A tear-resistant, high-temperature-resistant, soft insulating film, composite material and preparation method
By using oxazole structural block insulating film and paper-based lamination technology in new energy vehicle motors, the problem of easy tearing and high temperature resistance of insulating materials has been solved, the tear resistance and high temperature resistance have been improved, and the motor has been improved. Production efficiency and material life.
Patent Information
- Application Number
- CN202410961581.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Patents(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-18
- Publication Date
- 2024-10-11
- Estimated Expiration
- 2044-07-18
AI Technical Summary
Existing insulation materials in new energy vehicle motors are prone to tearing and are not resistant to high temperatures. They cannot solve the problems of tear resistance and high temperature resistance at the same time, which affects motor production efficiency and material life.
A method is used to prepare a tear-resistant and high-temperature-resistant soft insulating film. Pre-polycondensation reaction is carried out under the protection of inert gas to form an oxazole structural block, which is combined with aromatic acid chloride, polyphosphoric acid and aromatic diamine. After passing through the die The cast film is formed, stretched and dried to form an insulating film with excellent mechanical properties and high temperature resistance, and is pressed with the paper base to form a tear-resistant, high-temperature-resistant soft insulating composite material.
Significantly improves the tear resistance and high temperature resistance of the insulation material, solves the problem of easy tearing and lightweight of the material during the motor slotting process, improves the slotting success rate, extends the material life, and reduces raw material loss and environmental pollution .
Smart Images

Figure CN118496542B_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a tear-resistant, high-temperature-resistant, soft insulating film, a composite material and a preparation method, and belongs to the technical field of insulating composite materials. Background Art
[0002] As one of the three core components of new energy vehicles, the importance of new energy vehicle motors is self-evident. The development trend of new energy vehicle motors is gradually moving towards high speed, small size, compactness and lightweight, and these trends also put forward higher requirements for the insulation material used in the heart of variable frequency motors.
[0003] At present, the insulation materials of variable frequency motors are mainly used in slot insulation, phase insulation, slot wedge insulation, etc., and there are problems of easy tearing and high temperature resistance of materials in the slot process. Improving the tear resistance and high temperature resistance of insulating materials can effectively improve the efficiency of motor slots, thereby improving the production efficiency of motors; improving the tear resistance and high temperature resistance of materials can effectively extend the service life of materials, reduce the loss of raw materials and environmental pollution, and generate considerable economic and environmental value. At present, Chinese patent application CN114927297A discloses an insulating composite material for new energy motors, including a first calendered polyaramid fiber paper layer, a second polyphenylene sulfide film layer, a third calendered polyaramid fiber paper layer, and a fourth polyphenylene sulfide film layer, wherein the paper layer and the film layer are bonded by compounding a multi-component composite glue, and the composite glue is compounded by hydroxy acrylate resin, epoxy glue, and polyurethane glue. The insulating composite material is well thermoformed in the insulation process of new energy motor slots and is easy to process. Chinese patent application CN110349717A discloses a high-temperature stable flame-retardant insulating composite material for generators. The composite material is a three-layer composite material, the first layer is a polyoxadiazole fiber paper outer layer, the second layer is a polyimide film middle layer, and the third layer is a polyoxadiazole fiber paper outer layer, and the middle layer film layer and the outer layer paper layer are compounded by a dry compounding method using modified polyurethane glue. However, these disclosed technical solutions cannot solve the problem of easy tearing of insulating materials and high temperature resistance requirements at the same time. Summary of the invention
[0004] In view of the deficiencies in the prior art, the present invention provides a tear-resistant, high-temperature resistant, soft insulating film, a composite material and a preparation method, which are suitable for insulation protection of new energy vehicle motors. This not only solves the problem of easy tearing of insulating materials and the need for lightweighting during motor production, but also improves the high-temperature resistance of insulating materials.
[0005] The technical solution of the present invention to solve the above technical problems is as follows: a method for preparing a tear-resistant, high-temperature-resistant, soft insulating film, the preparation method comprising:
[0006] S1. Preparation of polymer solution:
[0007] S1.1, under the protection of inert gas, 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and aromatic acid chloride are subjected to a pre-condensation reaction to obtain a pre-polymer solution 1;
[0008] S1.2, in an organic solvent, the aromatic diamine reacts with the prepolymer solution 1 to obtain the prepolymer solution 2;
[0009] S1.3, reacting the prepolymer liquid 2 with an aromatic acyl chloride to obtain a prepolymer liquid 3; neutralizing the prepolymer liquid 3 and filtering to obtain a prepolymer liquid 4;
[0010] S1.4, adding aromatic acid chloride to the prepolymer solution 4 again to obtain polymerization solution 1, and after neutralization treatment to obtain polymerization solution 2;
[0011] S2. Preparation of insulating film:
[0012] After filtering and defoaming, the polymer solution 2 is cast into a film in a coagulation bath through a die head, and is sequentially stretched longitudinally and transversely in a water bath, and then dried to obtain the insulating film.
[0013] Furthermore, the specific operation of step S1.1 is:
[0014] Under the protection of inert gas, aromatic acid chloride and polyphosphoric acid are added to a reaction kettle, stirred evenly, and then 4,6-diaminoresorcinol hydrochloride is added, the temperature is raised to 70-90° C., stirred and reacted for 1-2 hours, and then the temperature is raised to 100-130° C., stirred and reacted for 4-6 hours, and the prepolymerization is completed to obtain the prepolymer solution 1.
[0015] Further, the reaction temperature of step S1.2 is 25-40°C;
[0016] The reaction temperature of step S1.3 is 0-10°C;
[0017] The reaction temperature of step S1.4 is 20-35°C.
[0018] Furthermore, in step S1.3, the prepolymer solution 3 is neutralized with aqueous ammonia, and the pH of the prepolymer solution 4 is 6.5-7.8;
[0019] In step S1.4, the polymerization solution 1 is neutralized with an organic base, and the pH of the polymerization solution 1 is 6.5-7.8;
[0020] The organic base is any one or a combination of methylamine, dimethylamine, ethylamine and diethylamine.
[0021] Furthermore, the aromatic acid chloride is one or more of isophthaloyl chloride and terephthaloyl chloride;
[0022] The aromatic diamine is one or more of m-phenylenediamine, p-phenylenediamine and o-phenylenediamine;
[0023] In the entire step S1, the mass ratio of the aromatic diamine, 4,6-diaminoresorcinol hydrochloride and aromatic acid chloride is (8.6-11): (3.5-4): (21.5-28.5);
[0024] In step S1.1, the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and aromatic acid chloride is (3.5-4): (13-21): 10;
[0025] The mass ratio of the aromatic acyl chloride in step S1.3 to the aromatic acyl chloride in step S1.4 is (9-15):(2.5-3.5).
