TPU material for antibacterial and anti-skid pads on offshore decks and preparation method thereof
Through the one-step method, TPU material is synthesized and modified 9Al2O3•B2O3 whiskers are used to solve the problem of insufficient bacteria resistance, anti-slip and corrosion resistance performance of TPU material in marine environments, and the performance improvement and stability guarantee of the material are achieved.
Patent Information
- Application Number
- CN202410953885.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-17
- Publication Date
- 2024-11-12
- Estimated Expiration
- 2044-07-17
AI Technical Summary
The existing TPU materials exhibit insufficient bacteria, slip and corrosion resistance in harsh marine environments, and other performance problems are reduced by enhancing one performance.
TPU materials were synthesized by one-step method using hydrolysis-resistant polyether polyol and octafluoro-1,6-hexanediol chain extender, and double modification of γ-glycidyl ether oxypropyl trimethoxysilane and white carbon black 9Al2O3•B2O3 whiskers are treated with a regular structure, strong polarity, hydrogen bonds and F-C bonds, enhancing the material's wear resistance and antibacterial properties.
It significantly improves the anti-slip, wear, bacteria and corrosion resistance of TPU materials, while maintaining the synthetic activity and dispersion properties, ensuring the stability and performance of the materials in the marine environment.
Smart Images

Figure SMS_18 
Figure SMS_1 
Figure SMS_2
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of TPU materials, and in particular relates to a TPU material for a bacteria-resistant and anti-slip mat for a marine deck and a preparation method thereof. Background Art
[0002] At present, the anti-skid materials used in the sea are mainly divided into two parts: polymer organic coating and inorganic metal coating. The functions of anti-skid mats in different areas such as ship decks, arresting cables, gangways, personnel activity areas, equipment storage areas, etc. are different. On ship decks, gangways, offshore operation areas, precision equipment placement areas, etc., a high friction factor is required to prevent skids and wear, so as to reduce casualties and equipment damage. Due to the particularity of the marine environment, in addition to the anti-skid properties that should be possessed, the anti-skid coating must also have antibacterial, wear-resistant and corrosion-resistant protective effects.
[0003] Thermoplastic polyurethane elastomer TPU material has mechanical properties such as high modulus and high mechanical properties, as well as certain wear resistance, weather resistance and good processing performance. It is widely used in many fields such as electronic components, mobile phone cases, casters, shoes, automobiles, aerospace, sports parts, etc. However, if it is used in harsh conditions such as the ocean, some of its properties such as corrosion resistance, wear resistance, anti-slip, and bacteria resistance are insufficient, and the performance of TPU materials needs to be further enhanced to meet the requirements.
[0004] At present, the main way to enhance TPU is to adjust the synthetic raw materials and add inorganic fillers to improve the material's anti-skid, wear-resistant and antibacterial properties. China's invention patent publication number CN117447675A discloses a high thermal conductivity and low dielectric constant TPU for electronic packaging and its preparation method. By using perfluorocarbon chain extenders, modified nano MnO 2 , fluorinated graphene, and prepared TPU materials with high thermal conductivity and low dielectric constant. China Invention Patent Publication No. CN104193949A discloses a nano antibacterial material and its preparation method, which greatly improves the antibacterial properties of TPU materials by adding modified inorganic nano antibacterial agents and adding them to polyurethane prepolymers.
[0005] However, in the existing research including the above-mentioned patent, there is a problem of inappropriate selection of raw materials for the reinforcement of TPU composite materials, which enhances one property and reduces other properties, and the use of large molecular weight chain extenders obviously reduces the activity during synthesis, and the addition of modified fillers causes uneven dispersion and performance degradation. Therefore, it is necessary to select suitable synthetic raw materials and modified enhanced TPU to cope with the harsh marine environment and improve the properties such as bacteria resistance, anti-skid, wear resistance, and corrosion resistance. Summary of the invention
[0006] In order to solve the above technical problems, the present invention provides a TPU material for a marine deck antibacterial anti-skid mat, which enhances the anti-skid, wear-resistant, antibacterial and corrosion-resistant properties of the TPU material. The present invention also provides a preparation method.
