A normal temperature dechlorinating agent for reforming hydrogen and hydrogen-containing synthesis gas and preparation method thereof

By using components such as zinc oxide, attapulgite and water glass binder in the normal temperature dechlorination agent, a multi-leaf grass structure is formed, which solves the problems of small surface area and low strength of the catalyst and achieves high-efficiency dechlorination and long life. effect, and supports the recycling of catalysts.

CN118491506BActive Publication Date: 2024-10-11杭州弘钰汇新材料有限公司
View PDF 17 Cites 0 Cited by

Patent Information

Application Number
CN202410955906.2
Authority / Receiving Office
CN · China
Patent Type
Patents(China)
Current Assignee / Owner
Filing Date
2024-07-17
Publication Date
2024-10-11
Estimated Expiration
2044-07-17

Smart Images

  • Figure CN118491506B_ABST
    Figure CN118491506B_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of normal temperature dechlorination agents, and is intended to provide a normal temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas and a preparation method thereof, wherein the normal temperature dechlorination agent formula comprises zinc oxide 10%-40%, attapulgite 10%-40%, light calcium carbonate 10%-30%, zinc carbonate 2%-8%, potassium carbonate 1%-8%, and water glass of 2%-5% of total weight is added to the above-mentioned mixed powder; the preparation method of the present invention comprises the processes such as liquid preparation, powder dry mixing, mixed liquid and powder wet mixing, die extrusion molding, blank curing, blank drying, blank calcination, and dechlorination agent finished product inspection packaging. The normal temperature dechlorination agent of the present invention has the characteristics of high body strength, large structural specific surface area, good dechlorination effect, green and environmentally friendly preparation process, and recyclable use, and water glass is used as a binder in the formula to increase the strength of the dechlorination agent, and repeated water washing is not pulverized, and recyclable use can be achieved, and it is widely used in the dechlorination technology field of reforming hydrogen and hydrogen-containing synthesis gas in petrochemical industry.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of normal-temperature dechlorination agents, and in particular, relates to a normal-temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas and a preparation method thereof. Background Art

[0002] In recent years, with the continuous development and application of the petroleum industry, people's demand for oil products has increased day by day, and the amount of oil production and processing has also continued to increase; with the continuous development of oil production technology, various types of oilfield chlorine-containing oil production chemical additives have emerged. The addition of such oilfield chemical additives has greatly improved the efficiency of crude oil production, but has caused an impact on the refining industry that cannot be ignored. In the process of oil refining, the organic chlorine in the oilfield chemical additives is converted into HCl after pre-hydrogenation. HCl will flow into the pipelines and equipment of the subsequent system with the regenerated gas, causing corrosion to the pipelines or equipment, or polluting the atmosphere after being vented; in addition, if the downstream process raw materials contain ammonia NH3, ammonium chloride will be generated, causing equipment blockage and frequent fouling at the inlet of the circulating compressor, affecting the normal operation of the device and causing great economic losses to the enterprise.

[0003] At present, room temperature dechlorination agents usually use alkali metal oxides such as aluminum oxide, calcium oxide, zinc oxide, and copper oxide as active components, add a certain amount of carboxymethyl cellulose or field sesbania powder as a pore-forming agent, and are formed into strips or block structures through an extrusion process. After forming, they are roasted at 350°C to obtain a dechlorination agent with a relatively good dechlorination effect under room temperature conditions. By consulting domestic and foreign literature, it is found that there are many introductions to room temperature dechlorination agent products and their preparation methods. For example, patent application number "CN201610831490" introduces a new type of high-efficiency dechlorination agent and its preparation method, which uses 20% to 75% active ingredients, 1% to 10% porosity additives, 5% to 70% carriers, and 5% to 25% synergistic additives. The active components are one or more of CaO, Na2CO3, MgO, CuO, and ZnO. The carriers are all cheap, easy to obtain, and have a high specific surface area. At the same time, they have good compatibility, have a good dechlorination effect, and the catalyst does not mud or powder. For example, patent application number "CN2013100951604" discloses a room temperature dechlorination agent, which is mainly made of ferrous sulfate, calcium oxide and attapulgite clay, wherein ferrous sulfate is 20-30 parts by weight, CaO is 20-40 parts by weight, and attapulgite clay is 10-25 parts by weight; the room temperature dechlorination agent also includes 15-25 parts by weight of catalyst waste agent, and the active components of the catalyst waste agent are copper oxide and zinc oxide; the present invention does not require a roasting process, reduces energy consumption, reduces the equipment used in the preparation process, simplifies the preparation steps, and reduces the preparation cost. For another example, patent application number "CN2021100684970" introduces a room temperature gas phase dechlorination agent and a preparation method thereof. By adopting a formula combination of transition metal oxides, light metal oxides, molecular sieves and supporting carriers, the room temperature gas phase dechlorination agent has a high utilization efficiency of active components, is suitable for removing acidic hydrogen chloride impurities in hydrocarbon materials at room temperature, and has a high chlorine capacity and removal accuracy. However, the room temperature dechlorination agent recorded in the literature and currently produced is mainly in a strip structure, because it is simple and easy to shape, and has high strength after shaping, but the surface area for catalytic contact is small, and the specific surface area utilization rate is low, which affects the catalytic dechlorination effect. Although CN107876005B, CN115888804A and other documents record spherical and clover-shaped structures, the specific formation and cross-section are not given in the documents. In addition, due to the complexity of the clover-shaped molding mold, the strength of the blank after molding is often too low to meet the use requirements, resulting in the existing public technology being only in the theoretical speculation stage; in addition, the ingredients in the components usually use organic binders such as CMC and PVA as plasticizers, resulting in low product strength after high-temperature sintering, easy to crush during use, and short service life. Even if there is no pulverization during use, the catalyst carrier after dechlorination cannot be washed and reused.