[0026] Furthermore, in step S1.2, the mass concentration of the aromatic diamine in the organic solvent is 12-16%; the organic solvent is one or a combination of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide;
[0027] The viscosity of the polymer solution 2 is 900-1500 Po.
[0028] Furthermore, in step S2, the coagulation bath is an aqueous solution of DMAC, wherein the mass concentration of DMAC in the coagulation bath is 55-65%, and the temperature of the coagulation bath is 35-55°C;
[0029] Step S2 is carried out in three stages in the water bath:
[0030] The water temperature in the first stage is 40~50℃, and longitudinal stretching is performed with a stretching ratio of 1.2~1.8;
[0031] The water temperature in the second stage is 55~70℃, and transverse stretching is performed with a stretching ratio of 0.3~0.9;
[0032] The water temperature in the third stage is 50~60℃, without stretching;
[0033] In step S2, the drying is carried out in two stages: the first stage is steam drying at 100-120°C; the second stage is hot roller drying at 90-100°C.
[0034] The invention also discloses a tear-resistant, high-temperature-resistant and soft insulating film, which is prepared by the preparation method of the invention.
[0035] The present invention also discloses a method for preparing a tear-resistant, high-temperature-resistant, soft insulating composite material, wherein glue is coated on the insulating film, and after drying, the film is pressed together with a paper base to form the tear-resistant, high-temperature-resistant, soft insulating composite material.
[0036] Furthermore, the preparation method of the paper base is:
[0037] (1) Preparation of staple fibers:
[0038] After filtering and removing bubbles, the polymer solution 2 is sprayed through a spinneret in a coagulation bath to form primary fibers, which are then stretched, washed, dried, shaped, and cut to obtain staple fibers;
[0039] The polymer solution 2 is the polymer solution 2 obtained in step S1 of the preparation method of the present invention;
[0040] (2) Preparation of precipitated pulp:
[0041] Mix water, glycerol and chloride salt to prepare a mixed solution, then mix the mixed solution with polymer solution 2 according to a certain proportion, and then perform high-speed shearing, cooling and forming, and multi-stage water washing to obtain precipitated pulp;
[0042] (3) Preparation of paper base:
[0043] The precipitated pulp which has been subjected to a beating and dispersion treatment and the short fibers which have been subjected to a debonding and dispersion treatment are stirred and blended to obtain paper pulp, and the paper base is obtained by subjecting the paper pulp to flow forming, pressing and drying, hot pressing forming, and rewinding and slitting treatment.
[0044] Furthermore, during the preparation of the staple fibers, the stretching ratio is 1.2-1.8; the washing is carried out in two stages: the water temperature in the first stage is 50-60°C, and the water temperature in the second stage is 60-70°C; the drying temperature is 130-170°C, and the setting temperature is 300-320°C.
[0045] Furthermore, in the preparation process of the precipitated pulp, the mass ratio of water, glycerol and chloride is (34-55): (42-60): (3-6); the mass ratio of the mixed solution to the polymer solution 2 is (8-16): 1;
[0046] The high-speed shearing speed is 3000-6000 rpm / min, the temperature is 20-60°C, and the high-speed shearing time is 20-40 min;
[0047] The cooling molding process is to immerse the slurry in -5~5℃ cold water for molding;
[0048] The multi-stage water washing adopts a four-stage countercurrent water washing method, and the water temperature of the multi-stage water washing is: 20-30°C for the first stage, 40-50°C for the second stage, 60-70°C for the third stage, and 80-90°C for the fourth stage;
[0049] The average length of the precipitated pulp is 0.8-1.6 mm, and the specific surface area is 30-45 m 2 / g.
[0050] Furthermore, in the process of preparing the paper base, the mass ratio of the precipitated pulp and the short fibers is (4-6): (4-6);
[0051] The pressure of the pressing and drying is 1-2 MPa and the temperature is 120-160°C;
[0052] The pressure of the hot pressing molding is 10-24 MPa and the temperature is 220-280°C.
[0053] Furthermore, the coating amount of the glue is 5-50 g / m 2 The pressure during pressing is 0.3~0.6MPa.
[0054] The invention also discloses a tear-resistant, high-temperature-resistant, soft insulating composite material. The tear-resistant, high-temperature-resistant, soft insulating composite material is prepared according to the preparation method of the invention.
[0055] The beneficial effects of the present invention are:
[0056] In the process of preparing the polymer solution of the present invention, after the aromatic acyl chloride and polyphosphoric acid are uniformly stirred, 4,6-diaminoresorcinol hydrochloride is added, and polymerization is first performed, and then the temperature is increased for polycondensation, thereby forming an oxazole structure block in the polymer (that is, the carbonyl group of the aromatic acyl chloride and the amino group in the 4,6-diaminoresorcinol hydrochloride undergo a preliminary dehalogenation reaction, and then under high temperature conditions, the water molecule is removed from the molecular chain, the carbonyl bond is opened for intramolecular condensation, and the oxazole functional group is formed). Using a polymer solution containing an oxazole structure block to prepare an insulating film and a paper base is beneficial to improving the mechanical properties and high temperature resistance of the insulating film and the paper base, so that the composite material finally prepared has excellent tear resistance and high temperature resistance compared with conventional products of the same thickness and specifications.
[0057] The preparation method of the present invention improves the mechanical properties and modulus of the substrate from the perspective of molecular structure by introducing a portion of oxazole structure blocks with a rigid planar structure and a strong electron-donating conjugation effect into the polymer solution of the paper base and the film. As a result, both the paper base and the film have excellent tear resistance and high temperature resistance, so that the tear resistance and high temperature resistance of the final aromatic flexible insulating composite material are more significantly excellent, achieving a multiple protection effect, so that the application in the motor slot process is more convenient and the slot success rate is higher. It is suitable for the insulation protection of new energy vehicle motors, which not only solves the problem of easy tearing and lightweight of insulating materials in the motor production process, but also improves the high temperature resistance of insulating materials.
[0058] In the process of electrode insertion, the thicker the composite material formed by paper or film, the easier it is to insert the slot because it is not easy to tear. However, the thicker the composite material, the heavier it is, which will also affect the insertion effect. The composite material prepared by the preparation method of the present invention is relatively thin. Conventional thin composite materials are very easy to tear during the insertion process. The composite material prepared by the present invention has a good insertion effect and is not easy to tear even if it is thin. Therefore, it is more conducive to solving the problem of lightweight demand for insulating materials in the electrode production process. BRIEF DESCRIPTION OF THE DRAWINGS
[0059] Figure 1 The present invention is a flow chart of the preparation process of the tear-resistant, high-temperature-resistant, soft insulating composite material. DETAILED DESCRIPTION
[0060] The specific implementation of the present invention is described in detail below. The present invention can be implemented in many other ways than those described herein, and those skilled in the art can make similar improvements without violating the connotation of the present invention, so the present invention is not limited by the specific embodiments disclosed.