[0007] The TPU material for the antibacterial and anti-slip mat for offshore decks of the present invention is prepared from the following raw materials in percentage by mass:
[0008] Polyether polyol 52.42%-76.95%,
[0009] Diisocyanate 10.93%-26.7%,
[0010] Diol chain extender 3.72%-14.48%,
[0011] Modified 9Al 2 O 3 •B 2 O 3 Whiskers 6%-10%,
[0012] Antioxidant 0.1%-0.3%,
[0013] Catalyst 0.1%-0.3%;
[0014] Among them, modified 9Al 2 O 3 •B 2 O 3 The whiskers are prepared by modification of γ-glycidyloxypropyltrimethoxysilane and white carbon black.
[0015] Preferably, the polyether polyol is polyethylene glycol, polypropylene glycol or polytetramethylene glycol, more preferably polytetramethylene glycol, and has a number average molecular weight of 1000-2000.
[0016] Preferably, the diisocyanate is 4,4'-diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate or xylylene diisocyanate, more preferably 4,4'-diphenylmethane diisocyanate.
[0017] Preferably, the diol chain extender is octafluoro-1,6-hexanediol.
[0018] Preferably, the antioxidant is antioxidant 1010, antioxidant 1024 or antioxidant 1076.
[0019] Preferably, the catalyst is one of the organic bismuth catalyst DY-20, the organic tin catalyst T-9, and tetra-tert-butyl titanate.
[0020] Preferably, modified 9Al 2 O 3 •B 2 O 3The preparation of whiskers includes the following steps:
[0021] a. Adjust the pH of the hydrolyzate of γ-glycidyloxypropyltrimethoxysilane to 8-9 to prepare the pretreatment solution C;
[0022] b. Place 10%-20% white carbon black by mass in a container with distilled water, and heat it by ultrasonic vibration to keep the temperature at 70-80°C to obtain a white carbon black suspension as the pretreatment liquid D;
[0023] c. 9Al 2 O 3 •B 2 O 3 The whiskers were added to the pretreatment solution C, and the temperature was maintained at 70-80°C by ultrasonic vibration heating, stirred for 2-4 hours, filtered and dried to obtain 9Al modified with γ-glycidyloxypropyltrimethoxysilane. 2 O 3 •B 2 O 3 Whiskers;
[0024] d. 9Al modified with γ-glycidyloxypropyltrimethoxysilane 2 O 3 •B 2 O 3 The whiskers were added to the pretreatment solution D, and the temperature was maintained at 50-60°C by ultrasonic vibration heating, stirred for 2-4 hours, filtered and dried to obtain modified 9Al modified twice by γ-glycidyloxypropyltrimethoxysilane and white carbon black. 2 O 3 •B 2 O 3 Whiskers.
[0025] Preferably, 9Al 2 O 3 •B 2 O 3 Whiskers and 9Al modified with γ-glycidyloxypropyltrimethoxysilane 2 O 3 •B 2 O 3 The amounts of the whiskers added in step c and step d are 35% and 40% of the mass fraction of the pretreatment liquid C and the pretreatment liquid D, respectively.
[0026] The method for preparing the TPU material for the antibacterial and anti-slip mat for marine decks of the present invention comprises the following steps:
[0027] (1) Dehydrate the polyether polyol under vacuum at 100-120°C for 2-3 hours, then add antioxidant and modified 9Al 2 O 3 •B2 O 3 Whiskers and catalysts are stirred evenly to obtain a mixed solution A, which is placed in an oven at 100-120°C for later use;
[0028] (2) heating and melting the diol chain extender at 75-95° C. to obtain a molten liquid B;
[0029] (3) Pour the mixed liquid A and the molten liquid B into a reaction container and stir evenly. Then add the diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place it in an oven at 100-120°C and mature for 6-8 hours to obtain the product.