[0004] In view of this, a room-temperature dechlorination agent with a special structure is studied, which is suitable for the use environment of reforming hydrogen and hydrogen-containing synthesis gas. The specific surface area is increased on the basis of the strip structure, thereby improving the dechlorination effect of the catalyst, which has broad market prospects. In addition, the introduction of a new high-temperature binder will be beneficial to improving the strength of the dechlorination agent, avoiding pulverization, and realizing recycling after washing and drying. Summary of the invention

[0005] The purpose of the present invention is to overcome the deficiencies in the prior art and provide a room-temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas and a preparation method thereof, which has the characteristics of high body strength, large structural specific surface area, good dechlorination effect, green and environmentally friendly preparation process, and recyclability, and can be widely used in the technical field of dechlorination of reforming hydrogen and hydrogen-containing synthesis gas in petrochemical industry.

[0006] In order to solve the above problems, the present invention adopts the following technical scheme: a room temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas, which is composed of the following components in weight percentage: 10%-40% zinc oxide, 10%-40% attapulgite, 10%-30% light calcium carbonate, 2%-8% zinc carbonate, and 1%-8% potassium carbonate; 2%-5% of water glass in total weight is added to the above mixed powder;

[0007] As an improvement of the present invention, the zinc oxide, attapulgite and light calcium carbonate are all micron-grade powders, and the 325-mesh standard sieve residue is less than 5%.

[0008] As an improvement of the present invention, the water glass is a sodium silicate aqueous solution diluted with water, the amount of water added is 3 to 5 times the weight of the water glass, and the concentration of the diluted water glass is 15% to 35%.

[0009] The present invention also provides a method for preparing the above-mentioned room-temperature dechlorinating agent for reformed hydrogen and hydrogen-containing synthesis gas, which specifically comprises the following steps:

[0010] (1) Liquid preparation: Evenly add the weighed water glass and water into a container equipped with a stirring device, and stir for a specified time to fully mix the water glass and water to obtain a mixed liquid;

[0011] (2) Dry mixing of powders: Weigh zinc oxide, attapulgite, light calcium carbonate, zinc carbonate and potassium carbonate in proportion, add the above raw materials into a mixer and mix and stir until all components are fully mixed and uniformly obtained to obtain dry powder materials;

[0012] (3) Wet mixing of the mixed liquid and powder: Put the mixed dry powder material into a mixer and press, add the mixed liquid in a specified proportion at a uniform speed, and mix and grind for 20 to 40 minutes to make the material have sufficient strength and plasticity to obtain a clay material that meets the molding requirements;

[0013] (4) Extrusion molding: The mixed and ground clay is formed by an extruder. The extruder is equipped with a multi-leaf steel mold. The clay is pressed from top to bottom. At the same time, the extrusion pressure is ≥8Mpa to obtain a cylindrical blank with a smooth and uniform multi-leaf cross-section structure. The outer diameter of the blank is φ4mm and the length is 10~12mm.

[0014] (5) Blank curing: Place the blank in a dust-free, enclosed space, maintain a temperature of 20°C to 50°C and a humidity of 45% to 75%, and let it stand for 1-3 days to allow the blank to cure;

[0015] (6) Drying of the blank: Put the solidified blank into a drying room for drying. The drying temperature in the drying room is 50-80°C and the drying time is 24-48 hours to obtain a dried dechlorination agent blank;

[0016] (7) Calcination of blanks: The dried blanks are sent to a rotary kiln via a mesh belt, and then calcined at 500-700°C at a rate of 1-3°C / min in a pusher kiln or shuttle kiln, and then naturally cooled to prepare the dechlorination agent body;

[0017] (8) Inspection and packaging: The dechlorinating agent body shall be inspected for appearance, specification, strength and chlorine capacity, and finally packaged into boxes according to weight.

[0018] As an improvement of the present invention, the stirring device in step (1) is an electromagnetic stirrer with an impeller at the bottom, and the stirring time is 2 to 15 minutes.

[0019] As an improvement of the present invention, in step (2), zinc carbonate, potassium carbonate and light calcium carbonate are first mixed, and then zinc oxide and attapulgite are added and mixed to ensure that the mixing is uniform and sufficient.

[0020] As an improvement of the present invention, the proportion of the mixed liquid added in step (3) is 10% to 25% of the weight of the dry powder material.

[0021] As an improvement of the present invention, the multi-leaf clover steel mold in step (4) is one of three-leaf clover, four-leaf clover or five-leaf clover, and the multi-leaf clover steel mold structure is cylindrical, with 6 to 10 three-leaf clover hollow mold cavities, four-leaf clover hollow mold cavities or five-leaf clover hollow mold cavities evenly distributed inside, and chamfers are provided on the upper and lower end surfaces.

[0022] As an improvement of the present invention, the moisture content of the carrier blank in step (6) is ≤1.5%.