[0061] Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those commonly understood by those skilled in the art to which the present invention belongs. The terms used are only for describing specific embodiments and are not intended to limit the present invention.
[0062] like Figure 1 As shown, a method for preparing a tear-resistant, high-temperature-resistant, aromatic, soft insulating composite material comprises the following preparation steps:
[0063] S1. Preparation of polymer solution:
[0064] S1.1, in a reaction kettle filled with nitrogen, 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid (the polyphosphoric acid used in the embodiment of the present invention is purchased from Jiangsu Runfeng Synthetic Technology Co., Ltd., product number 8017-16-1) and aromatic acid chloride are added to carry out a pre-polycondensation reaction to obtain a prepolymer solution 1;
[0065] S1.2, dissolving the aromatic diamine in an organic solvent to prepare an aromatic diamine solution, and then adding it to the prepolymer solution 1 to react, and wait until the prepolymer solution 2;
[0066] S1.3, adding aromatic acid chloride to prepolymer liquid 2 to react, to obtain prepolymer liquid 3; adding ammonia water to prepolymer liquid 3 to neutralize, and filtering to obtain prepolymer liquid 4;
[0067] S1.4, adding aromatic acid chloride to prepolymer solution 4 again to obtain polymerization solution 1, and neutralizing with an organic base to obtain polymerization solution 2;
[0068] S2. Preparation of insulating film:
[0069] After filtering and removing bubbles from the polymer solution 2, the polymer solution 2 is cast into a film in a coagulation bath through a die head, and longitudinally and transversely stretched in a water bath in sequence, and then dried to obtain an insulating film;
[0070] S3. Preparation of staple fibers:
[0071] After filtering and removing bubbles, the polymer solution 2 is sprayed through a spinneret in a coagulation bath to form primary fibers, which are then stretched, washed, dried, shaped, and cut to obtain staple fibers;
[0072] S4. Preparation of precipitated pulp:
[0073] Mix water, glycerol and chloride salt to prepare a mixed solution, then mix the mixed solution with polymer solution 2 according to a certain proportion, and then perform high-speed shearing, cooling and forming, and multi-stage water washing to obtain precipitated pulp;
[0074] S5. Preparation of paper base:
[0075] The precipitated pulp which has been subjected to a beating and dispersion treatment and the short fibers which have been subjected to a debonding and dispersion treatment are stirred and blended to obtain paper pulp, and then the paper pulp is subjected to a flow forming, a pressing and drying, a hot pressing forming, and a rewinding and slitting treatment to obtain the paper base;
[0076] S6. Preparation of soft insulating composite materials:
[0077] The insulating film coated with glue is baked and then pressed with the paper base to form the tear-resistant and high-temperature-resistant soft insulating composite material.
[0078] More specifically, the insulating film prepared in step S2 needs to be subjected to a step-by-step heat preservation after winding before it can be used: 110° C. constant temperature for 3 hours and 90° C. constant temperature for 6 hours.
[0079] Specifically, the specific operations of step S1 are as follows:
[0080] S1.1: Add aromatic acyl chloride and polyphosphoric acid into a reactor, stir for 20-40 min, add 4,6-diaminoresorcinol hydrochloride, then heat to 70-90°C, stir for 1-2 hours, heat to 100-130°C, stir for 4-6 hours, complete prepolymerization, and obtain prepolymer solution 1;
[0081] S1.2: Prepare aromatic diamine into aromatic diamine solution in a preparation kettle, then add it into prepolymer solution 1, raise the temperature to 25-40°C, stir for 10-15 minutes, and obtain prepolymer solution 2;
[0082] S1.3: Add part of the aromatic acid chloride to the prepolymer solution 2, keep the temperature in a cold water bath at 0-10°C, stir for 30-40 minutes, and obtain the prepolymer solution 3. Then, add ammonia water to adjust the pH to 6.5-7.8, and filter to obtain the prepolymer solution 4.
[0083] S1.4: Add the remaining aromatic acid chloride in the formula to the prepolymer solution 4, stir at 20-35°C for 20-30 minutes to carry out post-polymerization to obtain the polymerization solution 1, and adjust the pH to 6.5-7.8 by adding an organic base to obtain the polymerization solution 2.
[0084] Specifically, the organic base is any one or a combination of methylamine, dimethylamine, ethylamine and diethylamine.
[0085] Specifically, the aromatic acyl chloride is one or more of isophthaloyl chloride and terephthaloyl chloride;
[0086] The aromatic diamine is one or more of m-phenylenediamine, p-phenylenediamine and o-phenylenediamine;
[0087] In the entire step S1, the mass ratio of the aromatic diamine, 4,6-diaminoresorcinol hydrochloride and aromatic acid chloride is (8.6-11): (3.5-4): (21.5-28.5);
[0088] In step S1.1, the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and aromatic acid chloride is (3.5-4): (13-21): 10;
[0089] The mass ratio of the aromatic acyl chloride in step S1.3 to the aromatic acyl chloride in step S1.4 is (9-15):(2.5-3.5).
[0090] Specifically, in step S1.2, the mass concentration of the aromatic diamine in the organic solvent is 12-16%; the organic solvent is one or a combination of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide;
[0091] The viscosity of the polymer solution 2 is 900-1500 Po.
[0092] Specifically, in step S2, the coagulation bath is an aqueous solution of DMAC, wherein the mass concentration of DMAC in the coagulation bath is 55-65%, and the temperature of the coagulation bath is 35-55° C.;
[0093] Step S2 is carried out in three stages in the water bath:
[0094] The water temperature in the first stage is 40~50℃, and longitudinal stretching is performed with a stretching ratio of 1.2~1.8;
[0095] The water temperature in the second stage is 55~70℃, and transverse stretching is performed with a stretching ratio of 0.3~0.9;
[0096] The water temperature in the third stage is 50~60℃, without stretching;
[0097] In step S2, the drying is carried out in two stages: the first stage is steam drying at 100-120°C; the second stage is hot roller drying at 90-100°C.
[0098] Specifically, during the preparation of the staple fibers, the stretching ratio is 1.2-1.8; the washing is carried out in two stages: the water temperature in the first stage is 50-60°C, and the water temperature in the second stage is 60-70°C; the drying temperature is 130-170°C, and the setting temperature is 300-320°C.
[0099] Specifically, in the preparation process of the precipitated pulp, the mass ratio of water, glycerol and chloride salt is (34-55): (42-60): (3-6); the mass ratio of the mixed solution to the polymer solution 2 is (8-16): 1; the chloride salt is selected from any one or a combination of calcium chloride, lithium chloride, sodium chloride, magnesium chloride and potassium chloride;
[0100] The high-speed shearing speed is 3000-6000 rpm / min, the temperature is 20-60°C, and the high-speed shearing time is 20-40 min;
[0101] The cooling molding process is to immerse the slurry in -5~5℃ cold water for molding;
[0102] The multi-stage water washing adopts a four-stage countercurrent water washing method, and the water temperature of the multi-stage water washing is: 20-30°C for the first stage, 40-50°C for the second stage, 60-70°C for the third stage, and 80-90°C for the fourth stage;
[0103] The average length of the precipitated pulp is 0.8-1.6 mm, and the specific surface area is 30-45 m 2 / g.