[0030] Compared with the prior art, the present invention has the following beneficial effects:
[0031] 1. The present invention synthesizes TPU by a one-step method, uses a polyether diol with stronger hydrolysis resistance, does not use a conventional small molecule alcohol chain extender, and introduces an octafluoro-1,6-hexanediol chain extender, so that the synthesized TPU material introduces a structurally regular F element, which enhances the polarity of TPU, makes the soft and hard segment microphase separation more obvious, and makes the crystallinity stronger, thereby improving the mechanical properties; at the same time, the F element has a very strong antibacterial effect, prevents the intervention of foreign bacteria and microorganisms, and enhances the antibacterial and corrosion resistance of the material;
[0032] 2. The present invention modifies 9Al 2 O 3 •B 2 O 3 The whiskers are added to the TPU material system and are double modified by γ-glycidyloxypropyltrimethoxysilane and white carbon black, so that the modified Si-OH, Si-O-Si and other components are arranged tightly and evenly, and are more fully and effectively dispersed in TPU. At the same time, they form extremely strong hydrogen bonds with TPU, synergistically acting on the FC bonds introduced in TPU, and reacting with 9Al 2 O 3 •B 2 O 3 The whiskers' wear and corrosion resistance work together to form an interlaced network structure, which enhances the anti-slip, wear-resistant, bacteria-resistant and corrosion-resistant properties;
[0033] 3. The preparation method of the present invention is simple and convenient to operate, and is scientific and reasonable. DETAILED DESCRIPTION
[0034] The technical solution of the present invention will be clearly and completely described below in conjunction with embodiments.
[0035] Unless otherwise specified, all raw materials used in the examples are commercially available.
[0036] Example 1
[0037] The TPU material for the antibacterial and anti-slip mat of the offshore deck is prepared from the following raw materials in percentage by mass:
[0038] Polytetramethylene glycol 52.42%,
[0039] 4,4'-diphenylmethane diisocyanate 26.7%,
[0040] Octafluoro-1,6-hexanediol 14.48%,
[0041] Modified 9Al 2 O 3 •B 2 O 3 Whisker 6%,
[0042] Antioxidant 1010 0.1%,
[0043] Organic bismuth catalyst DY-20 0.3%,
[0044] The number average molecular weight of the polytetramethylene glycol is 1000;
[0045] The modified 9Al 2 O 3 •B 2 O 3 The preparation of whiskers includes the following steps:
[0046] a. Adjust the pH of the hydrolyzate of γ-glycidyloxypropyltrimethoxysilane to 8 to prepare the pretreatment solution C;
[0047] b. Place 10% white carbon black by mass in a container with distilled water, and heat it by ultrasonic vibration to keep the temperature at 70°C to obtain a white carbon black suspension as the pretreatment liquid D;
[0048] c. 9Al, which accounts for 35% of the mass fraction of pretreatment liquid C 2 O 3 •B 2 O 3 The whiskers were added to the pretreatment solution C, and the temperature was kept at 70°C by ultrasonic vibration heating. The mixture was stirred for 2 hours, filtered and dried to obtain 9Al modified with γ-glycidyloxypropyltrimethoxysilane. 2 O 3 •B 2 O 3 Whiskers;
[0049] d. 9Al modified with γ-glycidyloxypropyltrimethoxysilane, which accounts for 40% of the mass fraction of pretreatment solution D, is added. 2 O 3 •B 2 O 3The whiskers were added to the pretreatment solution D, and the temperature was maintained at 50°C by ultrasonic vibration heating, stirred for 2 hours, filtered and dried to obtain modified 9Al modified twice by γ-glycidyloxypropyltrimethoxysilane and white carbon black. 2 O 3 •B 2 O 3 Whiskers.