[0023] As an improvement of the present invention, the dechlorinating agent body in step (7) is in the form of a long column, and its horizontal cross section is in the form of a multi-leaf grass structure.

[0024] As an improvement of the present invention, the surface of the dechlorinating agent body is provided with grooves 2, and the grooves 2 are evenly distributed in the vertical direction, and the horizontal section of the dechlorinating agent body is one of three-leaf clover, four-leaf clover or five-leaf clover.

[0025] As an improvement of the present invention, in step (7), the dechlorination agent body has a diameter of φ3-φ8 mm and a length of 4-15 mm.

[0026] The invention has the following beneficial effects: a room-temperature dechlorinating agent for reforming hydrogen and hydrogen-containing synthesis gas and a preparation method thereof, which has the characteristics of high structural specific surface area, good dechlorination effect, high strength, green and environmentally friendly preparation process, recyclability, etc. By adopting low-cost alkaline zinc carbonate, potassium carbonate and light calcium carbonate as active additives, and adding water glass (also alkaline) as an inorganic binder in the formula, the mud material has plasticity, the water glass has high green body support strength after room-temperature solidification, and has higher strength after high-temperature roasting, so that the dechlorinating agent with multi-leaf grass structure can meet the use strength requirements, and is not easy to pulverize under repeated high temperatures. The dechlorinating agent can be recycled after washing with water, which greatly prolongs the service life of the dechlorinating agent. The service life of the dechlorinating agent can reach 1 to 3 years, which is more than 5 times longer than the service life of 2 to 3 months of ordinary dechlorinating agents; on this basis, the specific surface area of ​​the multi-leaf grass structure dechlorinating agent is increased, the gas-solid contact area of ​​the dechlorinating agent is increased, and the dechlorinating agent has better effect; on the other hand, abundant sodium ions are introduced by water glass, so that the catalytic activity is further improved.

[0027] In addition, the formula of the present invention adopts low-cost attapulgite as a stable layered framework, while providing the viscosity of the material itself. Compared with the use of active porous activated alumina, it has lower cost and more stable performance. In the atmosphere of hydrogen and hydrogen-containing synthesis gas, alumina will bring side reactions to the system; the pore-enlarging agent and the active component are all carbonate materials, and the carbonate is calcined and decomposed at 500-700°C to obtain alkali metal oxides, which can both form pores and increase the chlorine capacity of the dechlorination agent, achieving a dual-functional effect. The decomposition product is carbon dioxide, and it will not cause environmental pollution. The decomposition efficiency of commonly used hydrochloric acid or nitric acid metal compounds is low, and nitrogen oxides will be produced after decomposition to pollute the atmosphere.

[0028] The preparation method of the invention comprises the following processes: liquid preparation, dry mixing of powders, wet mixing of mixed liquid and powders, extrusion molding by molds, blank solidification, blank drying, blank calcination, inspection and packaging of finished dechlorinating agents, etc. The method comprises the following steps: firstly mixing zinc carbonate, potassium carbonate and light calcium carbonate, and then adding zinc oxide and attapulgite for mixing, thereby ensuring uniform and sufficient mixing and high activity of active components; 6 to 10 cavities are evenly distributed in the multi-leaf clover steel mold, thereby improving molding efficiency; and compared with the dechlorinating agent of the entire cylinder, the multi-leaf clover structure dechlorinating agent uses more economical materials, with a material saving of 5% to 10%, thereby reducing material costs. BRIEF DESCRIPTION OF THE DRAWINGS

[0029] Figure 1 : A schematic diagram of the structure of a normal temperature dechlorinating agent for reforming hydrogen and hydrogen-containing synthesis gas of the present invention;

[0030] Figure 2 : The process flow chart of the preparation process of the normal temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas of the present invention;

[0031] Figure 3 : A schematic structural diagram of a multi-leaf steel mold clover for producing a normal temperature dechlorinating agent for reforming hydrogen and hydrogen-containing synthesis gas according to the present invention;

[0032] Figure 4 : The front view of the multi-leaf steel mold three-leaf clover for the production of normal temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas of the present invention;

[0033] Figure 5 : The front view of the multi-leaf steel mold four-leaf clover for the production of room temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas of the present invention;

[0034] Figure 6 : The front view of the multi-leaf steel mold five-leaf clover used in the production of room-temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas of the present invention.

[0035] In the figure: 1. dechlorinating agent body; 2. groove; 3. multi-leaf clover steel mold; 4. three-leaf clover hollow mold cavity; 5. four-leaf clover hollow mold cavity; 6. five-leaf clover hollow mold cavity. DETAILED DESCRIPTION

[0036] In order to better understand the above technical solution of the present invention, the technical solution of the present invention is further described below in conjunction with embodiments.

[0037] like Figure 1 As shown, the room-temperature dechlorinating agent for reforming hydrogen and hydrogen-containing synthesis gas of the present invention comprises a dechlorinating agent body 1, which is in a long columnar structure and has a multi-leaf grass structure in horizontal section; grooves 2 are provided on the surface of the dechlorinating agent body 1, and the grooves 2 are evenly distributed in the vertical direction; the components of the dechlorinating agent body 1 include 10%-40% zinc oxide, 10%-40% attapulgite, 10%~30% light calcium carbonate, 2%-8% zinc carbonate, and 1%-8% potassium carbonate; and 2~5% water glass of the total weight of solid powder is added to the components of the dechlorinating agent body 1 as a binder, and the water glass provides high-temperature strength to the dechlorinating agent body 1, ensuring that the multi-leaf grass structure can have the same strength as the cylindrical structure to meet the use requirements.