[0104] Specifically, in the preparation process of the paper base, the mass ratio of precipitated pulp and short fibers is (4-6): (4-6); the stirring speed is 1000-3000 rpm / min, and the stirring time is 10-20 min;
[0105] The pressure of the pressing and drying is 1-2 MPa and the temperature is 120-160°C;
[0106] The pressure of the hot pressing molding is 10-24 MPa and the temperature is 220-280°C.
[0107] Specifically, in the process of preparing the soft insulating composite material in step S6, the coating amount of the glue is 5-50 g / m 2The pressure during pressing is 0.3~0.6MPa.
[0108] More specifically, the glue used in the embodiment of the present invention is Henkel Loctite 2681 (main agent) and Henkel Loctite 5094 (curing agent).
[0109] Example 1
[0110] A method for preparing a tear-resistant, high-temperature resistant aromatic soft insulating composite material, the preparation method comprising:
[0111] (1) Preparation of polymer solution:
[0112] Add 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride into a reactor filled with nitrogen, wherein the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride is 3.5:13.5:10, stir for 30 minutes, then heat to 80° C. and stir for 1.5 hours, and heat again to 115° C. and stir for 5 hours to obtain prepolymer solution 1;
[0113] Dissolve 10 parts of m-phenylenediamine in N,N-dimethylacetamide to prepare a solution with a mass concentration of 14%, then slowly pour it into the polymerization solution 1, heat it to 30°C, and stir it for 13 minutes to obtain the prepolymer solution 2;
[0114] Add 12 parts of isophthaloyl chloride to prepolymer solution 2, stir in a water bath at 5°C for 35 minutes to obtain prepolymer solution 3, then add ammonia water to adjust the pH to 7.1, and then filter to obtain prepolymer solution 4;
[0115] The remaining 3 parts of isophthaloyl chloride were added to the prepolymer solution 4, and the mixture was stirred at 25°C for 25 minutes to obtain a polymerization solution 1. Diethylamine was then added to adjust the pH to 7.1 to obtain a polymerization solution 2 with a viscosity of 1300 Po.
[0116] (2) Preparation of insulating film:
[0117] The polymer solution 2 is filtered and defoamed, and then sprayed through a die head in a coagulation bath with a mass concentration of 59% and a temperature of 44°C to form a primary film, and then the primary film is first washed with water at 46°C for longitudinal stretching with a stretch ratio of 1.6, then washed with water at 62°C for transverse stretching with a stretch ratio of 0.5, and finally washed with water at 55°C. The washed film is again steam dried at 112°C and hot roller dried at 96°C, and then rolled up and trimmed to obtain an insulating film. The prepared insulating film is placed in a curing room and treated at a constant temperature of 110°C for 3 hours and at a constant temperature of 90°C for 6 hours for use;
[0118] (3) Preparation of staple fibers
[0119] The polymer solution 2 is filtered and defoamed, and then sprayed through a spinneret in a coagulation bath with a mass concentration of 59% and a temperature of 44°C to form primary fibers. The primary fibers are stretched 1.6 times and then sequentially washed with water at 54°C and 67°C, and then dried with a hot roller at 152°C, and then shaped with a hot tube at 312°C, and then cut to obtain short fibers.
[0120] (4) Preparation of precipitation slurry:
[0121] Water, glycerol and potassium chloride were stirred evenly in a mass ratio of 46:50:4 to prepare a mixed solution, and then the mixed solution and polymer solution 2 were added to the precipitator in a mass ratio of 13:1, and high-speed shearing was performed at a temperature of 38°C and a speed of 4550 rpm / min for 35 minutes, and then the slurry was immersed in cold water at 0°C for molding, and then countercurrent washing was performed in a water bath at 26°C, 44°C, 65°C and 87°C in sequence to obtain a precipitated pulp with a diameter of 1.1 mm and a specific surface area of 32 m 2 / g.
[0122] (5) Preparation of paper base
[0123] The precipitated slurry is beaten and dispersed with a cone mill, and the aramid staple fibers are dispersed with a pulper. The precipitated slurry and the aramid staple fibers are stirred and blended in a ratio of 5.4:4.6. The pulp is obtained by stirring at a stirring speed of 1600 rpm / min for 15 minutes. The pulp is then formed on a chain plate, pressed and dried at a pressure of 1.5 MPa and a temperature of 140°C, and then hot-pressed at a temperature of 255°C and a pressure of 18 MPa. Finally, the paper-based material is obtained by slitting.
[0124] (6) Composite material preparation: Coat 20g / m2 on the film surface 2 The glue is then removed in an oven to remove the solvent, and the paper base and the insulating film coated with glue are compounded under a pressure of 0.5 MPa to obtain a tear-resistant, high-temperature resistant soft insulating composite material. Relevant tests can be carried out after being placed at room temperature for 7 days.
[0125] Example 2
[0126] A method for preparing a tear-resistant, high-temperature resistant aromatic soft insulating composite material, the preparation method comprising:
[0127] (1) Preparation of polymer solution:
[0128] Add 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride into a reactor filled with nitrogen, wherein the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride is 4:21:10, stir for 20 minutes, then heat to 70° C. and stir for 2 hours, and heat again to 100° C. and stir for 6 hours to obtain prepolymer solution 1;
[0129] Dissolve 11 parts of m-phenylenediamine in N-methylpyrrolidone to prepare a solution with a mass concentration of 16%, then slowly pour it into the polymerization solution 1, heat it to 40°C, and stir it for 15 minutes to obtain the prepolymer solution 2;
[0130] Add 15 parts of isophthaloyl chloride to prepolymer solution 2, stir in a water bath at 10°C for 30 minutes to obtain prepolymer solution 3, then add ammonia water to adjust the pH to 7.8, and then filter to obtain prepolymer solution 4;
[0131] Add the remaining 3.5 parts of isophthaloyl chloride to the prepolymer solution 4, stir at 30°C for 20 minutes to obtain a polymerization solution 1, and then add diethylamine to adjust the pH to 7.7 to obtain a polymerization solution 2 with a viscosity of 1400 Po;
[0132] (2) Preparation of insulating film:
[0133] The polymer solution 2 is filtered and defoamed, and then sprayed through a die head in a coagulation bath with a mass concentration of 65% and a temperature of 35°C to form a primary film, and then the primary film is first washed with water at 50°C for longitudinal stretching with a stretch ratio of 1.8, then washed with water at 55°C for transverse stretching with a stretch ratio of 0.3, and finally washed with water at 50°C, and the washed film is again steam dried at 120°C and hot roller dried at 100°C, and then rolled up and trimmed to obtain an insulating film, and the prepared insulating film is placed in a curing room and subjected to a constant temperature treatment at 110°C for 3 hours and a constant temperature treatment at 90°C for 6 hours for standby use;
[0134] (3) Preparation of staple fibers
[0135] The polymer solution 2 is filtered and defoamed, and then sprayed through a spinneret in a coagulation bath with a mass concentration of 65% and a temperature of 35°C to form primary fibers. The primary fibers are stretched 1.8 times and then sequentially washed with water at 60°C and 70°C, and then dried with a hot roller at 170°C, and then shaped with a hot pipe at 320°C, and then cut to obtain short fibers.