[0050] The method for preparing the TPU material for the antibacterial and anti-slip mat of the offshore deck comprises the following steps:
[0051] (1) Dehydrate polytetramethylene glycol in vacuum at 100°C for 2 h, then add antioxidant 1010 and modified 9Al 2 O 3 •B 2 O 3 Whiskers and organic bismuth catalyst DY-20 are stirred evenly to obtain a mixed solution A, which is placed in an oven at 100°C for later use;
[0052] (2) heating and melting the octafluoro-1,6-hexanediol chain extender at 75° C. to obtain a molten liquid B;
[0053] (3) Pour the mixed liquid A and the molten liquid B into a reaction container and stir evenly. Then add 4,4'-diphenylmethane diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place it in an oven at 100°C and mature for 6 hours to obtain the product.
[0054] Example 2
[0055] The TPU material for the antibacterial and anti-slip mat of the offshore deck is prepared from the following raw materials in percentage by mass:
[0056] Polyethylene glycol 76.95%,
[0057] 1,6-hexamethylene diisocyanate 10.93%,
[0058] Octafluoro-1,6-hexanediol 3.72%,
[0059] Modified 9Al 2 O 3 •B 2 O 3 Whiskers 8%,
[0060] Antioxidant 1024 0.2%,
[0061] Organic tin catalyst T-9 0.2%,
[0062] The number average molecular weight of the polyethylene glycol is 1500;
[0063] The modified 9Al 2 O3 •B 2 O 3 The preparation of whiskers includes the following steps:
[0064] a. Adjust the pH of the hydrolyzate of γ-glycidyloxypropyltrimethoxysilane to 8.5 to prepare the pretreatment solution C;
[0065] b. Place 15% white carbon black by mass in a container with distilled water, and heat it by ultrasonic vibration to keep the temperature at 75°C to obtain a white carbon black suspension as pretreatment liquid D;
[0066] c. 9Al, which accounts for 35% of the mass fraction of pretreatment liquid C 2 O 3 •B 2 O 3 The whiskers were added to the pretreatment solution C, and the temperature was kept at 75°C by ultrasonic vibration heating. The mixture was stirred for 3 hours, filtered and dried to obtain 9Al modified with γ-glycidyloxypropyltrimethoxysilane. 2 O 3 •B 2 O 3 Whiskers;
[0067] d. 9Al modified with γ-glycidyloxypropyltrimethoxysilane, which accounts for 40% of the mass fraction of pretreatment solution D, is added. 2 O 3 •B 2 O 3 The whiskers were added to the pretreatment solution D, and the temperature was maintained at 55°C by ultrasonic vibration heating. The mixture was stirred for 3 hours, filtered and dried to obtain the modified 9Al2O3 modified with γ-glycidyloxypropyltrimethoxysilane and white carbon black. 2 O 3 •B 2 O 3 Whiskers.
[0068] The method for preparing the TPU material for the antibacterial and anti-slip mat of the offshore deck comprises the following steps:
[0069] (1) Dehydrate polyethylene glycol in a vacuum oven at 110°C for 2.5 h. After dehydration, add antioxidant 1024 and modified 9Al 2 O 3 •B 2 O 3 Whiskers and organotin catalyst T-9 are stirred evenly to obtain a mixed solution A, which is placed in an oven at 110°C for later use;
[0070] (2) heating and melting the octafluoro-1,6-hexanediol chain extender at 85° C. to obtain a molten liquid B;
[0071] (3) Pour the mixed liquid A and the molten liquid B into a reaction container and stir evenly. Then add 1,6-hexamethylene diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place the mixture in an oven at 110°C and mature for 7 hours to obtain the product.