[0038] Furthermore, the zinc oxide, attapulgite and light calcium carbonate are all micron-sized powders, and the 325-mesh standard sieve residue is less than 5%. The micron-sized powders have a smoother surface and are more densely bonded.

[0039] Furthermore, the water glass is a sodium silicate aqueous solution diluted with water, the amount of water added is 3 to 5 times the weight of the water glass, and the concentration of the diluted water glass is 15% to 35%.

[0040] Furthermore, the horizontal section of the dechlorinating agent body 1 is one of three-leaf clover, four-leaf clover or five-leaf clover, thereby further increasing the specific surface contact area; specifically, the diameter of the dechlorinating agent body is φ3~φ8mm, preferably φ4mm, and the length is 4~15mm, preferably 12mm.

[0041] like Figure 2 As shown, the present invention also provides a method for preparing the above-mentioned room-temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas, which adopts a preparation process of first wet mixing and dry mixing to prepare a solution and a powder, and then mixing and grinding them together, specifically comprising the following steps:

[0042] (1) Liquid preparation: Evenly add the weighed water glass and water into a container equipped with a stirring device, and stir for a specified time to fully mix the water glass and water to obtain a mixed liquid;

[0043] (2) Dry mixing of powders: Weigh zinc oxide, attapulgite, light calcium carbonate, zinc carbonate and potassium carbonate in proportion, add the above raw materials into a mixer and mix and stir until all components are fully mixed and uniformly obtained to obtain dry powder materials;

[0044] (3) Wet mixing of the mixed liquid and powder: Put the mixed dry powder material into a mixer and press, add the mixed liquid in a specified proportion at a uniform speed, and mix and grind for 20 to 40 minutes to make the material have sufficient strength and plasticity to obtain a clay material that meets the molding requirements;

[0045] (4) Extrusion molding: The mixed and ground clay is formed by an extruder. The extruder is equipped with a multi-leaf steel mold. The clay is pressed from top to bottom. At the same time, the extrusion pressure is ≥8Mpa to obtain a cylindrical blank with a smooth and uniform multi-leaf cross-section structure. The outer diameter of the blank is φ4mm and the length is 10~12mm.

[0046] (5) Blank curing: Place the blank in a dust-free, enclosed space, maintain a temperature of 20°C to 50°C and a humidity of 45% to 75%, and let it stand for 1-3 days to allow the blank to cure;

[0047] (6) Drying of the blank: Put the solidified blank into a drying room for drying. The drying temperature in the drying room is 50-80°C and the drying time is 24-48 hours to obtain a dried dechlorination agent blank;

[0048] (7) Calcination of blanks: The dried blanks are sent to a rotary kiln via a mesh belt, and are calcined at a temperature of 1-3°C / min to 500-700°C in a pusher kiln or shuttle kiln, and then naturally cooled to prepare the dechlorination agent body 1;

[0049] (8) Inspection and packaging: The dechlorinating agent body 1 is inspected for appearance, specification, strength and chlorine capacity, and finally packaged into boxes according to weight.

[0050] Furthermore, in step (1), the stirring device is an electromagnetic stirrer with an impeller at the bottom, and the stirring time is 2 to 15 minutes.

[0051] Furthermore, the amount of each component added in step (2) is: 10%-40% zinc oxide, 10%-40% attapulgite, 10%-30% light calcium carbonate, 2%-8% zinc carbonate, and 1%-8% potassium carbonate.

[0052] Furthermore, in the step (2), zinc carbonate, potassium carbonate and light calcium carbonate are first mixed, and then zinc oxide and attapulgite are added and mixed to ensure that the mixing is uniform and sufficient.

[0053] Furthermore, in step (3), the mixed liquid is added in a proportion of 10-25% of the weight of the dry powder material.

[0054] Furthermore, if Figures 3 to 6 As shown, in the step (4), the multi-leaf clover steel mold 3 is one of three-leaf clover, four-leaf clover or five-leaf clover, the multi-leaf clover steel mold 3 is cylindrical in structure, and 6 to 10 three-leaf clover hollow mold cavities 4, four-leaf clover hollow mold cavities 5 or five-leaf clover hollow mold cavities 6 are evenly distributed inside, and the upper and lower end surfaces of the multi-leaf clover steel mold 3 are provided with chamfers 7.

[0055] Furthermore, in the step (6), the moisture content of the carrier blank is ≤1.5%.

[0056] The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas and the preparation method thereof are further introduced below with reference to specific examples. Embodiment 1

[0057] The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas in this embodiment is prepared by the following steps:

[0058] (1) Liquid preparation: Weigh 2 kg of 50% water glass and 10 kg of water, add them into an electromagnetic stirrer with an impeller at the bottom and stir for 2 minutes to fully mix the water glass and water to obtain a mixed liquid;

[0059] (2) Dry mixing of powders: Weigh 40 kg of zinc oxide, 40 kg of attapulgite, 10 kg of light calcium carbonate, 8 kg of zinc carbonate, and 2 kg of potassium carbonate, totaling 100 kg. First, mix the weighed zinc carbonate, potassium carbonate, and light calcium carbonate, then add zinc oxide and attapulgite for secondary mixing, so that all components are fully mixed to obtain dry powder materials, and use a forced mixer for mixing;