[0136] (4) Preparation of precipitation slurry:
[0137] Water, glycerol and sodium chloride were stirred evenly in a mass ratio of 55:42:3 to prepare a mixed solution, and then the mixed solution and polymer solution 2 were added to a precipitator in a mass ratio of 16:1, and high-speed shearing was performed at a temperature of 20°C and a speed of 3000 rpm / min for 40 minutes, and then the slurry was immersed in 5°C cold water for molding, and then countercurrent water washing was performed in a water bath of 30°C, 50°C, 70°C and 90°C in sequence to obtain a precipitated pulp of 1.6 mm and a specific surface area of 45 m 2 / g.
[0138] (5) Preparation of paper base
[0139] The precipitated pulp is beaten and dispersed with a cone mill, and the aramid staple fibers are dispersed with a pulper. The precipitated pulp and aramid staple fibers are then stirred and blended in a ratio of 6:4. The pulp is stirred at a stirring speed of 3000 rpm / min for 10 minutes to obtain pulp. The pulp is then formed on a chain plate, and then pressed and dried at a pressure of 2 MPa and a temperature of 160°C. It is then hot-pressed at a temperature of 280°C and a pressure of 24 MPa, and finally cut to obtain the paper-based material.
[0140] (6) Composite material preparation: Coat 20g / m2 on the film surface 2 The glue is then removed in an oven to remove the solvent, and the paper base and the insulating film coated with glue are compounded under a pressure of 0.3 MPa to obtain a tear-resistant, high-temperature resistant soft insulating composite material. Relevant tests can be carried out after being placed at room temperature for 7 days.
[0141] Example 3
[0142] A method for preparing a tear-resistant, high-temperature resistant aromatic soft insulating composite material, the preparation method comprising:
[0143] (1) Preparation of polymer solution:
[0144] Add 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride into a reactor filled with nitrogen, wherein the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride is 3.5:13:10, stir for 40 minutes, then heat to 90° C. and stir for 1 hour, and heat again to 130° C. and stir for 4 hours to obtain prepolymer solution 1;
[0145] Dissolve 8.6 parts of m-phenylenediamine in N,N-dimethylformamide to prepare a solution with a mass concentration of 12%, then slowly pour it into the polymerization solution 1, heat it to 25°C, and stir it for 10 minutes to obtain the prepolymer solution 2;
[0146] Add 9 parts of isophthaloyl chloride to prepolymer solution 2, stir in a water bath at 0°C for 40 minutes to obtain prepolymer solution 3, then add ammonia water to adjust the pH to 6.6, and then filter to obtain prepolymer solution 4;
[0147] Add the remaining 2.5 parts of isophthaloyl chloride to the prepolymer solution 4, stir at 20°C for 40 minutes to obtain a polymer solution 1, then add diethylamine to adjust the pH to 6.5 to obtain a polymer solution 2 with a viscosity of 900 Po;
[0148] (2) Preparation of insulating film:
[0149] The polymer solution 2 was filtered and defoamed, and then sprayed through a die head in a coagulation bath with a mass concentration of 55% and a temperature of 55°C to form a primary film, and then the primary film was first washed with water at 40°C for longitudinal stretching with a stretch ratio of 1.2, then washed with water at 70°C for transverse stretching with a stretch ratio of 0.9, and finally washed with water at 60°C. The washed film was again steam dried at 100°C and hot roller dried at 90°C, and then rolled up and trimmed to obtain an insulating film. The prepared insulating film was placed in a curing room and treated at a constant temperature of 110°C for 3 hours and at a constant temperature of 90°C for 6 hours for standby use;
[0150] (3) Preparation of staple fibers
[0151] The polymer solution 2 is filtered and defoamed, and then sprayed through a spinneret in a coagulation bath with a mass concentration of 55% and a temperature of 55°C to form primary fibers. The primary fibers are stretched 1.2 times and then sequentially washed with water at 50°C and 60°C, then dried with a hot roller at 130°C, and then shaped with a hot tube at 300°C before being cut to obtain staple fibers.
[0152] (4) Preparation of precipitation slurry:
[0153] Water, glycerol and potassium chloride were stirred evenly in a mass ratio of 34:60:6 to prepare a mixed solution, and then the mixed solution and polymer solution 2 were added to the precipitator in a mass ratio of 8:1, and high-speed shearing was performed at 60°C and 6000 rpm / min for 20 minutes, and then the slurry was immersed in -5°C cold water for molding, and then countercurrent water washing was performed in a water bath of 20°C, 40°C, 60°C and 80°C in sequence to obtain a precipitated pulp with a diameter of 0.8 mm and a specific surface area of 30m 2 / g.
[0154] (5) Preparation of paper base
[0155] The precipitated pulp is respectively beaten and dispersed by a cone mill, and the aramid staple fibers are dispersed by a pulper. The precipitated pulp and the aramid staple fibers are stirred and blended in a ratio of 4:6, and stirred at a stirring speed of 1000 rpm / min for 20 minutes to obtain pulp. The pulp is then formed on a chain plate, and then pressed and dried at a pressure of 2 MPa and a temperature of 120°C, and then hot-pressed at a temperature of 220°C and a pressure of 10 MPa, and finally cut to obtain a paper-based material.
[0156] (6) Composite material preparation: Coat 20g / m2 on the film surface 2 The glue is then removed in an oven to remove the solvent, and the paper base and the insulating film coated with glue are compounded under a pressure of 0.6MPa to obtain a tear-resistant, high-temperature resistant soft insulating composite material. Relevant tests can be carried out after being placed at room temperature for 7 days.