[0072] Example 3
[0073] The TPU material for the antibacterial and anti-slip mat of the offshore deck is prepared from the following raw materials in percentage by mass:
[0074] Polypropylene glycol 62.72%,
[0075] Xylene diisocyanate 14.61%,
[0076] Octafluoro-1,6-hexanediol 12.27%,
[0077] Modified 9Al 2 O 3 •B 2 O 3 Whiskers 10%,
[0078] Antioxidant 1076 0.3%,
[0079] Tetra-tert-butyl titanate 0.1%,
[0080] The number average molecular weight of the polypropylene glycol is 2000;
[0081] The modified 9Al 2 O 3 •B 2 O 3 The preparation of whiskers includes the following steps:
[0082] a. Adjust the pH of the hydrolyzate of γ-glycidyloxypropyltrimethoxysilane to 9 to prepare the pretreatment solution C;
[0083] b. Place 20% white carbon black by mass in a container with distilled water, and heat it by ultrasonic vibration to keep the temperature at 80°C to obtain a white carbon black suspension as a pretreatment liquid D;
[0084] c. 9Al, which accounts for 35% of the mass fraction of pretreatment liquid C 2 O 3 •B 2 O 3 The whiskers were added to the pretreatment solution C, and the temperature was kept at 80°C by ultrasonic vibration heating. The mixture was stirred for 4 hours, filtered and dried to obtain 9Al modified with γ-glycidyloxypropyltrimethoxysilane. 2 O 3 •B 2 O 3 Whiskers;
[0085] d. 9Al modified with γ-glycidyloxypropyltrimethoxysilane, which accounts for 40% of the mass fraction of pretreatment solution D, is added. 2 O 3 •B 2 O 3 The whiskers were added to the pretreatment solution D, and the temperature was maintained at 60°C by ultrasonic vibration heating, stirred for 4 hours, filtered and dried to obtain the modified 9Al modified twice by γ-glycidyloxypropyltrimethoxysilane and white carbon black. 2 O 3 •B 2 O 3 Whiskers.
[0086] The method for preparing the TPU material for the antibacterial and anti-slip mat of the offshore deck comprises the following steps:
[0087] (1) Polypropylene glycol was vacuum dehydrated at 120°C for 3 h, and antioxidant 1076 and modified 9Al were added after dehydration. 2 O 3 •B 2 O 3 Whiskers and tetra-tert-butyl titanate are stirred evenly to obtain a mixed solution A, which is placed in an oven at 120°C for later use;
[0088] (2) heating and melting the octafluoro-1,6-hexanediol chain extender at 95° C. to obtain a molten liquid B;
[0089] (3) Pour the mixed liquid A and the molten liquid B into a reaction container and stir evenly. Then add xylene diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place it in an oven at 120°C and mature for 8 hours to obtain the product.
[0090] Comparative Example 1
[0091] The TPU material for the antibacterial and anti-slip mat of the offshore deck is prepared from the following raw materials in percentage by mass:
[0092] Polytetramethylene glycol 52.42%,
[0093] 4,4'-diphenylmethane diisocyanate 26.7%,
[0094] Octafluoro-1,6-hexanediol 14.48%,
[0095] One-time modified 9Al 2 O 3 ·B 2 O 3 Whisker 6%,
[0096] Antioxidant 1010 0.1%,
[0097] Organic bismuth catalyst DY-20 0.3%,
[0098] The number average molecular weight of the polytetramethylene glycol is 1000;
[0099] Among them, one modified 9Al 2 O 3 ·B 2 O 3 The whiskers were only modified with γ-glycidyloxypropyltrimethoxysilane and not modified with silica.
[0100] One-time modified 9Al 2 O 3 ·B 2 O 3 The preparation of whiskers includes the following steps:
[0101] a. Adjust the pH of the hydrolyzate of γ-glycidyloxypropyltrimethoxysilane to 8 to prepare a pretreatment solution C;
[0102] b. 9Al, which accounts for 35% of the mass fraction of pretreatment liquid C 2 O 3 ·B 2 O 3 The whiskers were added to the pretreatment solution C, and the temperature was kept at 70°C by ultrasonic vibration heating. The mixture was stirred for 2 hours, filtered and dried to obtain 9Al modified with γ-glycidyloxypropyltrimethoxysilane. 2 O 3 ·B 2 O 3 Whiskers, i.e., once modified 9Al 2 O 3 ·B 2 O 3 Whiskers;
[0103] The method for preparing the TPU material for the antibacterial and anti-slip mat of the offshore deck comprises the following steps:
[0104] (1) Dehydrate polytetramethylene glycol in vacuum at 100°C for 2 h, then add antioxidant 1010 and primary modified 9Al 2 O 3 ·B 2 O 3 Whiskers and organic bismuth catalyst DY-20 are stirred evenly to obtain a mixed solution A, which is placed in an oven at 100°C for later use;
[0105] (2) heating and melting the octafluoro-1,6-hexanediol chain extender at 75° C. to obtain a molten liquid B;
[0106] (3) Pour the mixed liquid A and the molten liquid B into a reaction container and stir evenly. Then add 4,4'-diphenylmethane diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place it in an oven at 100°C and mature for 6 hours to obtain the product.