[0060] (3) Wet mixing of the mixed liquid and powder: Take out all the mixed dry powder materials mentioned above and put them into a mixer and press, add 12 kg of the prepared mixed liquid at a uniform speed, and mix and grind for 20 minutes to make the materials reach sufficient strength and plasticity to obtain a clay material that meets the molding requirements;

[0061] (4) Extrusion molding: The mixed and ground clay material is formed by an extruder. The extruder is provided with a multi-leaf clover steel mold with 4 hollow clover mold cavities. The multi-leaf clover steel mold is provided with 7 hollow clover mold cavities 4. The clay material is pressed from top to bottom. At the same time, the extrusion pressure is 20 MPa. Seven blanks can be obtained by one extrusion. The blanks are cut by an automatic cutting machine to obtain a cylindrical blank with a smooth and uniform clover cross-section structure. The outer diameter of the blank is 4 mm and the length is 12 mm.

[0062] (5) Blank curing: Place the blank in a dust-free, enclosed space, maintain a temperature of 25°C and a humidity of 65%, and let it stand for 1 day to allow the blank to cure;

[0063] (6) Drying of blanks: Place the solidified blanks in a drying room for drying. The drying temperature in the drying room is 50°C and the drying time is 48 hours to obtain a dechlorination agent blank with a moisture content of ≤0.5%;

[0064] (7) Calcination of blanks: The dried blanks are sent to a rotary kiln via a mesh belt, and are calcined in a push plate kiln at a temperature of 1°C / min to 500°C, and then naturally cooled to prepare a dechlorination agent body 1;

[0065] (8) Inspection and packaging: The dechlorinating agent body 1 is inspected for appearance, specification, strength and chlorine capacity, and finally packaged into boxes according to weight.

[0066] The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas prepared by the above steps, after relevant tests, has no obvious decrease in strength compared with the ordinary round bar dechlorination agent, and the radial crushing resistance of the dechlorination agent reaches 76N / cm, while the ordinary round bar is 78N / cm, indicating that after the multi-leaf clover steel mold with a special cylindrical solid structure design is formed, although the structural curvature increases, it does not greatly affect the strength of the dechlorination agent, as shown in Table 1; this is mainly due to the use of water glass as a binder in the present invention, so that the clover structure dechlorination agent has the use strength requirements. It is also concluded from the test that the room temperature dechlorination agent of the clover structure has better dechlorination and purification effects than the room temperature dechlorination agent of the ordinary round bar, with a chlorine capacity of 28.6% and a purification degree of 0.2ppm, while the chlorine capacity of the ordinary round bar is 25.9% and the purification degree is 0.5ppm, which confirms that the clover structure with a large contact area can improve the chlorine capacity and purification degree, as shown in Table 2. In addition, as the use temperature increases, the chlorine capacity of the clover structure room temperature dechlorination agent prepared in this embodiment is continuously improved, and can reach 34.9% at 250°C, as shown in Table 3. In addition, due to the use of water glass binder, the dechlorination agent has higher high temperature strength, significantly extended service life, up to more than 1 year, and can also be recycled, as shown in Table 4; and the ordinary organic binder formula and the water glass binder formula of this application are compared as shown in Table 5. The ordinary binder formula uses CMC, and the addition amount is 0.5~1.5%, so that the mixed mud has a certain plasticity, and the blank has a certain strength after drying, but the strength performance after roasting is low, and the radial crushing force of the clover structure is only 60N / cm, which cannot meet the strength requirements of production and use, and is prone to fracture and powdering; while the radial crushing force of the four-leaf clover using water glass as a binder is 87N / cm, which can meet the requirements of production and use, as shown in Table 6. Embodiment 2

[0067] The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas in this embodiment is prepared by the following steps:

[0068] (1) Liquid preparation: Weigh 3 kg of water glass with a concentration of 40% and 12 kg of water, add them into an electromagnetic stirrer with an impeller at the bottom and stir for 8 minutes to fully mix the water glass and water to obtain a mixed liquid;

[0069] (2) Dry mixing of powders: Weigh 30 kg of zinc oxide, 30 kg of attapulgite, 30 kg of light calcium carbonate, 2 kg of zinc carbonate, and 8 kg of potassium carbonate, totaling 100 kg. First, mix the weighed zinc carbonate, potassium carbonate, and light calcium carbonate, then add zinc oxide and attapulgite for secondary mixing, so that all components are fully mixed to obtain dry powder materials, and use a forced mixer for mixing;

[0070] (3) Wet mixing of the mixed liquid and powder: Take out all the mixed dry powder materials mentioned above and put them into a mixer and press, add 15 kg of the prepared mixed liquid at a uniform speed, and mix and grind for 30 minutes to make the materials reach sufficient strength and plasticity to obtain a mud material that meets the molding requirements;

[0071] (4) Extrusion molding: The mixed and ground clay material is formed by an extruder. The extruder is provided with a multi-leaf clover steel mold with a four-leaf clover hollow mold cavity 5. Seven four-leaf clover hollow mold cavities 4 are arranged inside the multi-leaf clover steel mold. The clay material is pressed from top to bottom. At the same time, the extrusion pressure is 15 MPa. Seven blanks can be obtained by one extrusion. The blanks are cut by an automatic cutting machine to obtain a cylindrical blank with a smooth and uniform four-leaf clover cross-section structure. The outer diameter of the blank is 5 mm and the length is 15 mm.