[0157] Example 4
[0158] A method for preparing a tear-resistant, high-temperature resistant aromatic soft insulating composite material, the preparation method comprising:
[0159] (1) Preparation of polymer solution:
[0160] Add 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and terephthaloyl chloride in a nitrogen-filled reactor, wherein the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and terephthaloyl chloride is 3.5:13.5:10, stir for 20 minutes, then heat to 80° C. and stir for 1.2 hours, and heat again to 105° C. and stir for 4 hours to obtain prepolymer solution 1;
[0161] Dissolve 10 parts of p-phenylenediamine in N,N-dimethylacetamide to prepare a solution with a mass concentration of 14%, then slowly pour it into the polymerization solution 1, heat it to 25°C, and stir it for 10 minutes to obtain the prepolymer solution 2;
[0162] Add 12 parts of terephthaloyl chloride to prepolymer liquid 2, stir in a water bath at 0°C for 30 minutes to obtain prepolymer liquid 3, then add ammonia water to adjust the pH to 7.0, and then filter to obtain prepolymer liquid 4;
[0163] Add the remaining 3 parts of terephthaloyl chloride to the prepolymer solution 4 and stir at 35°C for 30 minutes to obtain the polymerization solution 1. Then add diethylamine to adjust the pH to 7.3 to obtain the polymerization solution 2 with a viscosity of 1500 Po.
[0164] (2) Preparation of insulating film:
[0165] The polymer solution 2 is filtered and defoamed, and then sprayed through a die head in a coagulation bath with a mass concentration of 64% and a temperature of 55°C to form a primary film, and then the primary film is first washed with water at 50°C for longitudinal stretching with a stretch ratio of 1.8, then washed with water at 70°C for transverse stretching with a stretch ratio of 0.8, and finally washed with water at 60°C, and the washed film is again steam dried at 110°C and hot roller dried at 95°C, and then rolled up and trimmed to obtain an insulating film, and the prepared insulating film is placed in a curing room for constant temperature treatment at 110°C for 3 hours and at 90°C for 6 hours for standby use;
[0166] (3) Preparation of staple fibers
[0167] The polymer solution 2 is filtered and defoamed, and then sprayed through a spinneret in a coagulation bath with a mass concentration of 59% and a temperature of 44°C to coagulate and form primary fibers. The primary fibers are stretched 1.2 times and then sequentially washed with water at 60°C and 70°C, then dried with a hot roller at 160°C, and then shaped with a hot pipe at 320°C, and then cut to obtain short fibers.
[0168] (4) Preparation of precipitation slurry:
[0169] Water, glycerol and potassium chloride were stirred evenly in a mass ratio of 48:46:6 to prepare a mixed solution, and then the mixed solution and polymer solution 2 were added to the precipitator in a mass ratio of 15:1, and high-speed shearing was performed at 60°C and 5000 rpm / min for 40 minutes, and then the slurry was immersed in 5°C cold water for molding, and then countercurrent washing was performed in a water bath at 30°C, 50°C, 60°C and 80°C in sequence to obtain a precipitated pulp with a diameter of 0.9 mm and a specific surface area of 42 m 2 / g.
[0170] (5) Preparation of paper base
[0171] The precipitated slurry is beaten and dispersed with a cone mill, and the aramid staple fibers are dispersed with a pulper. The precipitated slurry and the aramid staple fibers are stirred and blended in a ratio of 5.6:4.4. The pulp is obtained by stirring at a stirring speed of 3000 rpm / min for 20 minutes. The pulp is then formed on a chain plate, pressed and dried at a pressure of 2 MPa and a temperature of 150°C, and then hot-pressed at a temperature of 275°C and a pressure of 23 MPa. Finally, the paper-based material is obtained by slitting.
[0172] (6) Composite material preparation: Coat 20g / m2 on the film surface 2 The glue is then removed in an oven to remove the solvent, and the paper base and the insulating film coated with glue are compounded under a pressure of 0.5 MPa to obtain a tear-resistant, high-temperature resistant soft insulating composite material. Relevant tests can be carried out after being placed at room temperature for 7 days.
[0173] Comparative Example 1
[0174] The tear-resistant, high-temperature-resistant soft insulating composite material was prepared by the same method as in Example 1, except that 4,6-diaminoresorcinol hydrochloride was not added when preparing the polymerization solution in step (1).
[0175] The specific process of step (1) of this comparative example 1 is:
[0176] (1) Preparation of polymer solution:
[0177] Add polyphosphoric acid and isophthaloyl chloride in a nitrogen-filled reactor, wherein the mass ratio of polyphosphoric acid to isophthaloyl chloride is 13.5:10, stir for 30 minutes, then heat to 80° C. and stir for 1.5 hours, and then heat to 115° C. and stir for 5 hours to obtain prepolymer solution 1;
[0178] Dissolve 10 parts of m-phenylenediamine in N,N-dimethylacetamide to prepare a solution with a mass concentration of 14%, then slowly pour it into the polymerization solution 1, heat it to 30°C, and stir it for 13 minutes to obtain the prepolymer solution 2;
[0179] Add 12 parts of isophthaloyl chloride to prepolymer solution 2, stir in a water bath at 5°C for 35 minutes to obtain prepolymer solution 3, then add ammonia water to adjust the pH to 7.1, and then filter to obtain prepolymer solution 4;
[0180] The remaining 3 parts of isophthaloyl chloride were added to the prepolymer solution 4, and the mixture was stirred at 25° C. for 25 minutes to obtain a polymerization solution 1. Diethylamine was then added to adjust the pH to 7.1 to obtain a polymerization solution 2.
[0181] The other subsequent operation methods are the same as those in Example 1.
[0182] Comparative Example 2
[0183] The tear-resistant, high-temperature-resistant soft insulating composite material was prepared by the same method as in Example 1, except that no polyphosphoric acid was added when preparing the polymerization solution in step (1).
[0184] The specific process of step (1) of this comparative example 2 is as follows:
[0185] (1) Preparation of polymer solution:
[0186] Add 4,6-diaminoresorcinol hydrochloride and isophthaloyl chloride in a nitrogen-filled reactor, wherein the mass ratio of 4,6-diaminoresorcinol hydrochloride to isophthaloyl chloride is 3.5:10, stir for 30 minutes, then heat to 80° C. and stir for 1.5 hours, and then heat to 115° C. and stir for 5 hours to obtain prepolymer solution 1;
[0187] Dissolve 10 parts of m-phenylenediamine in N,N-dimethylacetamide to prepare a solution with a mass concentration of 14%, then slowly pour it into the polymerization solution 1, heat it to 30°C, and stir it for 13 minutes to obtain the prepolymer solution 2;
[0188] Add 12 parts of isophthaloyl chloride to prepolymer solution 2, stir in a water bath at 5°C for 35 minutes to obtain prepolymer solution 3, then add ammonia water to adjust the pH to 7.1, and then filter to obtain prepolymer solution 4;
[0189] The remaining 3 parts of isophthaloyl chloride were added to the prepolymer solution 4, and the mixture was stirred at 25° C. for 25 minutes to obtain a polymerization solution 1. Diethylamine was then added to adjust the pH to 7.1 to obtain a polymerization solution 2.
[0190] The other subsequent operation methods are the same as those in Example 1.
[0191] Comparative Example 3
[0192] The tear-resistant, high-temperature-resistant soft insulating composite material was prepared by the same method as in Example 1, except that in step (1), the prepolymer solution 1 was reacted at 80° C. throughout the entire process.