[0107] Comparative Example 2
[0108] The TPU material for the antibacterial and anti-slip mat of the offshore deck is prepared from the following raw materials in percentage by mass:
[0109] Polytetramethylene glycol 52.42%,
[0110] 4,4'-diphenylmethane diisocyanate 26.7%,
[0111] Octafluoro-1,6-hexanediol 14.48%,
[0112] 9Al 2 O 3 ·B 2 O 3 Whisker 6%,
[0113] Antioxidant 1010 0.1%,
[0114] Organic bismuth catalyst DY-20 0.3%,
[0115] The number average molecular weight of the polytetramethylene glycol is 1000;
[0116] Compared with Example 1, 9Al 2 O 3 ·B 2 O 3 The whiskers were unmodified.
[0117] The method for preparing the TPU material for the antibacterial and anti-slip mat of the offshore deck comprises the following steps:
[0118] (1) Dehydrate polytetramethylene glycol in vacuum at 100°C for 2 h, and then add antioxidants 1010 and 9Al 2 O 3 ·B 2 O 3 Whiskers and organic bismuth catalyst DY-20 are stirred evenly to obtain a mixed solution A, which is placed in an oven at 100°C for later use;
[0119] (2) heating and melting the octafluoro-1,6-hexanediol chain extender at 75° C. to obtain a molten liquid B;
[0120] (3) Pour the mixed liquid A and the molten liquid B into a reaction container and stir evenly. Then add 4,4'-diphenylmethane diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place it in an oven at 100°C and mature for 6 hours to obtain the product.
[0121] Comparative Example 3
[0122] The TPU material for the antibacterial and anti-slip mat of the offshore deck is prepared from the following raw materials in percentage by mass:
[0123] Polytetramethylene glycol 52.42%,
[0124] 4,4'-diphenylmethane diisocyanate 33.68%,
[0125] 1,4-Butanediol 7.5%,
[0126] Modified 9Al 2 O 3 ·B 2 O 3 Whisker 6%,
[0127] Antioxidant 1010 0.1%,
[0128] Organic bismuth catalyst DY-20 0.3%,
[0129] The number average molecular weight of the polytetramethylene glycol is 1000;
[0130] The modified 9Al 2 O 3 ·B 2 O 3 The whisker preparation method is the same as that in Example 1.
[0131] The method for preparing the TPU material for the antibacterial and anti-slip mat of the offshore deck comprises the following steps:
[0132] (1) Dehydrate polytetramethylene glycol in vacuum at 100°C for 2 h, then add antioxidant 1010 and modified 9Al 2 O 3 ·B 2 O 3 Whiskers and organic bismuth catalyst DY-20 are stirred evenly to obtain a mixed solution A, which is placed in an oven at 100°C for later use;
[0133] (2) heating the 1,4-butanediol chain extender at 75°C as solution B;
[0134] (3) Pour the mixed solution A and solution B into a reaction container and stir evenly. Then add 4,4'-diphenylmethane diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place the mixture in an oven at 100°C and age for 6 hours to obtain the product.