[0072] (5) Blank curing: Place the blank in a dust-free, enclosed space, maintain a temperature of 35°C and a humidity of 55%, and let it stand for 2 days to allow the blank to cure;

[0073] (6) Drying of blanks: Place the solidified blanks in a drying room for drying. The drying temperature in the drying room is 60°C and the drying time is 36 hours to obtain a dechlorination agent blank with a moisture content of ≤0.2%;

[0074] (7) Calcination of blanks: The dried blanks are sent to a rotary kiln via a mesh belt, and then calcined in a pusher kiln at a temperature of 1.2°C / min to 600°C, and then naturally cooled to prepare the dechlorination agent body;

[0075] (8) Inspection and packaging: The dechlorinating agent body shall be inspected for appearance, specification, strength and chlorine capacity, and finally packaged into boxes according to weight.

[0076] The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas prepared by the four-leaf clover structure in the above steps has no obvious decrease in strength compared with the ordinary round bar dechlorination agent after relevant tests. The radial crushing resistance of the dechlorination agent reaches 75.5N / cm, while the ordinary round bar is 78N / cm, indicating that after the multi-leaf clover steel mold with a special structure design of a cylindrical solid is formed, although the structural curvature increases, it does not greatly affect the strength of the dechlorination agent, as shown in Table 1; this is mainly due to the fact that the present invention uses water glass as a binder, so that the four-leaf clover structure dechlorination agent has the use strength requirements. It is also concluded from the test that the room temperature dechlorination agent of the four-leaf clover structure has better dechlorination and purification effects than the room temperature dechlorination agents of ordinary round bars and three-leaf clover structures, with a chlorine capacity of 29.5% and a purification degree of 0.2ppm, while the ordinary round bar chlorine capacity is 25.9% and a purification degree of 0.5ppm, which confirms that the four-leaf clover structure with a large contact area can improve the chlorine capacity and purification degree, and is better than the three-leaf clover structure, as shown in Table 2. In addition, as the use temperature increases, the chlorine capacity of the four-leaf clover structure room temperature dechlorination agent prepared in this embodiment is continuously improved, and can reach 36.5% at 250°C, as shown in Table 3. In addition, due to the use of water glass binder, the dechlorination agent has higher high temperature strength, significantly extended service life, up to 9-10 months, and can also be recycled, as shown in Table 4; and the ordinary organic binder formula and the water glass binder formula of this application are compared as shown in Table 5. The ordinary binder formula uses CMC, and the addition amount is 0.5~1.5%, so that the mixed mud has a certain plasticity, and the blank has a certain strength after drying, but the strength performance after roasting is low, and the radial crushing force of the four-leaf clover structure is only 63N / cm, which cannot meet the strength requirements of production and use, and is prone to fracture and powdering; while the radial crushing force of the four-leaf clover using water glass as a binder is 85N / cm, which can meet the requirements of production and use, as shown in Table 6. Embodiment 3

[0077] The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas in this embodiment is prepared by the following steps:

[0078] (1) Liquid preparation: Weigh 5 kg of 30% water glass and 16 kg of water, add them into an electromagnetic stirrer with an impeller at the bottom and stir for 15 min to fully mix the water glass and water to obtain a mixed liquid;

[0079] (2) Dry mixing of powders: Weigh 35 kg of zinc oxide, 40 kg of attapulgite, 20 kg of light calcium carbonate, 4 kg of zinc carbonate, and 1 kg of potassium carbonate, totaling 100 kg. First, mix the weighed zinc carbonate, potassium carbonate, and light calcium carbonate, then add zinc oxide and attapulgite for secondary mixing, so that all components are fully mixed to obtain dry powder materials, and use a forced mixer for mixing;

[0080] (3) Wet mixing of the mixed liquid and powder: Take out all the mixed dry powder materials mentioned above and put them into a mixer and press, add 21 kg of the prepared mixed liquid at a uniform speed, and mix and grind for 40 minutes to make the materials reach sufficient strength and plasticity to obtain a clay material that meets the molding requirements;

[0081] (4) Extrusion molding: The mixed and ground clay material is formed by an extruder. The extruder is provided with a multi-leaf clover steel mold with 6 hollow clover mold cavities. The multi-leaf clover steel mold is provided with 7 hollow clover mold cavities 6. The clay material is pressed from top to bottom. At the same time, the extrusion pressure is 8 MPa. Seven blanks can be obtained by one extrusion. The blanks are cut by an automatic cutting machine to obtain a cylindrical blank with a smooth and uniform cross-sectional structure of a five-leaf clover. The outer diameter of the blank is 6 mm and the length is 10 mm.

[0082] (5) Blank curing: Place the blank in a dust-free, enclosed space, maintain a temperature of 35°C and a humidity of 45%, and let it stand for 3 days to allow the blank to cure;

[0083] (6) Drying of blanks: Place the solidified blanks in a drying room for drying. The drying temperature in the drying room is 75°C and the drying time is 24 hours to obtain a dechlorination agent blank with a moisture content of ≤0.1%;

[0084] (7) Calcination of blanks: The dried blanks are sent to a rotary kiln via a mesh belt, and then calcined in a pusher kiln at a temperature of 1.5°C / min to 700°C, and then naturally cooled to prepare the dechlorination agent body;

[0085] (8) Inspection and packaging: The dechlorinating agent body shall be inspected for appearance, specification, strength and chlorine capacity, and finally packaged into boxes according to weight.