[0193] The specific process of step (1) of this comparative example 3 is as follows:
[0194] (1) Preparation of polymer solution:
[0195] Add 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride into a reactor filled with nitrogen, wherein the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride is 3.5:13.5:10, stir for 30 minutes, then heat to 80° C. and stir for 6.5 hours to obtain prepolymer solution 1;
[0196] Dissolve 10 parts of m-phenylenediamine in N,N-dimethylacetamide to prepare a solution with a mass concentration of 14%, then slowly pour it into the polymerization solution 1, heat it to 30°C, and stir it for 13 minutes to obtain the prepolymer solution 2;
[0197] Add 12 parts of isophthaloyl chloride to prepolymer solution 2, stir in a water bath at 5°C for 35 minutes to obtain prepolymer solution 3, then add ammonia water to adjust the pH to 7.1, and then filter to obtain prepolymer solution 4;
[0198] The remaining 3 parts of isophthaloyl chloride were added to the prepolymer solution 4, and the mixture was stirred at 25° C. for 25 minutes to obtain a polymerization solution 1. Diethylamine was then added to adjust the pH to 7.1 to obtain a polymerization solution 2.
[0199] The other subsequent operation methods are the same as those in Example 1.
[0200] Comparative Example 4
[0201] The tear-resistant and high-temperature-resistant soft insulating composite material was prepared by the same method as in Example 1, except that in step (1), the prepolymer solution 1 was reacted at 115° C. throughout the entire process.
[0202] The specific process of step (1) of this comparative example 4 is as follows:
[0203] (1) Preparation of polymer solution:
[0204] Add 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride into a reactor filled with nitrogen, wherein the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and isophthaloyl chloride is 3.5:13.5:10, stir for 30 minutes, then heat to 115° C. and stir for 6.5 hours to obtain prepolymer solution 1;
[0205] Dissolve 10 parts of m-phenylenediamine in N,N-dimethylacetamide to prepare a solution with a mass concentration of 14%, then slowly pour it into the polymerization solution 1, heat it to 30°C, and stir it for 13 minutes to obtain the prepolymer solution 2;
[0206] Add 12 parts of isophthaloyl chloride to prepolymer solution 2, stir in a water bath at 5°C for 35 minutes to obtain prepolymer solution 3, then add ammonia water to adjust the pH to 7.1, and then filter to obtain prepolymer solution 4;
[0207] The remaining 3 parts of isophthaloyl chloride were added to the prepolymer solution 4, and the mixture was stirred at 25° C. for 25 minutes to obtain a polymerization solution 1. Diethylamine was then added to adjust the pH to 7.1 to obtain a polymerization solution 2.
[0208] The other subsequent operation methods are the same as those in Example 1.
[0209] The composite materials prepared in the above examples and comparative examples were subjected to performance tests, wherein the methods / standards involved in the performance tests were:
[0210] Stiffness performance: According to the national standard GT / T5591.2-2017, select a load of 5000N and a test speed of 25mm / min, test 5 groups of samples in each direction, and take the median value as the test result;
[0211] Edge tearing strength: According to the national standard GT / T5591.2-2017, select a load of 5000N and a test speed of 100mm / min, test 5 groups of specimens in each direction, and take the median value as the test result;
[0212] Temperature resistance strength: Test according to the hot spot tilt method in JB / T1544-2015 and the relevant provisions in JB / T3730-2015.
[0213] The specific performance test results of the composite materials described in the above embodiments and comparative examples are shown in Table 1 below.
[0214] Table 1 Composite material performance test results
[0215]
[0216] It can be seen from the data in the above table that the composite materials prepared by the preparation method of the present invention in Examples 1 to 4 have excellent mechanical properties and temperature resistance. In the preparation method of the present invention, by introducing a part of oxazole structure blocks with a rigid planar structure and a strong electron-donating conjugation effect into the polymerization liquid of the paper base and the film, the mechanical properties and modulus of the substrate are improved from the perspective of molecular structure, thereby making the final aromatic flexible insulating composite material more significantly tear-resistant and high-temperature resistant.
[0217] From the comparison of the experimental results of Example 1 and Comparative 1, it can be seen that if 4,6-diaminoresorcinol hydrochloride is not added during the preparation of the polymerization solution, the performance of the composite material will be significantly reduced. Therefore, the introduction of oxazole fragments by 4,6-diaminoresorcinol hydrochloride can significantly enhance the edge tear strength, stiffness and heat resistance of the composite material.
[0218] From the comparison of the experimental results of Example 1 and Comparative Example 2, it can be seen that even if polyphosphoric acid is not added, the performance of the composite material will change slightly. Polyphosphoric acid plays a catalytic role. If polyphosphoric acid is not added, even if 4,6-diaminoresorcinol hydrochloride is added, the formation efficiency of the oxazole fragment will be affected, which will ultimately affect the performance of the composite material.
[0219] From the comparison of the experimental results of Example 1 and Comparative Example 3, it can be seen that: under low temperature conditions, polymerization occurs between molecules, and dehydration condensation does not occur within the molecules to form oxazole fragments, so the performance is similar to the performance results without adding 4,6-diaminoresorcinol hydrochloride. Therefore, the temperature conditions defined in the present invention are more conducive to obtaining a composite material with excellent performance.
[0220] From the comparison of the experimental results of Example 1 and Comparative Example 4, it can be seen that the self-condensation of the small molecules of 4,6-diaminoresorcinol hydrochloride under high temperature conditions during continuous prepolymerization is not introduced into the molecular structure of the polymer, and the self-condensation of the small molecules causes the shortening of the polymer molecular chain, reducing the mechanical properties of the material. The material properties of Comparative Example 4 are much lower than those of Comparative Example 1.
[0221] The technical features of the above-described embodiments may be arbitrarily combined. To make the description concise, not all possible combinations of the technical features in the above-described embodiments are exhaustively listed. However, as long as there is no contradiction in the combination of these technical features, they should be considered to be within the scope of this specification.
[0222] For those skilled in the art, several modifications and improvements may be made without departing from the concept of the present invention, all of which belong to the protection scope of the present invention. The protection scope of the present invention shall be based on the attached claims.
Claims
1. A method for preparing a tear-resistant, high-temperature-resistant, soft insulating film, characterized in that: The preparation method is: S1. Preparation of polymer solution: S1.