[0135] Comparative Example 4
[0136] The TPU material for the antibacterial and anti-slip mat of the offshore deck is prepared from the following raw materials in percentage by mass:
[0137] Polytetramethylene glycol 55.78%,
[0138] 4,4'-diphenylmethane diisocyanate 28.42%,
[0139] Octafluoro-1,6-hexanediol 15.4%,
[0140] Antioxidant 1010 0.1%,
[0141] Organic bismuth catalyst DY-20 0.3%,
[0142] The number average molecular weight of the polytetramethylene glycol is 1000;
[0143] The method for preparing the TPU material for the antibacterial and anti-slip mat of the offshore deck comprises the following steps:
[0144] (1) Dehydrate polytetramethylene glycol in a vacuum at 100°C for 2 h, add antioxidant 1010 and organic bismuth catalyst DY-20 after dehydration, stir evenly to obtain a mixed solution A, and place it in an oven at 100°C for later use;
[0145] (2) heating and melting the octafluoro-1,6-hexanediol chain extender at 75° C. to obtain a molten liquid B;
[0146] (3) Pour the mixed liquid A and the molten liquid B into a reaction container and stir evenly. Then add 4,4'-diphenylmethane diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place it in an oven at 100°C and mature for 6 hours to obtain the product.
[0147] Comparative Example 5
[0148] Comparative Example 5: No modified 9Al added 2 O 3 ·B 2 O 3 Whiskers and octafluoro-1,6-hexanediol chain extender, using 1,4-butanediol instead of octafluoro-1,6-hexanediol.
[0149] The TPU material for the antibacterial and anti-slip mat of the offshore deck is prepared from the following raw materials in percentage by mass:
[0150] Polytetramethylene glycol 55.78%,
[0151] 4,4'-diphenylmethane diisocyanate 35.84%,
[0152] 1,4-Butanediol 7.98%,
[0153] Antioxidant 1010 0.1%,
[0154] Organic bismuth catalyst DY-20 0.3%,
[0155] The number average molecular weight of the polytetramethylene glycol is 1000;
[0156] The method for preparing the TPU material for the antibacterial and anti-slip mat of the offshore deck comprises the following steps:
[0157] (1) Dehydrate polytetramethylene glycol in a vacuum at 100°C for 2 h, add antioxidant 1010 and organic bismuth catalyst DY-20 after dehydration, stir evenly to obtain a mixed solution A, and place it in an oven at 100°C for later use;
[0158] (2) heating the 1,4-butanediol chain extender at 75°C as solution B;
[0159] (3) Pour the mixed solution A and solution B into a reaction container and stir evenly. Then add 4,4'-diphenylmethane diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place the mixture in an oven at 100°C and age for 6 hours to obtain the product.
[0160] The TPU materials prepared in Examples 1-3 and Comparative Examples 1-5 were in large blocks, which were crushed by a crusher and injection molded by an injection molding machine for performance testing. The test results are shown in Table 1 below. The test items and characterization methods are as follows:
[0161] Tensile strength test: Execute ASTM D412 standard;
[0162] Abrasion test: Execute ISO 4649 standard to characterize wear resistance;
[0163] Anti-slip test: Refer to the US military standard "MIL-PRF-24667C", use a testing machine to test the friction coefficient, generally ≥0.9 to pass;
[0164] Bacterial and corrosion resistance: The main bacteria in seawater are Gram-negative rods. The tensile strength is tested by immersing in Zhoushan seawater for 180 days to characterize the bacterial and corrosion resistance.
[0165] Table 1 Performance test results of Examples 1-3 and Comparative Examples 1-5
[0166]
[0167] As can be seen from Table 1, the TPU materials for marine deck antibacterial anti-skid mats prepared in Examples 1-3 of the present invention all have good wear resistance, anti-skid, antibacterial and corrosion resistance. 2 O 3 ·B 2 O 3 Whiskers, unmodified 9Al 2 O 3 ·B 2 O 3 Whiskers, no octafluoro-1,6-hexanediol chain extender, no modified 9Al 2 O 3 ·B 2 O 3 Whiskers, no modified 9Al 2 O 3 ·B 2 O 3 The TPU materials prepared by whiskers and octafluoro-1,6-hexanediol chain extender have obvious increased wear and reduced friction coefficient. The tensile strength decreases after immersion in seawater, showing poor bacteria and corrosion resistance.