[0086] The room temperature dechlorinating agent for reformed hydrogen and hydrogen-containing synthesis gas prepared in the five-leaf clover structure in the above steps has no obvious decrease in strength compared with the ordinary round bar dechlorinating agent after relevant tests. The radial crushing resistance of the dechlorinating agent reaches 75.1N / cm, while that of the ordinary round bar is 78N / cm, indicating that after being formed by the multi-leaf clover steel mold with a special cylindrical solid structure design, although the structural curvature increases, it does not greatly affect the strength of the dechlorinating agent, as shown in Table 1 for details; this is mainly due to the fact that the present invention uses water glass as a binder, so that the five-leaf clover structure dechlorinating agent has the strength requirements for use. The test also showed that the room-temperature dechlorinator with a five-leaf clover structure had better dechlorination and purification effects than the room-temperature dechlorinators with ordinary round bars, three-leaf clover, and four-leaf clover structures, with a chlorine capacity of 31.9% and a purification degree of 0.1ppm, while the chlorine capacity of ordinary round bars was 25.9% and the purification degree was 0.5ppm, which confirmed that the five-leaf clover structure with a large contact area can improve the chlorine capacity and purification degree, and has better effects than the three-leaf clover and four-leaf clover structures, as shown in Table 2. In addition, with the increase of the use temperature, the chlorine capacity of the room-temperature dechlorinator with a five-leaf clover structure prepared in this embodiment is continuously improved, and can reach 38.6% at 250°C, as shown in Table 3. In addition, due to the use of water glass binder, the high-temperature strength of the dechlorination agent is higher, the service life is significantly extended to 9-10 months, and it can be recycled, as shown in Table 4 for details; and the comparison between the common organic binder formula and the water glass binder formula of the present application is shown in Table 5. The common binder formula uses CMC with an addition amount of 0.5-1.5%, so that the mixed mud has a certain plasticity and ensures that the green body has a certain strength after drying, but the strength performance after roasting is low, and the radial crushing force of the five-leaf clover structure is only 60N / cm, which cannot meet the strength requirements of production and use, and is prone to fracture and pulverization; while the radial crushing force of the four-leaf clover using water glass as a binder is 83.5N / cm, which can meet the requirements of production and use, as shown in Table 6 for details.

[0087]

[0088] Finally, it should be noted that those skilled in the art should recognize that the above embodiments are only used to illustrate the present invention and are not intended to limit the present invention. As long as they are within the spirit of the present invention, any changes or modifications to the above embodiments will fall within the scope of the claims of the present invention.

Claims

1. A room temperature dechlorination agent for reforming hydrogen and hydrogen-containing synthesis gas, It is characterized in that The room temperature dechlorination agent is composed of the following components in weight percentage: 10%-40% zinc oxide, 10%-40% attapulgite, 10%-30% light calcium carbonate, 2%-8% zinc carbonate, and 1%-8% potassium carbonate; 2%-5% of water glass is added to the above mixed powder; The method for preparing the normal temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas comprises the following steps: (1) Liquid preparation: Evenly add the weighed water glass and water into a container equipped with a stirring device, and stir for a specified time to fully mix the water glass and water to obtain a mixed liquid; (2) Dry mixing of powders: Weigh zinc oxide, attapulgite, light calcium carbonate, zinc carbonate, and potassium carbonate in proportion, add the above raw materials into a mixer in order, and mix and stir to ensure that the components are fully mixed and uniformly obtained to obtain a dry powder material; (3) Wet mixing of the mixed liquid and powder: Put the mixed dry powder material into a mixer and press, add the mixed liquid at a ratio of 10% to 25% of the weight of the dry powder material at a uniform speed, and mix and grind for 20 to 40 minutes to make the material have sufficient strength and plasticity to obtain a clay material that meets the molding requirements; (4) Extrusion molding: The mixed and ground clay is formed by an extruder. The extruder is equipped with a multi-leaf steel mold. The clay is pressed from top to bottom. At the same time, the extrusion pressure is ≥8Mpa to obtain a cylindrical blank with a smooth and uniform multi-leaf cross-section structure. The outer diameter of the blank is φ4mm and the length is 10~12mm. (5) Blank curing: Place the blank in a dust-free, enclosed space, maintain a temperature of 20°C to 50°C and a humidity of 45% to 75%, and let it stand for 1-3 days to allow the blank to cure; (6) Drying of the blank: Put the solidified blank into a drying room for drying. The drying temperature in the drying room is 50-80°C and the drying time is 24-48 hours to obtain a dried dechlorination agent blank; (7) Calcination of blanks: The dried blanks are conveyed to a rotary kiln via a mesh belt, and calcined at a temperature of 1-3°C / min to 500-700°C in a pusher kiln or shuttle kiln, and then naturally cooled to prepare the dechlorination agent body (1); (8) Inspection and packaging: The dechlorinating agent body (1) is inspected for appearance, specification, strength and chlorine capacity, and finally packaged into boxes according to weight.

2. The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas according to claim 1, It is characterized in that The zinc oxide, attapulgite and light calcium carbonate are all of micro powder grade, and the residue on the 325-mesh standard sieve is less than 5%.