1. Under the protection of inert gas, add aromatic acid chloride and polyphosphoric acid into a reaction kettle, stir evenly, add 4,6-diaminoresorcinol hydrochloride, heat to 70-90°C, stir and react for 1-2 hours, then heat to 100-130°C, stir and react for 4-6 hours, complete prepolymerization, and obtain prepolymer solution 1; S1.2, in an organic solvent, reacting the aromatic diamine with the prepolymer solution 1 to obtain a prepolymer solution 2; S1.3, reacting the prepolymer liquid 2 with an aromatic acyl chloride to obtain a prepolymer liquid 3; neutralizing the prepolymer liquid 3 and filtering to obtain a prepolymer liquid 4; S1.4, adding aromatic acid chloride to the prepolymer solution 4 again to obtain polymerization solution 1, and after neutralization treatment to obtain polymerization solution 2; S2. Preparation of insulating film: After filtering and defoaming, the polymer solution 2 is cast into a film in a coagulation bath through a die head, and is sequentially stretched longitudinally and transversely in a water bath, and then dried to obtain the insulating film.
2. The method for preparing a tear-resistant, high-temperature-resistant, soft insulating film according to claim 1, characterized in that: The reaction temperature of step S1.2 is 25-40°C; The reaction temperature of step S1.3 is 0-10°C; The reaction temperature of step S1.4 is 20-35°C.
3. The method for preparing a tear-resistant, high-temperature-resistant, soft insulating film according to claim 1, characterized in that: In step S1.3, the prepolymer solution 3 is neutralized with aqueous ammonia, and the pH of the prepolymer solution 4 is 6.5-7.8; In step S1.4, the polymerization solution 1 is neutralized with an organic base, and the pH of the polymerization solution 1 is 6.5-7.8; The organic base is any one or a combination of methylamine, dimethylamine, ethylamine and diethylamine.
4. The method for preparing a tear-resistant and high-temperature-resistant soft insulating film according to claim 1, characterized in that: The aromatic acyl chloride is one or more of isophthaloyl chloride and terephthaloyl chloride; The aromatic diamine is one or more of m-phenylenediamine, p-phenylenediamine and o-phenylenediamine; In the entire step S1, the mass ratio of the aromatic diamine, 4,6-diaminoresorcinol hydrochloride and aromatic acid chloride is (8.6-11): (3.5-4): (21.5-28.5); In step S1.1, the mass ratio of 4,6-diaminoresorcinol hydrochloride, polyphosphoric acid and aromatic acid chloride is (3.5-4): (13-21): 10; The mass ratio of the aromatic acyl chloride in step S1.3 to the aromatic acyl chloride in step S1.4 is (9-15):(2.5-3.5).
5. The method for preparing a tear-resistant, high-temperature-resistant, soft insulating film according to claim 1, characterized in that: In step S1.2, the mass concentration of the aromatic diamine in the organic solvent is 12-16%; the organic solvent is one or a combination of N-methylpyrrolidone, N,N-dimethylformamide, and N,N-dimethylacetamide; The viscosity of the polymer solution 2 is 900-1500 Po.
6. The method for preparing a tear-resistant and high-temperature-resistant soft insulating film according to claim 1, characterized in that: In step S2, the coagulation bath is an aqueous solution of DMAC, wherein the mass concentration of DMAC in the coagulation bath is 55-65%, and the temperature of the coagulation bath is 35-55° C.; Step S2 is carried out in three stages in the water bath: The water temperature in the first stage is 40~50℃, and longitudinal stretching is performed with a stretching ratio of 1.2~1.8; The water temperature in the second stage is 55~70℃, and transverse stretching is performed with a stretching ratio of 0.3~0.9; The water temperature in the third stage is 50~60℃, without stretching; In step S2, the drying is carried out in two stages: the first stage is steam drying at 100-120°C; the second stage is hot roller drying at 90-100°C.
7. A tear-resistant and high-temperature-resistant soft insulating film, characterized in that: The insulating film is prepared by the preparation method described in any one of claims 1 to 6.
8. A method for preparing a tear-resistant, high-temperature-resistant, soft insulating composite material, characterized in that: Glue is applied on the insulating film of claim 7, and after drying, it is pressed with a paper base to form the tear-resistant, high-temperature-resistant, soft insulating composite material; The preparation method of the paper base is: (1) Preparation of staple fibers: After filtering and removing bubbles, the polymer solution 2 is sprayed through a spinneret in a coagulation bath to form primary fibers, which are then stretched, washed, dried, shaped, and cut to obtain staple fibers; The polymer solution 2 is the polymer solution 2 obtained in step S1 of the preparation method according to any one of claims 1 to 6; (2) Preparation of precipitated pulp: Mix water, glycerol and chloride salt to prepare a mixed solution, then mix the mixed solution with polymer solution 2 according to a proportion, and then perform high-speed shearing, cooling and molding, and multi-stage water washing to obtain precipitated pulp; (3) Preparation of paper base: The precipitated pulp which has been subjected to a beating and dispersion treatment and the short fibers which have been subjected to a debonding and dispersion treatment are stirred and blended to obtain paper pulp, and the paper base is obtained by subjecting the paper pulp to flow forming, pressing and drying, hot pressing forming, and rewinding and slitting treatment.
9. The method for preparing a tear-resistant, high-temperature-resistant, soft insulating composite material according to claim 8, characterized in that: During the preparation of the staple fibers, the stretching ratio is 1.2-1.8; the washing is carried out in two stages: the water temperature of the first stage is 50-60°C, and the water temperature of the second stage is 60-70°C; the drying temperature is 130-170°C, and the setting temperature is 300-320°C.
10. The method for preparing a tear-resistant, high-temperature-resistant, soft insulating composite material according to claim 8, characterized in that: During the preparation of the precipitated pulp, the mass ratio of water, glycerol and chloride is (34-55): (42-60): (3-6); the mass ratio of the mixed solution to the polymer solution 2 is (8-16): 1; The high-speed shearing speed is 3000-6000 rpm / min, the temperature is 20-60°C, and the high-speed shearing time is 20-40 min; The cooling molding process is to immerse the slurry in -5~5℃ cold water for molding; The multi-stage water washing adopts a four-stage countercurrent water washing method, and the water temperature of the multi-stage water washing is: 20-30°C for the first stage, 40-50°C for the second stage, 60-70°C for the third stage, and 80-90°C for the fourth stage; The average length of the precipitated pulp is 0.8-1.6 mm, and the specific surface area is 30-45 m 2 / g.
11. The method for preparing a tear-resistant, high-temperature-resistant, soft insulating composite material according to claim 8, characterized in that: During the preparation of the paper base, the mass ratio of precipitated pulp and short fibers is (4-6): (4-6); The pressure of the pressing and drying is 1-2 MPa and the temperature is 120-160°C; The pressure of the hot pressing molding is 10-24 MPa and the temperature is 220-280°C.
12. The method for preparing a tear-resistant, high-temperature-resistant, soft insulating composite material according to claim 8, characterized in that: The coating amount of the glue is 5~50g / m 2 The pressure during pressing is 0.3~0.6MPa.
13. A tear-resistant, high-temperature-resistant, soft insulating composite material, characterized in that: The tear-resistant, high-temperature-resistant, soft insulating composite material is prepared according to the preparation method according to any one of claims 8 to 12.