirring is completed, returning to the step S201 for another judgment; if not, jumping to step S203;
[0041] Step S203, judging whether the viscosity of the second carrier is less than 60 PaS, if so, stirring is performed after the temperature is lowered, and after the stirring is completed, the process returns to the step S201 for another judgment; if not, the process jumps to step S204;
[0042] Step S204, determine whether the fineness of the second carrier is not greater than 6μm, with an error control of ±0.5μm. If so, jump to step S3; if not, maintain the current temperature and continue stirring until the fineness of the second carrier is not greater than 6μm, then jump to step S3.
[0043] It is worth noting that the fineness and viscosity of the second carrier in this embodiment are related to the dispersion fineness and viscosity of the slurry after mixing the silver particles. If the fineness of the second carrier is too small, it will undoubtedly pose great difficulties and adjustments to the production process and production costs. If the fineness of the second carrier is too large, the advantage of adjusting the proportion of components other than the silver particles to the second carrier is lost, which is not conducive to reasonably controlling the dispersion fineness and viscosity of the slurry in step S4. Because, in this embodiment, for the fineness and viscosity of the second carrier, not only the upper limit needs to be reasonably set and the corresponding stirring temperature needs to be controlled, but also the lower limit needs to be reasonably set and the corresponding stirring temperature needs to be controlled.
[0044] In this embodiment, as the stirring temperature increases, the viscosity decreases; and, by reasonably controlling the temperature and stirring speed, the fineness of the second carrier can also be better controlled. Therefore, in the step S2 of this embodiment, it is first determined whether the viscosity of the second carrier meets the requirements. If not, it is determined whether the viscosity exceeds the preset upper limit of 200PaS. When it exceeds the upper limit of the viscosity, stirring is performed after temperature increase control to reduce the viscosity; when it exceeds the lower limit of the viscosity of 60PaS, stirring is performed after temperature decrease control to increase the viscosity; until the viscosity meets the requirements, it is further determined whether the fineness meets the requirements. The above judgment and control steps of this embodiment cannot be adjusted, and the parameters set therein are not set arbitrarily, but are set corresponding to the components, proportions and preparation methods adopted in this embodiment. This relationship does not belong to a linear change relationship, and it is impossible for ordinary technicians in this field to obtain the above technical solution through a limited number of experiments.
[0045] More preferably, in step S202 and step S203, the temperature adjustment range of the temperature increase control and the temperature decrease control is 5-10°C / time, and after each temperature increase control or temperature decrease control, the stirring speed is controlled to 60-200r / min, and the stirring time is 12-16min, thereby ensuring the stirring effect after the temperature increase control or the temperature decrease control, and promoting the fineness of the second carrier to meet the requirements more quickly. In step S204, the viscosity of the second carrier actually meets the requirements, so the current temperature is maintained and stirring is continued. The stirring speed is also preferably controlled to 60-200r / min, and the stirring time is preferably 12-16min, and then detection is performed; this cycle is repeated until the fineness of the second carrier is no more than 6μm, and then jumps to step S3.
[0046] In step S3 of this embodiment, the silver particles are added to the stirred second carrier in proportion, and stirred and mixed again at 65-70° C., the stirring speed is controlled to be 60-180 r / min, and the stirring time is 25-30 min to obtain a slurry with the silver particles added. In step S3, the temperature control can not only provide a more suitable basis for the subsequent dispersion fineness and viscosity of the slurry, but also cooperate with the stirring speed and stirring time to achieve efficient stirring faster.
[0047] In step S4 of this embodiment, the slurry after stirring in step S3 is taken out and dispersed by grinding equipment at 30~55°C until the dispersion fineness of the slurry is controlled to be no more than 4μm, the error is controlled to be ±0.5μm, and the viscosity of the slurry is controlled to be 800~1200Kcps. It is worth noting that since the slurry is a conductive silver paste for filling holes directly for printing, in order to ensure the conductive effect and hole filling effect during the printing process, the fineness of the slurry in this embodiment needs to be smaller than the fineness of the second carrier, and the viscosity of the slurry also needs to be higher than the viscosity of the second carrier. Therefore, it is necessary to perform a cooling operation on the original basis and maintain the grinding and dispersion treatment at an environment of 30~55°C. More preferably, the temperature can be controlled at 30~35°C, at which time the effect is optimal.
[0048] In fact, the dispersion fineness of the slurry needs to be controlled to no more than 4 μm. If conventional grinding treatment is adopted under normal pressure, the required grinding time will be relatively long, and the requirements for the grinding equipment will also be relatively high. In addition, the problem needs to be maintained during the grinding process. Therefore, not only will there be a problem of long dispersion time, but also higher costs.
[0049] In view of this problem, in the step S4 of the present embodiment, the operating environment pressure of the dispersion treatment is controlled at 1.05~1.08MPa, that is, the required dispersion treatment time is effectively shortened by appropriate supercharging, and then, appropriate supercharging can be used to be more conducive to shortening the required dispersion time and reasonably controlling the cost. It should be noted that the pressure described in the present embodiment is not the greater the better. Excessive pressure not only places high demands on the grinding equipment, but is also not conducive to actual operation. The present embodiment performs grinding by a pressure slightly greater than normal pressure, which has reasonable requirements on the equipment, and can promote the effect of the dispersion treatment by the squeezing effect of the pressure. The comparison of the dispersion treatment time before and after supercharging is shown in the following table.