3. The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas according to claim 1, It is characterized in that The stirring device in step (1) is an electromagnetic stirrer with an impeller at the bottom, and the stirring time is 2 to 15 minutes.

4. The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas according to claim 1, It is characterized in that In the step (2), zinc carbonate, potassium carbonate and light calcium carbonate are first mixed, and then zinc oxide and attapulgite are added and mixed to ensure that the mixture is uniform and sufficient.

5. The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas according to claim 1, It is characterized in that In the step (4), the multi-leaf clover steel mold (3) is one of a three-leaf clover, a four-leaf clover or a five-leaf clover. The multi-leaf clover steel mold (3) is cylindrical in structure, with 6 to 10 three-leaf clover hollow mold cavities (4), four-leaf clover hollow mold cavities (5) or five-leaf clover hollow mold cavities (6) evenly distributed inside, and chamfers (7) are provided on the upper and lower end surfaces.

6. The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas according to claim 1, It is characterized in that The moisture content of the carrier blank in the step (6) is ≤1.5%.

7. The room temperature dechlorination agent for reformed hydrogen and hydrogen-containing synthesis gas according to claim 1, It is characterized in that In the step (7), the dechlorinating agent body (1) has a long columnar structure, and a horizontal cross-section has a multi-leaf grass structure; the surface of the dechlorinating agent body (1) is provided with grooves (2), and the grooves (2) are evenly distributed in the vertical direction.

8. The method for preparing the room temperature dechlorinating agent according to any one of claims 1 to 7, It is characterized in that The following steps are involved: (1) Liquid preparation: Evenly add the weighed water glass and water into a container equipped with a stirring device, and stir for a specified time to fully mix the water glass and water to obtain a mixed liquid; (2) Dry mixing of powders: Weigh zinc oxide, attapulgite, light calcium carbonate, zinc carbonate, and potassium carbonate in proportion, add the above raw materials into a mixer in order, and mix and stir to ensure that the components are fully mixed and uniformly obtained to obtain a dry powder material; (3) Wet mixing of the mixed liquid and powder: Put the mixed dry powder material into a mixer and press, add the mixed liquid at a ratio of 10% to 25% of the weight of the dry powder material at a uniform speed, and mix and grind for 20 to 40 minutes to make the material have sufficient strength and plasticity to obtain a clay material that meets the molding requirements; (4) Extrusion molding: The mixed and ground clay is formed by an extruder. The extruder is equipped with a multi-leaf steel mold. The clay is pressed from top to bottom. At the same time, the extrusion pressure is ≥8Mpa to obtain a cylindrical blank with a smooth and uniform multi-leaf cross-section structure. The outer diameter of the blank is φ4mm and the length is 10~12mm. (5) Blank curing: Place the blank in a dust-free, enclosed space, maintain a temperature of 20°C to 50°C and a humidity of 45% to 75%, and let it stand for 1-3 days to allow the blank to cure; (6) Drying of the blank: Put the solidified blank into a drying room for drying. The drying temperature in the drying room is 50-80°C and the drying time is 24-48 hours to obtain a dried dechlorination agent blank; (7) Calcination of blanks: The dried blanks are conveyed to a rotary kiln via a mesh belt, and calcined at a temperature of 1-3°C / min to 500-700°C in a pusher kiln or shuttle kiln, and then naturally cooled to prepare the dechlorination agent body (1); (8) Inspection and packaging: The dechlorinating agent body (1) is inspected for appearance, specification, strength and chlorine capacity, and finally packaged into boxes according to weight.

9. The preparation method according to claim 8, It is characterized in that The zinc oxide, attapulgite and light calcium carbonate are all of micro powder grade, and the residue on the 325-mesh standard sieve is less than 5%.

10. The preparation method according to claim 8, It is characterized in that The stirring device in step (1) is an electromagnetic stirrer with an impeller at the bottom, and the stirring time is 2 to 15 minutes.

11. The preparation method according to claim 8, It is characterized in that In the step (2), zinc carbonate, potassium carbonate and light calcium carbonate are first mixed, and then zinc oxide and attapulgite are added and mixed to ensure that the mixture is uniform and sufficient.

12. The preparation method according to claim 8, It is characterized in that In the step (4), the multi-leaf clover steel mold (3) is one of a three-leaf clover, a four-leaf clover or a five-leaf clover. The multi-leaf clover steel mold (3) is cylindrical in structure, with 6 to 10 three-leaf clover hollow mold cavities (4), four-leaf clover hollow mold cavities (5) or five-leaf clover hollow mold cavities (6) evenly distributed inside, and chamfers (7) are provided on the upper and lower end surfaces.

13. The preparation method according to claim 8, It is characterized in that The moisture content of the carrier blank in the step (6) is ≤1.5%.

14. The preparation method according to claim 8, It is characterized in that In the step (7), the dechlorinating agent body (1) has a long columnar structure, and a horizontal cross-section has a multi-leaf grass structure; the surface of the dechlorinating agent body (1) is provided with grooves (2), and the grooves (2) are evenly distributed in the vertical direction.

Citation Information

Patent Citations

  • An adsorbent for removing chlorinated pollutants, its preparation method and application

    CN107876005B

  • Dechlorinating agent and preparation method thereof

    CN115888804A

  • Desulfurizing agent and preparation method thereof

    CN101485954A

  • Normal-temperature dechlorinating agent

    CN103127903A

  • Dechlorination agent and preparation method thereof

    CN103386244A