Claims
1. A TPU material for antibacterial and anti-slip mats on offshore decks, characterized in that: It is prepared from the following raw materials in percentage by weight: Polyether polyol 52.42%-76.95%, Diisocyanate 10.93%-26.7%, Diol chain extender 3.72%-14.48%, Modified 9Al2O3•B2O3 whisker 6%-10%, Antioxidant 0.1%-0.3%, Catalyst 0.1%-0.3%; Wherein, the diol chain extender is octafluoro-1,6-hexanediol; Modified 9Al2O3•B2O3 whiskers were prepared by modification with γ-glycidyloxypropyltrimethoxysilane and white carbon black; The preparation of modified 9Al2O3•B2O3 whiskers includes the following steps: a. Adjust the pH of the hydrolyzate of γ-glycidyloxypropyltrimethoxysilane to 8-9 to prepare the pretreatment solution C; b. Place 10%-20% white carbon black by mass in a container with distilled water, and heat by ultrasonic vibration to maintain the temperature at 70-80°C to obtain a white carbon black suspension as pretreatment liquid D; c. Add 9Al2O3•B2O3 whiskers to pretreatment solution C, maintain the temperature at 70-80°C by ultrasonic vibration heating, stir for 2-4 hours, filter and dry to obtain 9Al2O3•B2O3 whiskers modified with γ-glycidyloxypropyltrimethoxysilane; d. Add 9Al2O3•B2O3 whiskers modified with γ-glycidyloxypropyltrimethoxysilane into pretreatment solution D, maintain the temperature at 50-60°C by ultrasonic vibration heating, stir for 2-4 hours, filter and dry to obtain modified 9Al2O3•B2O3 whiskers modified twice with γ-glycidyloxypropyltrimethoxysilane and white carbon black.
2. The TPU material for antibacterial and anti-slip mats for offshore decks according to claim 1, characterized in that: The polyether polyol is polyethylene glycol, polypropylene glycol or polytetramethylene glycol, and has a number average molecular weight of 1000-2000.
3. The TPU material for antibacterial and anti-slip mats for offshore decks according to claim 1, characterized in that: The diisocyanate is 4,4'-diphenylmethane diisocyanate, 1,6-hexamethylene diisocyanate or xylylene diisocyanate.
4. The TPU material for antibacterial and anti-slip mats for offshore decks according to claim 1, characterized in that: The antioxidant is antioxidant 1010, antioxidant 1024 or antioxidant 1076.
5. The TPU material for antibacterial and anti-slip mats for offshore decks according to claim 1, characterized in that: The catalyst is one of the organic bismuth catalyst DY-20, the organic tin catalyst T-9, and tetra-tert-butyl titanate.
6. The TPU material for antibacterial and anti-slip mats for offshore decks according to claim 1, characterized in that: The amounts of 9Al2O3•B2O3 whiskers and 9Al2O3•B2O3 whiskers modified with γ-glycidyloxypropyltrimethoxysilane added in step c and step d are 35% and 40% of the mass fraction of pretreatment solution C and pretreatment solution D, respectively.
7. A method for preparing the TPU material for the antibacterial and anti-slip mat for offshore decks according to any one of claims 1 to 6, characterized in that: The steps include: (1) Dehydrate the polyether polyol under vacuum at 100-120°C for 2-3h, add antioxidant, modified 9Al2O3•B2O3 whisker and catalyst after dehydration, stir evenly to obtain mixed solution A, and place in a 100-120°C oven for later use; (2) heating and melting the diol chain extender at 75-95° C. to obtain a molten liquid B; (3) Pour the mixed liquid A and the molten liquid B into a reaction container and stir evenly. Then add the diisocyanate into the reaction container and continue stirring until the material in the reaction container is in a gel state. Place it in an oven at 100-120°C and mature for 6-8 hours to obtain the product.