[0050] Pressure environment (MPa) 1 1.05 1.06 1.07 1.08 Distributed processing time (min) 50 32 30 31 32 Dispersion fineness of slurry (μm) 3.5~4.5μm 3.5~4.5μm 3.5~4.5μm 3.5~4.5μm 3.5~4.5μm
[0051] Therefore, in summary, the present embodiment adopts nanomaterial additives including Al2O3, SiO2, Bi2O3 and SrCaO3, and there is no need to use CaCO3; and in order to further deal with the problem of nano-agglomeration that may occur in the preparation process of the nanomaterial additive, a dispersant is added in a targeted manner, and the percentage between the components and the preparation method are optimized, thereby effectively improving the dispersion effect and uniformity, making the printing effect better, effectively avoiding the problem of incomplete filling or light leakage in the prior art, and efficiently improving the hole filling effect during the printing process.
[0052] The above contents are further detailed descriptions of the present invention in combination with specific preferred embodiments, and it cannot be determined that the specific implementation of the present invention is limited to these descriptions. For ordinary technicians in the technical field to which the present invention belongs, several simple deductions or substitutions can be made without departing from the concept of the present invention, which should be regarded as falling within the protection scope of the present invention.
Claims
1. A method for preparing a conductive silver paste for hole filling, characterized in that: Used for preparing a via-filling conductive silver paste for ceramic packaging, the via-filling conductive silver paste comprises: 85% to 91% of silver particles, 3% to 6% of nanomaterial additives, 0.2% to 0.5% of a dispersant, 3% to 10% of a first carrier, 0.5% to 0.8% of an auxiliary agent, and 1.5% to 3.5% of a solvent; the nanomaterial additive comprises Al2O3, SiO2, Bi2O3, and SrCaO3, and the dispersant is BYK-111 dispersant or BYK-104 dispersant; And includes the following steps: Step S1, premixing the nano material additive, dispersant, first carrier, auxiliary agent and solvent in proportion to prepare a second carrier; Step S2, detecting whether the fineness and viscosity of the second carrier meet the requirements, if yes, jumping to step S3; if not, stirring after heating or cooling, and returning after stirring to re-detect whether the fineness and viscosity of the second carrier meet the requirements; Step S3, adding the silver particles to the stirred second carrier in proportion, and stirring and mixing again at a first preset temperature; Step S4, taking out the slurry after the stirring in step S3, and dispersing it through a grinding device at a second preset temperature; Step S5, filtering the dispersed slurry using a filter screen with a preset mesh size to obtain a conductive silver paste for hole filling; The step S2 comprises the following sub-steps: Step S201: when the fineness of the second carrier is not greater than 6 μm and the viscosity of the second carrier is 60-200 PaS, it is judged to meet the requirements and jump to step S3; if it does not meet the requirements, jump to step S202; Step S202, judging whether the viscosity of the second carrier is greater than 200 PaS, if so, stirring is performed after temperature control, and after stirring is completed, returning to the step S201 for another judgment; if not, jumping to step S203; Step S203, judging whether the viscosity of the second carrier is less than 60 PaS, if so, stirring is performed after the temperature is lowered, and after the stirring is completed, the process returns to the step S201 for another judgment; if not, the process jumps to step S204; Step S204, determine whether the fineness of the second carrier is not greater than 6 μm, if so, jump to step S3; if not, maintain the current temperature and continue stirring until the fineness of the second carrier is not greater than 6 μm, then jump to step S3.
2. The method for preparing the conductive silver paste for hole filling according to claim 1, characterized in that: The weight ratio of Al2O3, SiO2, Bi2O3 and SrCaO3 is 13:8:7:
3.
3. The method for preparing the conductive silver paste for hole filling according to claim 1, characterized in that: The auxiliary agent includes a silane coupling agent and / or an aluminate coupling agent.
4. The method for preparing a conductive silver paste for hole filling according to any one of claims 1 to 3, characterized in that: The first carrier is a mixed carrier of resin and alcohol, the weight ratio of the resin and alcohol is 1:2-6; or a mixed carrier of resin and ether is used, the weight ratio of the resin and ether is 1:2-5.5; the solvent is alcohol and / or ether.
5. The method for preparing a conductive silver paste for hole filling according to any one of claims 1 to 3, characterized in that: In step S202 and step S203, the temperature adjustment range of the temperature increase control and the temperature decrease control is 5-10°C / time, and after each temperature increase control or temperature decrease control, the stirring speed is controlled to 60-200 r / min, and the stirring time is 12-16 min.
6. The method for preparing a conductive silver paste for hole filling according to any one of claims 1 to 3, characterized in that: In the step S3, the silver particles are added to the stirred second carrier in proportion, and the mixture is stirred again at 65-70° C., with the stirring speed controlled at 60-180 r / min and the stirring time being 25-30 min.
7. The method for preparing a via-filling conductive silver paste according to any one of claims 1 to 3, characterized in that: In the step S4, the slurry after stirring in the step S3 is taken out and dispersed by a grinding device at 30-55° C. until the dispersion fineness of the slurry is controlled to be no greater than 4 μm and the viscosity of the slurry is controlled to be in the range of 800-1200 Kcps.
8. The method for preparing a via-filling conductive silver paste according to any one of claims 1 to 3, characterized in that: In step S4, the operating environment pressure of the dispersion treatment is controlled at 1.05-1.08 MPa.